Spherical boron nitride particles, filler for resin, resin composition, and method for producing spherical boron nitride particles

By cavitating spherical boron nitride particles in a water liquid and controlling their surface state, the problem of reduced fluidity of boron nitride particles in resin is solved and a resin composition with excellent fluidity is realized.

CN118765260APending Publication Date: 2024-10-11DENKA CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202380020526.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-02-16
Filing Date
2023-02-14
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

When boron nitride particles are blended into a resin, it is difficult to maintain a resin composition with excellent fluidity.

Method used

By cavitating spherical boron nitride particles in a liquid containing water, the surface state of the particles is controlled so that the B1s/O1s ratio is 90 or less to suppress aggregation and maintain fluidity in the resin.

Benefits of technology

When 15 volume % of spherical boron nitride particles are filled in the resin, the thixotropic index of the viscosity is lower than 6, the fluidity is excellent, and the resin is suitable for manufacturing efficient resin compositions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004980636370000131
    Figure BDA0004980636370000131
Patent Text Reader

Abstract

The invention provides spherical boron nitride particles capable of obtaining a resin composition with excellent fluidity, a filler for resin containing the spherical boron nitride particles, a resin composition, and a method for producing the spherical boron nitride particles. The spherical boron nitride particles according to the present invention have a B1s / O1s ratio of 90 or less between a semi-quantitative value calculated from an O1s peak intensity measured by X-ray photoelectron spectroscopy and a semi-quantitative value calculated from a B1s peak intensity. It is preferable that the thixotropic index (T.I value), which is represented by the ratio ([eta] 1 / [eta] 2) of the viscosity [eta] 1 measured at a shear velocity of 1 (1 / s) to the viscosity [eta] 2 measured at a shear velocity of 10 (1 / s), among viscosities measured at 25 DEG C by changing the shear velocity from 0.01 (1 / s) to 100 (1 / s), is 2 or less.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to spherical boron nitride particles, a filler for resin, a resin composition and a method for producing spherical boron nitride particles. Background Art

[0002] Hexagonal boron nitride (hereinafter referred to as "boron nitride") has lubricity, high thermal conductivity, insulation, and the like, and is widely used in solid lubricants, molten gas, aluminum and other release agents, and fillers for heat dissipation materials.

[0003] As boron nitride particles that take advantage of the lubricity and high thermal conductivity characteristics of boron nitride, Patent Document 1 describes a submicron spherical boron nitride particle with a scaly shape having a small diameter / thickness ratio (aspect ratio) and having a high purity and high crystallinity. Patent Document 2 describes a submicron spherical boron nitride particle with a high sphericity.

[0004] Patent Document 1: International Publication No. 2015 / 122378

[0005] Patent Document 2: International Publication No. 2015 / 122379 Summary of the invention

[0006] Generally speaking, if an inorganic filler is mixed with a resin, the fluidity of the resin composition tends to decrease. The inventors of the present application have conducted in-depth research on boron nitride particles that can achieve excellent fluidity even when boron nitride particles are mixed with a resin. As a result, it was surprisingly found that spherical boron nitride particles with a predetermined surface state can achieve a resin composition with excellent fluidity.

[0007] The technical problem of the present invention is to provide spherical boron nitride particles capable of realizing a resin composition having excellent fluidity, a resin filler and a resin composition containing the spherical boron nitride particles, and a method for producing the spherical boron nitride particles.

[0008] The present invention has the following configurations.

[0009] [1] A spherical boron nitride particle having an O content measured by X-ray photoelectron spectroscopy. 1s The semi-quantitative value calculated from the peak intensity is consistent with that calculated from B 1s The semi-quantitative value B calculated from the peak intensity 1s / O 1s The ratio is below 90.

[0010] [2] Spherical boron nitride particles as described in [1], wherein, for a mixture of spherical boron nitride particles filled with 15 volume % of epoxy resin, the thixotropic index (TI value) represented by the ratio (η1 / η2) of the viscosity η1 measured at a shear rate of 1 (1 / s) to the viscosity η2 measured at a shear rate of 10 (1 / s), measured at 25°C with the shear rate varied from 0.01 (1 / s) to that measured.

[0011] [3] Spherical boron nitride particles as described in [1] or [2], wherein, for a mixture of spherical boron nitride particles filled with 15 volume % of epoxy resin, the thixotropic index (TI value) represented by the ratio (η1 / η2) of the viscosity η1 measured at a shear rate of 1 (1 / s) to the viscosity η2 measured at a shear rate of 10 (1 / s) measured at 25°C is 6 or less.

[0012] [4] The spherical boron nitride particles according to any one of [1] to [3], wherein the volume-based cumulative particle size (D50) evaluated by a laser diffraction scattering method is 35 μm or less when the particles are not treated with a homogenizer.

[0013] [5] The spherical boron nitride particles according to any one of [1] to [4], wherein the average circularity is greater than 0.80.

[0014] [6] The spherical boron nitride particles according to any one of [1] to [5], wherein the O 1s The semi-quantitative value calculated from the peak intensity was 0.6 or more.

[0015] [7] A filler for a resin, comprising the spherical boron nitride particles according to any one of [1] to [6].

[0016] [8] A resin composition comprising a resin and the spherical boron nitride particles according to any one of [1] to [6].

[0017] [9] A method for producing spherical boron nitride particles as described in any one of [1] to [6], comprising the step of generating cavitation bubbles in a liquid containing raw material spherical boron nitride particles and water.

[0018] According to the present invention, there can be provided spherical boron nitride particles capable of realizing a resin composition having excellent fluidity, a filler for a resin containing the spherical boron nitride particles, a resin composition, and a method for producing the spherical boron nitride particles. DETAILED DESCRIPTION

[0019] Hereinafter, one embodiment of the present invention will be described in detail. The present invention is not limited to the following embodiment, and can be implemented with appropriate modifications within a range that does not inhibit the effects of the present invention.

[0020] (Spherical Boron Nitride Particles)

[0021] The spherical boron nitride particles of this embodiment are measured by X-ray photoelectron spectroscopy. 1s The semi-quantitative value calculated from the peak intensity is consistent with that calculated from B 1s The semi-quantitative value B calculated from the peak intensity 1s / O 1s B 1s / O 1s ratio”) is below 90.

[0022] The O 1s The semi-quantitative value calculated from the peak intensity is consistent with that calculated from B 1s The semi-quantitative value B calculated from the peak intensity 1s / O 1s When the ratio is 90 or less, the spherical boron nitride particles of the present embodiment can realize a resin composition having excellent fluidity when filled in a resin.

[0023] In this specification, the term "spherical" means a granular shape that is round or has rounded corners when observed at 10,000 times using a scanning electron microscope. 1s The semi-quantitative value calculated from the peak intensity is consistent with that calculated from B 1s The semi-quantitative value B calculated from the peak intensity 1s / O 1s "Ratio" refers to the calculation of B by subtracting the background value using the Shirley method 1s and O 1s The semi-quantitative value of the peak intensity is calculated, and B is calculated 1s / O 1s Ratio, the value obtained thereby.

[0024] In this specification, the "Shirley method" refers to a method of determining the shape of the subtracted background value on the assumption that there is no energy correlation with inelastic scattered electrons that cause the background value or that the number of inelastic scattered electrons is proportional to the peak intensity.

[0025] O was determined by X-ray photoelectron spectroscopy 1s The semi-quantitative value calculated from the peak intensity is consistent with that calculated from B 1s The semi-quantitative value B calculated from the peak intensity 1s / O 1sThe spherical boron nitride particles having a ratio of 90 or less have a surface state that is excellent in dispersibility in water. Furthermore, it has surprisingly been found that such spherical boron nitride particles improve the fluidity of a resin composition when mixed with a resin.

[0026] The spherical boron nitride particles according to one embodiment have an O 1s The semi-quantitative value calculated from the peak intensity is consistent with that calculated from B 1s The semi-quantitative value B calculated from the peak intensity 1s / O 1s The ratio is preferably 85 or less, more preferably 85 or less, further preferably 80 or less, further preferably 75 or less, and particularly preferably 70 or less.

[0027] B 1s / O 1s The lower limit of the ratio is not particularly limited, and may be 10 or more, 15 or more, or 20 or more.

[0028] As a 1s / O 1s The method of reducing the ratio to less than 90 can be exemplified by subjecting the raw material spherical boron nitride particles to cavitation treatment in a liquid containing water. The raw material spherical boron nitride particles have the property of being easily aggregated, but if cavitation treatment is performed in a liquid containing water, the aggregated state will be crushed while maintaining the shape (spherical) of the primary particles. Many hydroxyl groups will be introduced into the surface of the crushed primary particles, which can easily make B 1s / O 1s The ratio is 90 or less. 1s / O 1s The ratio is 90 or less, and the crushed spherical boron nitride particles can be prevented from agglomerating again in the resin. The details of the cavitation treatment will be described later.

[0029] By lengthening the cavitation treatment time, B 1s / O 1s Than becomes smaller.

[0030] By treating under conditions with many cavitation bubbles or by prolonging the cavitation treatment time, the surface hydroxyl groups can be increased, making B 1s / O 1s Than becomes smaller.

[0031] The inventors of the present application have found through research that the spherical boron nitride particles treated by this method can further improve the fluidity of the resin compared to the pulverized particles obtained by mechanical pulverization.

[0032] The spherical boron nitride particles according to one embodiment have an O 1sThe semi-quantitative value calculated from the peak intensity is preferably 0.6 or more, more preferably 0.65 or more, and still more preferably 0.7 or more. In this specification, the term "O measured by X-ray photoelectron spectroscopy" means 1s The semi-quantitative value calculated by peak intensity is obtained by subtracting the background value from the obtained spectrum using the Shirley method. 1s The semi-quantitative value calculated from the peak intensity. 1s The upper limit of the semi-quantitative value calculated from the peak intensity is not particularly limited, and may be 5.0 or less, 4.0 or less, 3.0 or less, or 2.0 or less.

[0033] The spherical boron nitride particles according to one embodiment have a B 1s The semi-quantitative value calculated from the peak intensity is preferably less than 48.4, more preferably less than 48.35, and still more preferably less than 48.3. In this specification, the term "B measured by X-ray photoelectron spectroscopy" means 1s The semi-quantitative value calculated by peak intensity is obtained by subtracting the background value from the obtained spectrum using the Shirley method. 1s Semi-quantitative value calculated from peak intensity.

[0034] For the spherical boron nitride particles of one embodiment, for a mixture in which 15 volume % of the spherical boron nitride particles are filled in an epoxy resin, the viscosity measured at 25° C. with the shear rate varied from 0.01 (1 / s) to 100 (1 / s) is expressed as a thixotropic index (TI value, hereinafter also referred to as “TI value”) expressed as a ratio (η1 / η2) of the viscosity η1 measured when the shear rate is 1 (1 / s) to the viscosity η2 measured when the shear rate is 10 (1 / s). (0.01-100) ”) is preferably 2 or less, more preferably 1.8 or less, further preferably 1.6 or less, further preferably 1.4 or less, and particularly preferably 1.2 or less.

[0035] The epoxy resin containing spherical boron nitride particles according to one embodiment has the low thixotropic index (TI value) described above and is therefore excellent in fluidity.

[0036] TI value (0.01-100) The lower limit of , the closer to 1, the better.

[0037] For the spherical boron nitride particles of one embodiment, for a mixture in which 15 volume % of the spherical boron nitride particles are filled in an epoxy resin, the viscosity measured at 25° C. with the shear rate varied from 100 (1 / s) to 0.01 (1 / s) is expressed as a thixotropic index (TI value, hereinafter also referred to as “TI value”) expressed as a ratio (η1 / η2) of the viscosity η1 measured when the shear rate is 1 (1 / s) to the viscosity η2 measured when the shear rate is 10 (1 / s).(100-0.01) ”) is preferably 6 or less, more preferably 5.6 or less, further preferably 5.2 or less, further preferably 4.8 or less, and particularly preferably 4.6 or less.

[0038] The epoxy resin containing spherical boron nitride particles according to one embodiment has excellent fluidity because it has the low thixotropic index (TI value) in the viscosity when the shear rate is changed from high shear to low shear.

[0039] TI value (100-0.01) The lower limit of , the closer to 1, the better.

[0040] The method for determining the "thixotropic index (TI value)" in this specification is as follows. That is, 15 volume % of spherical boron nitride particles are filled in an epoxy resin by a known method to obtain a mixture (resin composition). For the obtained mixture, a dynamic viscoelasticity measuring device is used to measure the viscosity at 25°C, (1) changing the shear rate from 0.01 (1 / s) to 100 (1 / s), or (2) changing the shear rate from 100 (1 / s) to 0.01 (1 / s). The thixotropic index (TI value) is obtained in the form of the ratio (η1 / η2) of the viscosity η1 measured when the shear rate is 1 (1 / s) and the viscosity η2 measured when the shear rate is 10 (1 / s).

[0041] In one embodiment, the mixture (resin composition) filled with spherical boron nitride particles has a thixotropic index (TI value) close to 1 when the shear rate is changed from low shear to high shear or when the shear rate is changed from high shear to low shear, that is, it has excellent fluidity.

[0042] For the spherical boron nitride particles of one embodiment, the volume-based cumulative (D50) evaluated by the laser diffraction scattering method without a specific dispersion treatment, such as homogenizer treatment (i.e., without applying external force) is preferably 35 μm or less, more preferably 33 μm or less, further preferably 32 μm or less, further preferably 30 μm or less, and particularly preferably 28 μm or less. In addition, the lower limit of the volume-based cumulative (D50) evaluated by the laser diffraction scattering method without homogenizer treatment (i.e., without applying external force) is not particularly limited, and can be 5 μm or more, 10 μm or more, or 15 μm or more.

[0043] The term "volume-based cumulative (D50)" as used herein refers to the particle size at which the cumulative value is equivalent to 50% in the volume-based cumulative particle size distribution measured by the laser diffraction scattering method (refractive index: 1.7). The cumulative particle size distribution is represented by a distribution curve with the horizontal axis being the particle size (μm) and the vertical axis being the cumulative value (%).

[0044] Although not subjected to homogenizer treatment, the volume-based cumulative (D50) of the spherical boron nitride particles of one embodiment evaluated by the laser diffraction scattering method is still as small as 30 μm or less. That is, the spherical boron nitride particles of one embodiment have the characteristics of being essentially smaller particles and having a higher proportion of primary particles than secondary particles even without being subjected to treatment such as homogenizer treatment. The spherical boron nitride particles of one embodiment contribute to the improvement of the fluidity of the mixture (resin composition) filled with the spherical boron nitride particles. 1s / O 1s Spherical boron nitride particles having a ratio exceeding 90 have difficulty in achieving such volume-based accumulation (D50).

[0045] The spherical boron nitride particles of this embodiment can obtain smaller particles by further treating with a homogenizer. The spherical boron nitride particles of one embodiment, after being treated with a homogenizer (conditions: 300W, 90 seconds) in ethanol, the volume-based cumulative (D50) evaluated by the laser diffraction scattering method is preferably 0.6μm or less, more preferably 0.58μm or less, and further preferably 0.56μm or less. In addition, the lower limit of the volume-based cumulative (D50) evaluated by the laser diffraction scattering method after being treated with a homogenizer (conditions: 300W, 90 seconds) is not particularly limited, and can be 0.1μm or more, 0.2μm or more, or 0.3μm or more.

[0046] The spherical boron nitride particles of one embodiment preferably have an average circularity greater than 0.70, more preferably greater than 0.725, further preferably greater than 0.75, further preferably greater than 0.775, and particularly preferably greater than 0.80. In addition, the upper limit of the average circularity is not particularly limited, and the upper limit may be less than 1, and may be less than 0.95.

[0047] The "average circularity" in this specification refers to a value calculated as follows.

[0048] The projected area (S) and perimeter (L) of the boron nitride particles are calculated by image analysis using image analysis software (e.g., manufactured by Mountech, trade name: MacView) for the image taken with a scanning electron microscope (SEM) (magnification: 10,000 times, image resolution: 1280×1024 pixels). The circularity is calculated using the projected area (S) and perimeter (L) according to the following formula:

[0049] Circularity = 4πS / L 2 .

[0050] The average circularity obtained for 100 randomly selected boron nitride particles is defined as the average circularity.

[0051] The spherical boron nitride particles of one embodiment have a feature of having a high average circularity. The high average circularity contributes to improving the fluidity of the mixture (resin composition) filled with the spherical boron nitride particles of one embodiment.

[0052] (use)

[0053] Spherical boron nitride particles can provide a resin composition having excellent fluidity and thus can be preferably used as a filler for a resin.

[0054] (Manufacturing method)

[0055] The method for producing spherical boron nitride particles according to the present embodiment includes the step of generating cavitation bubbles in a liquid containing raw material spherical boron nitride particles and water.

[0056] (Raw material spherical boron nitride particles)

[0057] The raw material spherical boron nitride particles are preferably produced by the method described in Patent Document 2. That is, boric acid ester and ammonia having a molar ratio of ammonia to boric acid ester of 1 to 10 are reacted in an inert gas stream at 750° C. or higher within 30 seconds, and then heat treated at 1000 to 1600° C. for 1 hour or more in an atmosphere of ammonia or a mixed gas of ammonia and an inert gas, and then calcined at 1800 to 2200° C. for 0.5 hour or more in an inert gas atmosphere to obtain the spherical boron nitride particles.

[0058] Examples of the boric acid ester include trimethyl borate.

[0059] The volume-based cumulative diameter (D50) of the raw material spherical boron nitride particles evaluated by the laser diffraction scattering method (the method described in the last paragraph on page 12 of the specification (particle size distribution 2) described later) can be 0.01 μm or more, 0.05 μm or more, 0.1 μm or more, 0.2 μm or more, 0.3 μm or more, or 0.4 μm or more. From the viewpoint of improving the dielectric breakdown characteristics of the heat dissipation component, it can be 1 μm or less, 0.9 μm or less, 0.8 μm or less, or 0.7 μm or less. It is preferably 0.01 to 1.0 μm, and more preferably 0.3 to 0.8 μm.

[0060] The average circularity of the raw material spherical boron nitride particles is preferably 0.8 or more, and more preferably 0.87 or more. The method for measuring the volume-based cumulative diameter (D50) and the average circularity is as described above.

[0061] (cavitation bubbles)

[0062] In the method for producing spherical boron nitride particles of the present embodiment, the raw material spherical boron nitride particles are placed in a liquid containing water (preferably water) to generate cavitation bubbles in the liquid.

[0063] In this specification, the term "cavitation bubbles" refers to bubbles generated when liquid vaporizes under low pressure.

[0064] By generating cavitation bubbles in a liquid containing spherical boron nitride particles and water, the secondary particles of the spherical boron nitride particles are crushed into primary particles by the expansion and contraction force caused by the pressure difference of the bubbles generated by cavitation, and at the same time, the surface state of the particles is changed, such as an increase in the presence ratio of hydroxyl groups.

[0065] Cavitation bubbles can be generated by a commercially available device that generates cavitation bubbles by foaming in a liquid caused by reduced pressure or ultrasonic waves. It is preferably carried out using a commercially available powder suction continuous dissolution and dispersion device, and it is particularly preferred to treat the powder by circulating the liquid. The powder suction continuous dissolution and dispersion device generally has a component that generates a flow rate by a stirring blade, and the rotation speed of the stirring blade is preferably 2000 to 10000 rpm, more preferably 4000 to 9000 rpm, further preferably 4500 to 8000 rpm, further preferably 5000 to 8000 rpm, and particularly preferably 6000 to 7200 rpm.

[0066] The secondary particles are crushed into primary particles by the expansion and contraction force caused by the pressure difference of the bubbles generated by cavitation, and the surface state of the particles is changed, such as an increase in the abundance ratio of hydroxyl groups.

[0067] In one embodiment, the cavitation bubble generation treatment is preferably performed 50 times or more, more preferably 100 times or more, and even more preferably 150 times or more, as the number of cavitation treatments calculated from the rotation speed (rpm) of the stirring blade of the device and the discharge amount. By performing the cavitation bubble generation treatment 50 times or more, B can be easily 1s / O 1s The ratio is below 90.

[0068] The O measured by X-ray photoelectron spectroscopy can be obtained 1s The semi-quantitative value calculated from the peak intensity is consistent with that calculated from B 1s The semi-quantitative value B calculated from the peak intensity 1s / O 1s Spherical boron nitride particles with a ratio of 90 or less.

[0069] In the method for producing spherical boron nitride particles of the present embodiment, the liquid used in the production may be a liquid consisting only of an organic solvent such as ethanol, or may be a mixed solution of water and an organic solvent.

[0070] In the case of a mixed solution of water and an organic solvent, the content of water in the mixed solution is preferably 80% by mass or more, more preferably 90% by mass or more, further preferably 95% by mass or more, and particularly preferably composed only of water.

[0071] The liquid used in the production preferably contains 5 to 30% by weight of spherical boron nitride particles, more preferably 5 to 20% by weight, further preferably 5 to 15% by weight, further preferably 5 to 10% by weight, and particularly preferably 8 to 10% by weight.

[0072] (Filler for resin)

[0073] The filler for resin of the present embodiment contains the spherical boron nitride particles. The spherical boron nitride particles are as described above.

[0074] Examples of the resin to be filled with the resin filler of the present embodiment include: epoxy resin, silicone resin, phenolic resin, melamine resin, urea-formaldehyde resin, unsaturated polyester, fluororesin, polyimide, polyamide-imide, polyetherimide and other polyamides, polybutylene terephthalate, polyethylene terephthalate and other polyesters, polyphenylene ether, polyphenylene sulfide, wholly aromatic polyester, polysulfone, liquid crystal polymer, polyether sulfone, polycarbonate, maleimide-modified resin, ABS resin, AAS (acrylonitrile-acrylic rubber / styrene) resin, AES (acrylonitrile / ethylene / propylene / diene rubber-styrene) resin, etc., preferably a resin containing one or more selected from these, more preferably an epoxy resin.

[0075] The resin filler of the present embodiment is preferably added in such a manner that the content of the spherical boron nitride particles in the resin composition becomes 5 to 80 volume %. When added in such a manner that it becomes 5 to 30 volume %, more preferably 10 to 25 volume %, and further preferably 15 to 20 volume %, a resin composition with higher fluidity can be obtained. When added in such a manner that the content of the spherical boron nitride particles in the resin composition becomes 50 to 80 volume %, more preferably 60 to 80 volume %, and further preferably 70 to 80 volume %, a resin composition with higher thermal conductivity can be obtained. In one embodiment, the resin filler is added in such a manner that the content of the spherical boron nitride particles in the resin composition becomes more than 5 volume % and less than 20 volume %.

[0076] (Resin composition)

[0077] The resin composition of the present embodiment contains a resin and the above-mentioned spherical boron nitride particles.

[0078] Examples of the resin include epoxy resins, silicone resins, phenolic resins, melamine resins, urea resins, unsaturated polyesters, fluororesins, polyimides, polyamide-imides, polyetherimides and other polyamides, polybutylene terephthalate, polyethylene terephthalate and other polyesters, polyphenylene ethers, polyphenylene sulfides, wholly aromatic polyesters, polysulfones, liquid crystal polymers, polyethersulfones, polycarbonates, maleimide-modified resins, ABS resins, AAS (acrylonitrile-acrylic rubber / styrene) resins, AES (acrylonitrile / ethylene / propylene / diene rubber-styrene) resins, and the like. It is preferred that the resin contains one or more selected from these, and more preferably an epoxy resin.

[0079] The content of spherical boron nitride particles is 5 to 80 volume % in the resin composition. From the viewpoint of fluidity, the content of spherical boron nitride particles is preferably 5 to 30 volume %, more preferably 10 to 25 volume %, and further preferably 15 to 20 volume %. In one embodiment, the content of spherical boron nitride particles exceeds 5 volume % and is less than 20 volume % in the resin composition. From the viewpoint of thermal conductivity, the content of spherical boron nitride particles is 50 to 80 volume %, more preferably 60 to 80 volume %, and further preferably 70 to 80 volume %. In one embodiment, the content of spherical boron nitride particles exceeds 70 volume % and is less than 80 volume % in the resin composition.

[0080] The following components and other additives can be added to the resin composition as needed. Other additives include: rubber-like substances such as silicone rubber, polysulfide rubber, acrylic rubber, butadiene rubber, styrene block copolymers, saturated elastomers, various thermoplastic resins, resin-like substances such as silicone resins, and resins obtained by partially or completely modifying epoxy resins and phenolic resins with aminosilicone, epoxysilicone, alkoxysilicone, etc.; flame retardant additives include: Sb2O3, Sb2O4, Sb2O5, etc.; flame retardants include: halogenated epoxy resins, phosphorus compounds, etc.; and colorants include: carbon black, iron oxide, dyes, pigments, etc.

[0081] The manufacture of the resin composition can be carried out by stirring, dissolving, mixing, and dispersing the predetermined amounts of the above-mentioned materials. As devices for mixing, stirring, and dispersing these mixtures, a grinder, a three-roll mill, a ball mill, a planetary mixer, etc. equipped with a stirring and heating device can be used. Alternatively, these devices can be used in appropriate combination.

[0082] [Example]

[0083] The present invention will be described in more detail below with reference to Examples, but the interpretation of the present invention is not limited to these Examples.

[0084] The raw material spherical boron nitride particles were prepared in the following steps.

[0085] (1) A reaction tube (quartz tube) disposed in a resistance heating furnace is heated to 1150° C. The trimethyl borate is introduced into the reaction tube by passing nitrogen gas through the trimethyl borate. Next, ammonia gas is directly introduced into the reaction tube. The molar ratio of the amount of ammonia introduced to the amount of trimethyl borate introduced (ammonia / trimethyl borate) is set to 1.8. The trimethyl borate is reacted with ammonia to obtain a precursor of boron nitride particles (white powder).

[0086] (2) The obtained boron nitride particle precursor was placed in a boron nitride crucible in a resistance heating furnace, and nitrogen and ammonia were introduced into the reaction tube at flow rates of 10 L / min and 15 L / min, respectively. The reaction tube was heated at 1500° C. for 5 hours to obtain a second precursor.

[0087] (3) The obtained second precursor was placed in a boron nitride crucible and heated at 2000° C. for 5 hours in an induction heating furnace under a nitrogen atmosphere to obtain spherical boron nitride particles.

[0088] The volume-based cumulative diameter (D50) of the raw material spherical boron nitride particles evaluated by a laser diffraction scattering method was 0.62 μm, and the average circularity was 0.87.

[0089] (Examples 1 to 4, Comparative Example 1)

[0090] Spherical boron nitride powder was mixed into 1000cc of ion exchange water at 10 wt%. For Examples 1 to 4, the obtained aqueous solution was subjected to cavitation treatment using a powder absorption continuous dissolution dispersion device (manufactured by Japan Spindle Co., Ltd., "JET PASTER", model: JPSS) under the conditions shown in Table 1. For Comparative Example 1, no cavitation treatment was performed.

[0091] In Table 1, the "number of treatments" refers to the number of times the treatment solution passes through the stirring blades calculated from the rotation speed (rpm) of the stirring blades of the powder absorption continuous dissolution and dispersion device and the discharge amount per rotation.

[0092] After the cavitation treatment, the liquid is filtered and dried to recover the spherical boron nitride powder.

[0093] (Measurement)

[0094] The spherical boron nitride powders obtained in Examples 1 to 4 and Comparative Example 1 were measured for various physical properties described below. The results are shown in Table 1.

[0095] (B 1s / O 1s Compare)

[0096] The spectra of the spherical boron nitride powders of Examples 1 to 4 and Comparative Example 1 were measured using an X-ray photoelectron spectrometer (manufactured by Thermo Corporation, "K-Alpha X-ray Photoelectron Analyzer", Al-X-ray source with monochromator, measuring area: 400×200 μm), and the background value was subtracted by the Shirley method. 1s and O 1s The peak intensity is calculated to obtain the semi-quantitative value and B 1s / O 1s Compare.

[0097] (Particle size distribution 1)

[0098] Regarding the spherical boron nitride particles of Examples 1 to 4 and Comparative Example 1, 0.1 g was dispersed in 80 mL of ethanol, and the volume-based particle size distribution was measured using a laser diffraction scattering particle size distribution measuring device (manufactured by Beckman Coulter, trade name: LS-13 320) without being treated with a homogenizer. At this time, the refractive index of ethanol was 1.359, or a value of 1.7 was used for the refractive index of boron nitride powder. From the obtained frequency particle size distribution, the median diameter D50 (μm) of the particles not treated with a homogenizer was obtained.

[0099] (Particle size distribution 2)

[0100] Regarding the spherical boron nitride particles of Examples 1 to 4 and Comparative Example 1, 0.01 g was dispersed in 80 mL of ethanol, and ultrasonic dispersion was performed for 1 minute and 30 seconds at an amplitude of 70 to 80% using an ultrasonic homogenizer (manufactured by Nippon Seiki Manufacturing Co., Ltd., trade name: US-300E). The volume-based particle size distribution was measured using a laser diffraction scattering particle size distribution measuring device (manufactured by Beckman Coulter, trade name: LS-13 320). The median diameter was calculated from the obtained volume-based particle size distribution. This median diameter is the particle size at which the cumulative value of the cumulative particle size distribution is 50%. At this time, the refractive index of ethanol is 1.359, or a value of 1.7 is used for the refractive index of boron nitride powder. The results are shown in Table 1.

[0101] (Average circularity)

[0102] The projected area (S) and perimeter (L) of the boron nitride particles were calculated by image analysis using image analysis software (e.g., manufactured by Mountech, trade name: MacView) using an image of the boron nitride particles taken using a scanning electron microscope (SEM) (magnification: 10,000 times, image resolution: 1280×1024 pixels). The circularity was calculated using the projected area (S) and perimeter (L) according to the following formula:

[0103] Circularity = 4πS / L2

[0104] The average circularity obtained for 100 randomly selected boron nitride particles is defined as the average circularity.

[0105] (Preparation of resin composition)

[0106] The spherical boron nitride particles of Examples 1 to 4 and Comparative Example 1 were mixed with an epoxy resin in the following manner to prepare a resin composition.

[0107] A dispersant ("DISPERBYK-111", manufactured by BYK Chemicals, Japan, 0.3 wt%), an SC material ("3-glycidyloxypropyltrimethoxysilane", manufactured by Tokyo Chemical Industry Co., Ltd., 1 wt%), and spherical boron nitride particles (15 wt%) of Examples 1 to 4 and Comparative Example 1 were added to the epoxy resin, and kneaded for 3 minutes at room temperature, a revolution speed of 2000 rpm, and a rotation speed of 800 rpm using a mixer ("AWATORI AR-250", manufactured by Thinky). Then, kneading was performed twice using a three-roll mill ("BR-150VIII", manufactured by IMEX, gap: 10 μm, processing roll speed: 60 μm) to obtain a resin composition.

[0108] (Thixotropic Index (TI value))

[0109] The obtained resin composition was subjected to a rheometer (manufactured by Anton Paar, “MCR92”) and the thixotropic index (TI value) was calculated at 25°C from the viscosity η1 measured when the shear rate was 1 (1 / s) to the viscosity η2 measured when the shear rate was 10 (1 / s), of the viscosities measured (1) when the shear rate was changed from 0.01 (1 / s) to 100 (1 / s) and (2) when the shear rate was changed from 100 (1 / s) to 0.01 (1 / s).

[0110] Table 1

[0111]

[0112] As shown in Table 1, the resin compositions containing spherical boron nitride particles of Examples 1 to 4 have better fluidity than the resin composition containing spherical boron nitride particles of Comparative Example 1. Surprisingly, the thixotropic index (TI value) is low and closer to 1 not only when the shear rate is changed from low shear to high shear, but also when the shear rate is changed from high shear to low shear, and has the characteristic of high fluidity.

[0113] Industrial applicability

[0114] The spherical boron nitride particles of the present embodiment can provide a resin composition having excellent fluidity, and thus can be suitably used for a resin filler and a resin composition containing the spherical boron nitride particles, and have industrial applicability.

Claims

1. A spherical boron nitride particle, wherein the O 1s The semi-quantitative value calculated from the peak intensity is consistent with that calculated from B 1s The semi-quantitative value B calculated from the peak intensity 1s / O 1s The ratio is below 90.

2. The spherical boron nitride particles according to claim 1, wherein For a mixture of epoxy resin filled with 15 volume % of spherical boron nitride particles, the viscosity is measured at 25°C with the shear rate varied from 0.01 (1 / s) to 100 (1 / s). The thixotropic index, i.e., the TI value, is expressed as the ratio (η1 / η2) of the viscosity η1 measured when the shear rate is 1 (1 / s) to the viscosity η2 measured when the shear rate is 10 (1 / s) and is less than 2.

3. The spherical boron nitride particles according to claim 1 or 2, wherein For a mixture of spherical boron nitride particles filled with 15 volume % of epoxy resin, the viscosity is measured at 25°C with the shear rate changed from 100 (1 / s) to 0.01 (1 / s). The thixotropic index, i.e., the TI value, is expressed as the ratio (η1 / η2) of the viscosity η1 measured when the shear rate is 1 (1 / s) to the viscosity η2 measured when the shear rate is 10 (1 / s) is 6 or less. 4 . The spherical boron nitride particles according to claim 1 , wherein the spherical boron nitride particles have a volume-based cumulative diameter D50 of 35 μm or less as evaluated by a laser diffraction scattering method without being treated with a homogenizer. The spherical boron nitride particles according to claim 1 or 2, wherein the average circularity is greater than 0.

80.

6. The spherical boron nitride particles according to claim 1 or 2, wherein the O 1s The semi-quantitative value calculated from the peak intensity was 0.6 or more. 7 . A filler for resin, comprising the spherical boron nitride particles according to claim 1 . 8 . A resin composition comprising a resin and the spherical boron nitride particles according to claim 1 .

9. A method for producing spherical boron nitride particles according to claim 1 or 2, comprising the step of generating cavitation bubbles in a liquid containing raw material spherical boron nitride particles and water.

Citation Information

Patent Citations

  • Boron nitride particles and production method therefor

    WO2015122378A1

  • Spherical boron nitride particles and production method thereof

    WO2015122379A1

  • Method for preparing modified boron nitride nanosheets by water-phase shearing method

    CN110921638A

  • Oriented arrangement boron nitride high-thermal-conductivity composite material and preparation method thereof

    CN113831685A

  • Composition for forming heat-conducting material, heat-conducting material, heat-conducting sheet, and device with heat-conducting layer

    WO2021059806A1