Powdered lithium oxide and preparation method and application thereof

By decomposing lithium peroxide at a mild calcination temperature and mixing it with transition metal oxides, the problem of high energy input and impurities in the lithium oxide production process in the existing technology is solved, and the preparation of high specific surface area lithium oxide and the production of lithium metal oxide are achieved. Efficient conversion.

CN118765262APending Publication Date: 2024-10-11ALBEMARLE GERMANY GMBH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202280088349.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-01-10
Filing Date
2022-12-27
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

It is difficult to economically produce high specific surface area powdered lithium oxide with existing technology, and there are problems with high energy input and the introduction of impurities during the conversion process when mixed with transition metal oxides.

Method used

By using high-purity lithium peroxide for thermal decomposition of lithium oxide at a mild calcination temperature of 280-370°C, controlling the calcination time to obtain high specific surface area lithium oxide, and oxidizing it with transition metals in an oxygen-free or inert atmosphere The materials are mixed to achieve the conversion of the corresponding lithium metal oxide.

Benefits of technology

It achieves the preparation of high specific surface area lithium oxide under low energy input, simplifies the grinding process, and reduces the introduction of impurities. It is suitable for the preparation of efficient lithium metal oxides, especially compounds such as Li2NiO2 and Li5FeO4.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004935152140000051
    Figure BDA0004935152140000051
Patent Text Reader

Abstract

The invention relates to powdered lithium oxide Li2O having a specific surface area according to BET of at least 5 m2 / g and a bulk density of at most 0.3 g / ml, as well as to a method for producing and to the use thereof for producing over-lithiated metal oxides.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to powdered surface-rich lithium oxide, an economical method for producing lithium oxide from lithium peroxide, and the use of lithium oxide for producing overlithiated lithium metal oxides. For the prelithiation of lithium-ion batteries, the overlithiated lithium metal oxides are used as cathode additives. Background Art

[0002] Lithium oxide is currently used as a raw material for the production of glass, glass ceramics, ceramics and for the positive electrodes of lithium batteries. In addition, it can be used to produce lithium hydroxide. Of particular importance is the use of Li2O to produce overlithiated lithium metal oxides, which may also be referred to as lithium-rich metal oxides. These are lithium-containing oxide compounds that have an increased lithium content compared to those used as standard LIB cathode materials and that make this excess content available during the first charge / discharge cycle to compensate for the irreversible lithium losses on the anode side. Examples of overlithiated metal compounds are: Li5FeO4, Li2NiO2, Li6CoO4 or overlithiated manganese-containing spinel compounds, in particular Li 1+x Mn2O4 or Li 1+x Ni 0.5 Mn 1.5 O4, wherein x=>0 to 1.

[0003] Lithium oxide can be produced by the combustion of lithium metal in an oxygen-containing atmosphere. This process is uneconomical because it starts with metallic lithium, which in turn is produced by energy-intensive molten salt electrolysis.

[0004] In addition, lithium oxide can be obtained starting from lithium-based chemical lithium carbonate. The process is based on:

[0005] Li2CO3→Li2O+CO2(1)

[0006] Very high temperatures of about 900-1000° C. are required, preferably under reduced pressure. Due to the intermediate melting of lithium carbonate, the oxide usually forms lumps, which must be ground before further use (DS Appleton, RB Poeppel in: Advances in Ceramics, Vol. 25, "Fabrication and properties of lithium ceramics," ed. IJ Hastings and GW Hollenberg, 1989, 111-116). The strong corrosive effect of molten lithium salts at such high temperatures inevitably leads to the introduction of undesirable impurities into the pyrolysis products and to destructive effects caused by corrosion of the crucible material used.

[0007] In <10 -5At extremely low pressures of 100 torr, Li2CO3 will also undergo thermal decomposition below the melting point of 720°C (T. Takahashi, H. Watanabe, Fusion Eng. Design 8 (1989) 399-405). However, such low pressures are not economically feasible in engineering equipment.

[0008] Mixtures of elemental carbon, such as carbon black, are used to accelerate the decomposition of lithium carbonate (J.-W. Kim, H.-G. Lee, Metallurgical Mater. Trans. B, 32B (2001) 17-24). This carbon thermal decomposition does not require a vacuum, but occurs under an Ar flow and proceeds rapidly at temperatures above about 720° C. (i.e., the melting point of lithium carbonate) according to the following reaction in an alumina crucible:

[0009] Li2CO3+C→Li2O+2CO (2).

[0010] A disadvantage is the strong corrosive effect of the carbonate melt on the aluminum oxide of the used container material. The calcined product is thus contaminated with aluminum.

[0011] Li2O can also be prepared by thermal decomposition of lithium peroxide, Li2O2:

[0012] Li2O2→Li2O+1 / 2O2 (3).

[0013] The advantage of this process is that Li2O can be obtained directly in powder form without going through a melting or sintering phase. The calcination process starting from lithium peroxide also has lower energy costs and is not expected to corrode the container material due to the mild calcination temperature and the avoidance of melting phenomena.

[0014] The document P. Pierron, Bull. France Chim. 1939, 235-238 states that pure white lithium oxide can be obtained by heating lithium peroxide to 300°C in a Pyrex tube. Details such as the pyrolysis time are not recorded. In our own experiments, it was found that at least 20 hours were required to achieve >90% lithium oxide conversion at 300°C.

[0015] US-A-3 321 277 teaches decomposing particulate porous Li2O2 at temperatures between 225° C. and 450° C. to obtain particulate Li2O suitable for CO2 absorption. In this case, calcination at 386° C. under an argon stream required 22 hours and 47 minutes.

[0016] US Pat. No. 4,732,751 describes a process for producing high-purity Li2O by decomposing Li2O2 in an inert atmosphere at an initial temperature of 350 to 450°C and then calcining at 900°C under a slight vacuum.

[0017] KR 20200051931 teaches the production of Li2NiO2 using Li2O with a primary particle size D50 ≤ 5 μm and a secondary particle size D50 between 10 and 100 μm, wherein lithium oxide is produced by thermal decomposition of Li2O2 at a temperature range of 400-600° C. In this example, Li2O is obtained by heat treatment at 420° C. for 3 hours.

[0018] KR 20210079844 teaches the preparation of finely divided lithium peroxide (particle size 1-130 μm, preferably 5-50 μm) and its use in the preparation of lithium oxide. Calcination is carried out at least at 300° C., preferably at 350-650° C. In the experiment, a temperature of 425° C. was described.

[0019] CN 109336139 relates to a method for preparing high-purity nano lithium oxide, characterized in that lithium peroxide is decomposed into lithium oxide at an initial temperature of 350-500°C, then further calcined at 600-800°C, and then ground to a desired fineness by a ball mill.

[0020] The preparation of over-lithiated nickel oxide Li2NiO2 from nickel oxide and Li2O, the latter obtained by thermal decomposition of Li2O2, is described in the literature of J.Kim et al. (Molecules 2019, 24, 4624). The process of calcining Li2O2 in a temperature range of 350 to 600°C was studied. Li2NiO2 was prepared using the Li2O reaction product calcined at 450°C. According to the cited literature (K.Kang et al., Chem.Mater. 2009, 16, 2685-2690), a mixture of NiO and Li2O was ground in a ball mill under argon for one day, and then the homogeneous mixture was pyrolyzed at 650°C under an argon atmosphere for 24 hours (Kang) or 12 hours (Kim) to obtain the final product Li2NiO2.

[0021] The known processes for preparing Li2O from Li2O2 have the disadvantage that they either require long reaction times (at least 20 hours at 300°C) for commercial reasons, or produce granular Li2O, or require relatively high temperatures of at least 350°C. Temperatures ≥350°C are not achievable in conventional fuel-fired reactors and require furnace technology. In addition, pyrolysis temperatures of 350°C and above result in Li2O with a low surface area, which is disadvantageous for solid / solid conversions, for example in the preparation of overlithiated metal oxide compounds (e.g. Li2NiO2) from transition metal oxides and Li2O. In order to achieve a complete conversion of transition metal oxides to Li2O within an acceptable reaction time (<12-24 hours), the material must be intensively pre-coated. When conventional Li2O (e.g. prepared by pyrolysis of Li2O2 at ≥350°C) is used, the process requires very long milling (24 hours). This leads to high costs and, in addition, the introduction of impurities due to abrasion phenomena increases with the milling time.

[0022] Purpose of the Invention

[0023] The object of the present invention is to provide a process which enables the preparation of powdered lithium oxide having a high specific surface area and a low density, which can be ground with the lowest possible energy input and which can be advantageously converted into the corresponding lithium metal oxide when mixed with transition metal oxides, such as nickel oxide.

[0024] Embodiments of the invention

[0025] Surprisingly, it was found that the calcination temperature has a significant effect on the morphology of the lithium oxide formed from the lithium peroxide. This is shown in the summary of the following table:

[0026] Calcination temperature (℃) Calcination time (hours) <![CDATA[Specific surface area (m 2 / g)]]> Bulk density (g / mL) Remark 285 30 14.7 0.1 High liquidity 325 5 13.5 0.12 High liquidity 350 2 8 0.15 High liquidity 380 2 0.3 0.5 High liquidity 425 2 0.4 0.7 High liquidity 450 2 0.23 0.7 High liquidity

[0027] The specific surface area is between 15 and 20 m 2 / g and a peroxide content of at least 97% (the remainder to 100% consisting mainly of LiOH and Li2CO3) was used for the experiments. All experiments were carried out under an inert gas atmosphere consisting of nitrogen, i.e., excluding air, respectively O2, CO2 and H2O.

[0028] It can be seen that within the temperature range of 325 °C, high specific surface area (≥10m 2 / g) of product mass. When reaching and exceeding about 350°C, the specific surface area decreases sharply. At the same time, the bulk density becomes larger.

[0029] Li2O variants with a higher surface area are easier to grind and can therefore reach the particle size range required for conversion with finely divided metal oxides, ie, a particle size of <20 μm, preferably <10 μm, more quickly and with less energy input.

[0030] The lithium peroxide used in the process according to the invention has a Li2O2 content (by weight) of at least 95%, preferably at least 97%, particularly preferably at least 98%, determined by manganese titration. The remainder to 100% consists essentially of LiOH and Li2CO3. When mild calcination temperatures are used, surface-rich lithium oxide is also formed from impure lithium peroxide grades, but this usually contains undesirable particle components, and the content of carbonates and hydroxides remaining in the Li2O interferes with its use in the preparation of overlithiated lithium transition metal oxides.

[0031] The specific surface area of ​​the lithium peroxide used is 5 to 30 m 2 / g, preferably 10 to 30m 2 / g, more preferably 15 to 20m 2 / g.

[0032] The calcination is carried out with the exclusion of ambient air, in particular with the exclusion of compounds that can react with lithium oxide and / or lithium peroxide. These are water (moisture), CO2 and other trace components of air. Therefore, the calcination is preferably carried out under an inert gas (argon, helium, nitrogen) or under a vacuum (<10 mbar). In addition, synthetic, dry and CO2-free air can be used. Due to the mild reaction temperature, there are no special requirements for the container material, that is, most heat-resistant materials, metals as well as glasses (e.g. borosilicate glass, quartz glass) and ceramics (alumina, porcelain, etc.) can be used.

[0033] The calcination is carried out statically, i.e. the Li2O2 starting material is placed in a crucible and calcined in a furnace, or under mixed conditions, i.e. in a stirred tank reactor, a rotating tube or a heatable mixing unit such as a vertical or horizontal dryer, a drum dryer, etc. A fluidized bed reactor can also be used.

[0034] The calcination temperature is 280 to 370° C., preferably 300 to 350° C., more preferably 310 to 350° C., particularly preferably 310 to 340° C. The calcination time for achieving complete conversion depends on the temperature used. Calcination is carried out until the lithium peroxide residual content is a maximum of 5% by weight, preferably a maximum of 2% by weight, particularly preferably a maximum of 1% by weight. This is achieved by a calcination duration of 1 to 30, especially 1 to 20, preferably 1 to 10 hours.

[0035] The specific surface area of ​​the powdered lithium oxide is at least 5 m 2 / g, preferably at least 8m 2 / g, particularly preferably at least 10m 2 / g. The measurement is carried out according to standard specification ASTM D6556 by gas adsorption, a method known as "BET measurement" named after its developers Stephen Brunauer, Paul Hugh Emmett and Edward Teller. In this case, the adsorbed gas is nitrogen.

[0036] The bulk density of the powdered lithium oxide is at most 0.3 g / mL, preferably at most 0.2 g / mL, more preferably at most 0.15 g / mL. The bulk density is determined according to the EN ISO 60 standard.

[0037] The high surface area lithium oxide of the present invention is preferably used to prepare a perlithiated metal compound, wherein the perlithiated metal compound is preferably composed of Li5FeO 4、 Li2NiO 2、 Li6CoO4 or overlithiated manganese-containing spinel compounds, especially Li 1+x Mn2O4 or Li 1+x Ni 0,5 Mn 1,5 O4, where x>0 to 1. For this purpose, the surface-rich lithium oxide is reacted with the corresponding transition metal hydroxide or transition metal oxide or a mixture of hydroxides or oxides of different transition metals.

[0038] Typically, the surface-rich lithium oxide is first intensively mixed and / or ground with the transition metal salt. Preferably, the mixture is ground in a grinding media mill using hard grinding media such as balls, rods, etc., consisting of metals (steel or nickel-based alloys) or hard ceramics (metal oxides, metal carbides, metal nitrides, etc.). The Vickers hardness of the grinding container and the grinding media is at least 400, preferably at least 600. Particularly preferred are materials made of stainless steel or metal oxides, such as aluminum oxide or zirconium oxide. Ball mills, rod mills or hammer mills can be used.

[0039] The subsequent reaction of the mixture of surface-rich lithium oxide and transition metal oxide or hydroxide with the overlithiated metal oxide is usually carried out in the absence of oxygen, i.e. in a reducing atmosphere, or in a vacuum at a pressure of 0.01 to 50 mbar and a temperature of 400 to 900° C. The reducing atmosphere consists of nitrogen or a nitrogen compound. The reducing atmosphere consists of nitrogen or an inert gas, preferably argon or helium. However, there are exceptions to the atmosphere, i.e. when the oxidation state of the transition metal in the starting oxide or hydroxide is lower than that in the final product to be produced. In this case, an oxidizing atmosphere is necessary, at least temporarily. This will be explained with reference to some characteristic conversions.

[0040] For example, according to the prior art (G. Cedar, Chem. Mater. 2004, 2685), overlithiated lithium nickel oxide (Li2NiO2) is prepared by reacting lithium oxide with nickel oxide in an inert (i.e., reducing, oxygen-free) atmosphere:

[0041]

[0042] To this end, nickel oxide is first ground with surface-rich lithium oxide in a ball mill and calcined in an inert argon atmosphere at about 650°C for 1-24 hours. Overlithiated lithium cobalt oxide Li6CoO4 was prepared by solid / solid reaction of CoO and Li2O in a nitrogen atmosphere at 900°C (Yingying Zhou, dissertation 2021, https: / / doi.org / 10.14989 / doctor.k22548). Li5FeO4 was prepared from Li2O and Fe3O4 at 500°C or 800°C in an air atmosphere (MV Blanco et al., Chem. Eng. J. 354, 2018, 370-7), with the formula:

[0043] Fe3O4+7,5Li2O+0,5O2→3Li5FeO4

[0044] Fe3O4 contains two kinds of iron, one in the +2 oxidation state and the other in the +3 oxidation state. To convert the +2 state to the +3 state, the reaction is at least temporarily carried out under oxidizing conditions. In contrast, the synthesis of the same overlithiated metal compound from a ground mixture of Fe2O3 (iron +3 oxidation state) and Li2O is done by first heating to 450°C and then to 750°C under inert conditions (WMDose et al., J. Electrochem. Soc. 2020, 167 160543):

[0045] Fe2O3+5Li2O→2Li5FeO4

[0046] Overlithiated spinels, such as Li 1+x Ni 0,5 Mn 1,5 O4, through the corresponding common cathode material LiNi 0,5 Mn 1,5 O4 is prepared by reacting lithium oxide at 600°C under reducing conditions (G.Gabrielli et al., J.Power Sources, 351, 2017, 35). Example

[0047] Example 1. Preparation of surface-rich Li2O from Li2O2 according to the present invention.

[0048] In an Ar-filled glove box, 15.0 g of lithium peroxide (peroxide content 97.9%) was filled into a ceramic container composed of alumina ceramic and placed in a hinged tube furnace with a borosilicate reaction tube while excluding air. With a slight nitrogen overflow, the furnace temperature was set to 325° C. and maintained at this temperature for 5 hours.

[0049] Yield: 9.5 g of fine white powder (97% of theory).

[0050] Specific surface area: 13.5m 2 / g

[0051] Bulk density: 0.12 g / mL

[0052] Li2O content: 98.6wt% (acidity titration)

[0053] Peroxide content: Undetectable (<0.5wt%)

[0054] Example 2. Preparation of Li2NiO2 from surface-rich Li2O and NiO according to the present invention.

[0055] In an Ar-filled glove box, 1.49 g (50 mmol) of lithium oxide (from Example 1) and 3.73 g (50 mmol) of nickel (II) oxide (nanopowder from Sigma-Aldrich, 99.8% purity based on trace metal impurities) were mixed in an agate mortar and ground using a pestle.

[0056] The mixture is then filled into a crucible composed of alumina and placed in an articulated tube furnace that is substantially air-excluded. The heated, nitrogen-permeated furnace tube is made of Inconel 601.

[0057] The ground mixture was calcined at a furnace temperature of 650°C for 10 hours.

[0058] After cooling to room temperature, the crucible was introduced into an Ar-filled glove box while excluding air.

[0059] Yield: 5.1 g (98% of theory).

[0060] XRD: nearly phase-pure Li2NiO2 (Immm structure); trace (<1%) NiO.

[0061] Uses in.

Claims

1. A method for preparing powdered lithium oxide Li2O, wherein the lithium oxide has a BET value of at least 5 m 2 / g specific surface area and a bulk density of up to 0.3g / ml, Features include: Powdered lithium peroxide Li2O2 with a minimum Li2O2 content of 95 wt.% is calcined at a temperature of 280 to 370°C under inert gas conditions or in vacuum and at a pressure of <10 mbar until the reaction <h2 style=";text-align:left;direction:ltr">Li2O2→Li2O+<h2 style=";text-align:left;direction:ltr"> 1 <h2 style=";text-align:left;direction:ltr"> / 2O2 The conversion rate to lithium oxide Li2O has reached at least 95% based on the weight of the calcined reaction product.

2. The method according to claim 1, characterized in that The residual content of Li2O2 after calcination is at most 2% by weight, preferably at most 1% by weight, based on the weight of the calcination reaction product.

3. The method according to claim 1 or 2, characterized in that: The inert gas is selected from nitrogen, argon, helium or dry CO2-free air.

4. The method according to any one of claims 1 to 3, characterized in that: The calcination time is 1 to 30 hours, particularly 1 to 20 hours, preferably 1 to 10 hours.

5. The method according to any one of claims 1 to 4, characterized in that: The Li2O2 content of the powdered lithium peroxide is at least 97% by weight, preferably at least 98% by weight.

6. The method according to any one of claims 1 to 5, characterized in that: The calcination temperature is 300 to 350°C, preferably 310 to 350°C, and particularly 310 to 340°C.

7. The method according to any one of claims 1 to 6, characterized in that: The lithium peroxide used has a specific surface area according to BET of 5 to 30 m 2 / g, preferably 10 to 30 m 2 More preferably, it is 15 to 20 m / g 2 / g.

8. A powdered lithium oxide Li2O, characterized in that it has a BET value of at least 5m 2 / g specific surface area and a bulk density of at most 0.3g / ml.

9. The powdered lithium oxide according to claim 8, characterized in that it has a specific surface area according to BET of at least 8 m 2 / g, preferably at least 10m 2 / g, more preferably at least 12m 2 / g, still more preferably at least 15m 2 / g.

10. Powdered lithium oxide according to claim 8 or 9, characterized in that it has a bulk density of at most 0.2 g / mL, preferably at most 0.12 g / mL.

11. A method for preparing a perlithiated metal oxide, characterized in that one or more oxidic transition metal salts are thoroughly mixed and / or ground with powdered lithium oxide Li2O as described in any one of claims 8 to 10 or prepared by the method as described in any one of claims 1 to 7, and then reacted in a calcination process at a temperature of 400 to 900° C. under inert gas or in a vacuum of <50 mbar to obtain a perlithiated metal oxide.

12. The method according to claim 11, characterized in that the one or more oxidic transition metal salts are selected from transition metal oxides and transition metal hydroxides.

13. The method according to claim 11 or 12, characterized in that the oxidic transition metal salt is selected from the oxides of nickel, manganese, cobalt or iron, preferably from NiO, CoO, Fe2O3, Fe3O4 and FeO, particularly preferably from NiO, CoO and Fe2O3 or the corresponding hydroxides.

14. The method according to any one of claims 11 to 13, characterized in that the calcination is carried out under reducing conditions, in particular in an oxygen-free atmosphere or in a vacuum of 0.01 to 50 mbar, wherein the oxidation state of the transition metal in the starting material is the same as in the final product.

15. The method according to any one of claims 11 to 14, characterized in that the reducing atmosphere is selected from nitrogen, argon and helium.

16. The method according to any one of claims 11 to 15, characterized in that the overlithiated metal oxide is selected from Li5FeO4, Li2NiO2, Li6CoO4 or an overlithiated manganese-containing spinel compound, in particular Li 1+x Mn2O4 or Li 1+x Ni 0,5 Mn 1, 5O4, where x=>0 to 1.

17. A use of the lithium oxide according to any one of claims 8 to 10 or the lithium oxide prepared by the method according to any one of claims 1 to 7 for preparing a perlithiated metal oxide, in particular selected from Li5FeO4, L i2 NiO2, Li6CoO4 or an over-lithiated manganese-containing spinel compound, preferably Li 1+x Mn2O4 or Li 1+x Ni 0,5 Mn 1,5 O4, where x=>0 to 1, characterized in that one or more oxidic transition metal salts are intensively mixed and / or ground with lithium oxide and then reacted in a reducing atmosphere or in a vacuum of 0.01 to 50 mbar during calcination to obtain an overlithiated metal oxide.