Glass

By optimizing the composition and ingredient content of the glass, the problem of reduced visible light transmittance of high refractive index glass is solved, and a combination of high refractive index and ultraviolet resistance is achieved, making it suitable for applications such as light guide plates.

CN118765266APending Publication Date: 2024-10-11AGC INC
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380023908.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-07
Filing Date
2023-03-02
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

Adding high refractive index components to existing glass can easily lead to a decrease in transmittance of visible light, and the degree of deterioration is high when exposed to ultraviolet rays, making it impossible to effectively suppress the decrease in transmittance.

Method used

By optimizing the composition of the glass to ensure the content range of TeO2, P2O5, B2O3, TiO2 and other components, combined with the specific oxide molar ratio and calculation of parameters A and B, a refractive index of 1.94 or above and a degree of deterioration in ultraviolet irradiation tests were prepared Glass with ΔT of 2.2% or less.

Benefits of technology

Achieving a high refractive index glass while suppressing the decrease in transmittance of visible light and improving resistance to ultraviolet rays, making it suitable for applications such as light guide plates.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005012492910000101
    Figure BDA0005012492910000101
  • Figure BDA0005012492910000151
    Figure BDA0005012492910000151
  • Figure BDA0005012492910000161
    Figure BDA0005012492910000161
Patent Text Reader

Abstract

Provided is a glass having a high refractive index and capable of suppressing a decrease in transmittance to visible light. The glass (10) has a refractive index of 1.94 or more, an internal transmittance of 70% or more with respect to light having a wavelength of 440 nm at a plate thickness of 10 mm, and a degree of deterioration ([Delta] T) of 2.2% or less in an ultraviolet irradiation test.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to glass. Background Art

[0002] In recent years, glass with a high refractive index has been sought. In particular, in wearable devices such as head-mounted displays that realize AR (Augumented Reality), VR (Virtual Reality), and MR (Mixed Reality), as shown in Patent Document 1, a high refractive index for visible light is required as a light guide plate.

[0003] Prior art literature

[0004] Patent Literature

[0005] Patent Document 1: International Publication No. 2020 / 090051 Summary of the invention

[0006] Glass may have a reduced transmittance to visible light due to various important factors such as coloration caused by an increase in high refractive index components, incorporation of impurities, and changes over time. Therefore, it is necessary to have a high refractive index and suppress a reduction in the transmittance to visible light.

[0007] The present invention has been made in view of the above-mentioned problems, and an object of the present invention is to provide a glass having a high refractive index and capable of suppressing a decrease in transmittance of visible light.

[0008] In order to solve the above problems and achieve the purpose, the glass involved in the present disclosure has a refractive index of 1.94 or more, an internal transmittance of 70% or more for light with a wavelength of 440 nm when the plate thickness is 10 mm, and a degradation degree ΔT in an ultraviolet irradiation test of 2.2% or less. Here, the degradation degree ΔT in the ultraviolet irradiation test is obtained by the following formula (1).

[0009] ΔT(%)={(T0-T1) / T0}·100···(1)

[0010] The transmittance T1 is the value obtained by applying UV irradiation of 50 mW / cm2 to the surface of the glass with a thickness of 1 mm. 2 The external transmittance of the glass at a wavelength of 470 nm after irradiation with ultraviolet rays at a wavelength of 365 nm for 10 minutes is the external transmittance of the glass at a wavelength of 470 nm before irradiation with the ultraviolet rays. Transmittance T0 is the external transmittance of the glass at a wavelength of 470 nm before irradiation with the ultraviolet rays.

[0011] According to the present invention, it is possible to provide glass having a high refractive index and capable of suppressing a decrease in transmittance of visible light. BRIEF DESCRIPTION OF THE DRAWINGS

[0012] Figure 1It is a schematic diagram of the glass involved in this embodiment.

[0013] Figure 2 This is a cross-sectional view when the glass according to the present embodiment is made into a glass plate. DETAILED DESCRIPTION

[0014] Hereinafter, the preferred embodiments of the present invention will be described in detail with reference to the accompanying drawings. It should be noted that the present invention is not limited to the embodiments, and when there are multiple embodiments, the technical solutions formed by combining the embodiments are included. In addition, the numerical values ​​include the range of rounding.

[0015] (Glass)

[0016] Figure 1 Schematic diagram of the glass involved in this embodiment. Figure 1 As shown, although the glass 10 involved in this embodiment is a plate-shaped glass plate, the shape of the glass 10 is not limited to the plate shape and can be any shape. In this embodiment, the glass 10 is used as a light guide plate. More specifically, the glass 10 is used as a light guide plate for a head-mounted display. A head-mounted display refers to a display device (wearable device) worn on a person's head. However, the use of the glass 10 is arbitrary and is not limited to being used as a light guide plate. In addition, it is not limited to being used for a head-mounted display.

[0017] (Glass composition)

[0018] Next, the composition of glass 10 will be described.

[0019] (TeO2)

[0020] TeO2 is a component that promotes vitrification and contributes to high refractive index. On the other hand, if it is contained in large quantities, the mechanical properties of the glass will be reduced. Therefore, the glass 10 is expressed in mole % based on oxides, and the content of TeO2 is preferably 0.1% or more and less than 40.0%, more preferably 0.5% to 35.0%, more preferably 1.0% to 33.0%, more preferably 2.0% to 30.0%, more preferably 5.0% to 27.0%, more preferably 8.0% to 26.0%, more preferably 10.0% to 25.6%, more preferably 12.0% to 25.5%, and further preferably 18.0% or more. By having the content of TeO2 within this range, the glass 10 can be made to have a high refractive index and suppress the reduction of the transmittance to visible light.

[0021] It should be noted that the content here refers to the mole % of the oxide content when the mole % of the total amount of the glass 10 is 100% expressed as the mole % of the oxide basis. For example, "the content of TeO2 is greater than 10.1%" means that the glass 10 contains more than 10.1% of TeO2 when the mole % of the total amount of the glass 10 is 100% expressed as the mole % of the oxide basis. In addition, the upper limit and the lower limit of the numerical range can be appropriately combined, and the same applies to the following.

[0022] (P2O5)

[0023] P2O5 is a glass-forming component that stabilizes the glass. On the other hand, if it is contained in large amounts, the refractive index decreases. Therefore, the glass 10 is expressed in mole percent based on oxides, and the content of P2O5 is preferably 0% to 30.0%, more preferably 0.1% to 27%, more preferably 1.0% to 24%, more preferably 2.0% to 23%, more preferably 3.0% to 17%, more preferably 4.0% to 12%, more preferably 5.0% to 9.7%, more preferably 9.6% or less, and further preferably 9.5% or less. By making the content of P2O5 within this range, the glass 10 can have a high refractive index and suppress the reduction in the transmittance of visible light. Among them, the glass 10 may not contain P2O5.

[0024] (B2O3)

[0025] B2O3 is a glass-forming component, and is a component that helps to improve glass stability and manufacturing characteristics. However, if it is contained in large quantities, the refractive index is likely to decrease. Therefore, the glass 10 is expressed in mole % based on oxides, and the content of B2O3 is preferably 0% to 40%, more preferably 5.0% to 35.0%, more preferably 10.0% to 29.0%, more preferably 15.0% to 25.0%, and further preferably 20.0% to 22.0%. By making the content of B2O3 within this range, the glass 10 can have a high refractive index and suppress the reduction of the transmittance of visible light. Among them, the glass 10 may not contain B2O3.

[0026] (Li2O)

[0027] Li2O is a component that can improve the mechanical properties of glass. On the other hand, if it is contained in too much, it becomes easy to lose transparency and the manufacturing characteristics deteriorate. Therefore, the glass 10 is preferably 0% to 15.0% in terms of mol% based on oxides, more preferably 0.10% to 10.0%, more preferably 0.50% to 8.0%, and further preferably 1.0% to 4.0%. By making the content of Li2O within this range, the glass 10 can have a high refractive index and suppress the reduction of the transmittance of visible light. Among them, the glass 10 does not need to contain Li2O.

[0028] (Na2O)

[0029] The glass 10 is expressed in terms of mole % based on oxides, and the content of Na2O is preferably 0% to 15.0%, more preferably 0.10% to 10.0%, more preferably 0.50% to 5.0%, and more preferably 1.0% to 3.0%. In addition, it can be said that the content of Na2O is preferably 1.0% or less. By making the content of Na2O within this range, the glass 10 can have a high refractive index and suppress the reduction of the transmittance of visible light. However, the glass 10 may not contain Na2O.

[0030] (K2O)

[0031] The glass 10 preferably has a K2O content of 0% to 15.0%, more preferably 0.10% to 10.0%, more preferably 0.50% to 5.0%, and more preferably 1.0% to 3.0%, expressed as a mole % based on oxides. In addition, it can also be said that the K2O content is preferably 1.0% or less. By setting the K2O content to this range, the glass 10 can have a high refractive index and suppress a decrease in the transmittance of visible light. However, the glass 10 may not contain K2O.

[0032] (TiO2)

[0033] TiO2 is a high refractive index component and suppresses the decrease in transmittance, but if it is contained in large quantities, the internal transmittance of the glass will be reduced. Therefore, the content of TiO2 in glass 10 is preferably 0% to 32.0%, more preferably 0.20% to 26.0%, more preferably 0.50% to 20.0%, more preferably 1.0% to 13.0%, and more preferably 2.0% to 10.0%, expressed as a mole % based on the oxide. In addition, the content of K2O is also preferably 1.0% to 7.0%, and it can be said that it is also preferably less than 2.0%. By making the content of TiO2 within this range, the glass 10 can have a high refractive index and suppress the decrease in the transmittance of visible light. Among them, the glass 10 may not contain TiO2.

[0034] (Ta2O5)

[0035] Ta2O5 is a component that can increase the refractive index, but if it is contained in too much, it becomes easy to lose clarity and the manufacturing characteristics deteriorate. Therefore, the glass 10 is expressed in mole % based on the oxide, and the content of Ta2O5 is preferably 0% to 20.0%, more preferably 0.1% to 10.0%, more preferably 0.5% to 5.0%, and further preferably 1.00% to 2.0%. By making the content of Ta2O5 within this range, the glass 10 can have a high refractive index and suppress the reduction of the transmittance of visible light. Among them, the glass 10 does not need to contain Ta2O5.

[0036] (WO3)

[0037] WO3 is a component that can increase the refractive index of glass, but if it is contained in too much, the internal transmittance decreases. Therefore, the glass 10 is expressed in mole % based on the oxide, and the content of WO3 is preferably 0% to 15.0%, more preferably 0.10% to 10.0%, more preferably 0.50% to 5.0%, and more preferably 1.0% to 2.0%. In addition, the content of WO3 is also preferably 0.4% or less. By making the content of WO3 within this range, the glass 10 can have a high refractive index and suppress the reduction of the transmittance of visible light. Among them, the glass 10 may not contain WO3.

[0038] (Nb2O5)

[0039] Nb2O5 is a component that increases the refractive index of glass and improves mechanical properties, but if it is contained in large amounts, it becomes easy to devitrify and the manufacturing characteristics deteriorate. Therefore, the content of Nb2O5 in glass 10, expressed as mole % based on oxides, is preferably 0% or more and less than 15.0%, more preferably 0.10% to 12.0%, more preferably 0.50% to 10.0%, more preferably 1.0% to 8.0%, more preferably 2.0% to 7.0%, and further preferably 3.0% to 6.5%. By making the content of Nb2O5 within this range, the glass 10 can have a high refractive index and suppress the reduction of the transmittance of visible light. Among them, the glass 10 does not need to contain Nb2O5.

[0040] (ZrO2)

[0041] ZrO2 is a component that can improve mechanical properties while increasing the refractive index, but if it is contained in too much, it becomes easy to lose clarity and the manufacturing characteristics deteriorate. Therefore, the glass 10 is expressed in mole % based on the oxide, and the content of ZrO2 is preferably 0% to 20%, more preferably 0.10% to 15.0%, more preferably 0.50% to 10.0%, more preferably 1.0% to 9.0%, more preferably 2.0% to 8.0%, more preferably 3.0% to 6.0%, and it can be said that it is further preferably 5.0% or less. By making the content of ZrO2 within this range, the glass 10 can have a high refractive index and suppress the reduction of the transmittance of visible light. Among them, the glass 10 may not contain ZrO2.

[0042] (Bi2O3)

[0043] Bi2O3 is a component that can greatly increase the refractive index, but if contained in large amounts, it will not only deteriorate the manufacturing characteristics but also reduce the transmittance. Therefore, the content of Bi2O3 in glass 10, expressed as a mole % based on the oxide, is preferably greater than 15% and less than 45%, more preferably 20% to 40%, more preferably 24% to 38%, more preferably 28% to 36.0%, more preferably 30.0% to 34.0%, more preferably 30.0% to 33.0%, more preferably 30.0% to 32.0%, and further preferably 30.0% to 31.0%. By making the content of Bi2O3 within this range, the glass 10 can have a high refractive index and suppress the reduction of the transmittance of visible light. Among them, the glass 10 may not contain Bi2O3.

[0044] (ZnO)

[0045] The glass 10 preferably has a ZnO content of 0% to 20%, more preferably 0.5% to 15%, more preferably 1.0% to 10%, more preferably 1.5% to 8.0%, more preferably 2.0% to 6.0%, more preferably 3.0% to 5.4%, and further preferably 4.0% to 5.3%, expressed in terms of mole percent based on oxides. By setting the ZnO content within this range, the glass 10 can have a high refractive index and suppress a decrease in the transmittance of visible light. However, the glass 10 may not contain ZnO.

[0046] (SrO)

[0047] The glass 10 preferably has a SrO content of 0% to 20%, more preferably 0.5% to 15%, more preferably 1.0% to 10%, more preferably 1.5% to 8.0%, and more preferably 2.0% to 5.0%, expressed as a mole % based on oxides. In addition, the SrO content is also preferably 2.0% or less. By setting the SrO content to this range, the glass 10 can have a high refractive index and suppress a decrease in the transmittance of visible light. However, the glass 10 may not contain SrO.

[0048] (La2O3)

[0049] The glass 10 preferably contains La2O3 in an amount of 0% to 30% expressed as a mole percent of an oxide basis, more preferably 0.5% to 20%, more preferably 1.0% to 15%, more preferably 1.5% to 10%, and more preferably 2.0% to 5.0%. In addition, the La2O3 content is also preferably 2.0% or less. By making the La2O3 content within this range, the glass 10 can have a high refractive index and suppress the reduction of the transmittance of visible light. However, the glass 10 may not contain La2O3.

[0050] (SiO2)

[0051] The glass 10 preferably has a SiO2 content of 0% to 30%, more preferably 0.5% to 20%, more preferably 1.0% to 15%, more preferably 1.5% to 10%, more preferably 2.0% to 9.0%, more preferably 3.0% to 9.0%, more preferably 4.0% to 8.0%, and even more preferably 8.0% or less, expressed as a mole % based on oxides. By making the SiO2 content within this range, the glass 10 can have a high refractive index and suppress the reduction of the transmittance of visible light. However, the glass 10 may not contain SiO2.

[0052] (P2O5+TeO2+B2O3+TiO2+Ta2O5+WO3+ZrO2+Bi2O3+ZnO)

[0053] Glass 10 preferably has a total content of (P2O5+TeO2+B2O3+TiO2+Ta2O5+WO3+ZrO2+Bi2O3+ZnO) based on the oxide molar ratio, i.e., P2O5, TeO2, B2O3, TiO2, Ta2O5, WO3, ZrO2, Bi2O3, and ZnO of 70% or more, more preferably 73% to 99.5%, more preferably 75% to 98.0%, more preferably 78% to 97.0%, more preferably 85% to 96.0%, more preferably 90% to 95.0%, and further preferably 92% to 94.0%. By making the total content of these components within this range, glass 10 can have a high refractive index and suppress the reduction of the transmittance of visible light. Among them, glass 10 can contain at least one of these components.

[0054] (Parameter A)

[0055] The parameter A of the glass 10 is described. The parameter A is a parameter related to the Young's modulus calculated from the composition of the glass 10. For example, there is a tendency that the greater the value of the parameter A, the higher the degree of degradation in the ultraviolet irradiation test. The parameter A is calculated as shown in the following formula (A).

[0056] A=c(P2O5) 2 +c(Nb2O5) 2 -c(TiO2) 2 ···(A)

[0057] Here, c in formula (A) is the content (%) of the oxide shown in parentheses relative to the entire glass 10 when expressed in mol % based on the oxide. That is,

[0058] c(P2O5) is the content (%) of P2O5 expressed as mol% based on oxide,

[0059] c(Nb2O5) is the content (%) of Nb2O5 when expressed as mole % based on oxide,

[0060] c(TiO2) is the TiO2 content (%) expressed as mol% based on oxide.

[0061] The parameter A of the glass 10 is preferably 270 or less, more preferably -20 to 200, more preferably -10 to 170, more preferably -7 to 150, more preferably -5 to 140, more preferably -4 to 130, and even more preferably -3 to 120. By setting the parameter A within this range, the degree of degradation can be kept low, and the concern of a decrease in transmittance can be suppressed.

[0062] It should be noted that the glass 10 may contain oxides other than the oxides listed in formula (A), and the content of oxides other than the oxides listed in formula (A) is not used for calculating the parameter A. That is, it can be said that the value of the parameter A does not change due to the presence or absence of oxides other than the oxides listed in formula (A).

[0063] In addition, the glass 10 is not limited to contain all the oxides listed in the formula (A). In this case, the value of the right side of the formula (A) for the oxides listed in the formula (2) but not contained in the glass 10 is zero. That is, for example, when the glass 10 does not contain P2O5, the parameter A is calculated by taking c(P2O5) of the formula (A) as zero.

[0064] (Parameter B)

[0065] The parameter B of the glass 10 is described. The parameter B is a parameter related to the degree of degradation in the ultraviolet irradiation test calculated based on the composition of the glass 10. For example, there is a tendency that the greater the value of the parameter B, the higher the degree of degradation in the ultraviolet irradiation test. The parameter B is calculated as shown in the following formula (B).

[0066] B=0.13455·2.7183 (0.014912·A) ···(B)

[0067] Here, A in formula (B) is parameter A.

[0068] The parameter B of the glass 10 is preferably 2.5 or less, more preferably 2.3 or less, preferably 1.8 or less, more preferably 1.5 or less, more preferably 1.3 or less, more preferably 1.1 or less, more preferably 1.0 or less, more preferably 0.8 or less, more preferably 0.7 or less, more preferably 0.6 or less, and further preferably 0.5 or less. By setting the parameter B within this range, the degree of degradation can be kept low, and concerns about reduced transmittance can be suppressed.

[0069] (Fe, Cr, Ni content)

[0070] The total content of Fe, Cr and Ni in glass 10 is preferably less than 4ppm, more preferably less than 3ppm, more preferably less than 2ppm, more preferably less than 1ppm, more preferably less than 0.7ppm, more preferably less than 0.5ppm, more preferably less than 0.3ppm, and more preferably less than 0.1ppm. Here, Fe, Cr and Ni do not refer only to the single metals of Fe, Cr and Ni contained in glass 10, but may include single metals and compounds of Fe, Cr and Ni. That is, it can be said that the total content of Fe, Cr and Ni refers to the content of single metals containing Fe, Cr and Ni and the content of ions of Fe, Cr and Ni in the compound. By making the total content of Fe, Cr and Ni as coloring transition metals within this range, it is possible to suppress the transmittance of glass 10 to visible light from becoming low, so that glass 10 has a high transmittance relative to visible light. The total content of Fe, Cr and Ni can be measured using ICP mass spectrometry. As a measuring instrument, for example, Agilent 8800 manufactured by Agilent Technologies can be used.

[0071] The total content of Fe, Cr, Ni, Cu, Mn, Co and V in the glass 10 is preferably less than 4 ppm, more preferably 3 ppm or less, more preferably 2 ppm or less, and further preferably 1 ppm or less, in terms of mass ratio, relative to the entire glass 10. Here, Fe, Cr, Ni, Cu, Mn, Co and V, like the above-mentioned Fe, Cr and Ni, do not refer only to the single metals of Fe, Cr, Ni, Cu, Mn, Co and V contained in the glass 10, but may include single metals and compounds of Fe, Cr, Ni, Cu, Mn, Co and V. That is, it can be said that the total content of Fe, Cr, Ni, Cu, Mn, Co and V includes the content of single metals of Fe, Cr, Ni, Cu, Mn, Co and V and the content of ions of Fe, Cr, Ni, Cu, Mn, Co and V in the compound. By making the total content of the above-mentioned components as coloring transition metals within this range, it is possible to suppress the transmittance of the glass 10 with respect to visible light from being reduced, and make the glass 10 have a high transmittance with respect to visible light. The total content of the above components can be measured by ICP mass spectrometry.

[0072] (Pb content)

[0073] The total content of Pb in the glass 10 is preferably less than 1000 ppm, more preferably less than 100 ppm, and further preferably less than 10 ppm, relative to the entire glass 10 in terms of mass ratio. That is, it is preferred that the glass 10 does not substantially contain Pb. The Pb here, like the above-mentioned Fe, Cr, and Ni, does not refer only to the single metal of Pb contained in the glass 10, but may include single metals and compounds of Pb. That is, it can be said that the content of Pb includes the content of single metal of Pb and the content of Pb ions in the compound. The content of Pb can be measured by ICP mass spectrometry.

[0074] In addition, the glass 10 preferably contains boric acid or phosphoric acid. That is, the glass 10 is preferably boric acid glass, phosphoric acid glass, or fluorophosphate glass.

[0075] (Characteristics of glass)

[0076] Next, the characteristics of the glass 10 will be described.

[0077] (Refractive index n d )

[0078] The refractive index n of glass 10 is d 1.94 or more, more preferably 1.95 or more, more preferably 1.97 or more, more preferably 1.99 or more, more preferably 2.01 or more, more preferably 2.03 or more, more preferably 2.05 or more, more preferably 2.06 or more, more preferably 2.07 or more, more preferably 2.08 or more, and further preferably 2.09 or more. d In this range, a high refractive index for visible light can be achieved. The refractive index n of the glass 10 is d It is preferably 2.20 or less, more preferably 2.17 or less, more preferably 2.15 or less, and still more preferably 2.13 or less. That is, the refractive index n of the glass 10 is d It is preferably 1.94 to 2.20, more preferably 1.95 to 2.17, more preferably 1.97 to 2.15, more preferably 1.99 to 2.13, more preferably 2.01 to 2.13, more preferably 2.03 to 2.13, more preferably 2.05 to 2.13, more preferably 2.06 to 2.13, more preferably 2.07 to 2.13, more preferably 2.08 to 2.13, and further preferably 2.09 to 2.13.

[0079] It should be noted that the refractive index n d Refers to the refractive index at the helium d line (wavelength 587.6nm). Refractive index n d The measurement can be performed using the V-block method.

[0080] (Deterioration degree ΔT)

[0081] The degree of degradation ΔT of the glass 10 in the ultraviolet irradiation test is 2.2% or less, preferably 1.8% or less, more preferably 1.5% or less, more preferably 1.4% or less, more preferably 1.3% or less, more preferably 1.2% or less, more preferably 1.0% or less, more preferably 0.9% or less, more preferably 0.8% or less, more preferably 0.7% or less, and further preferably 0.5% or less. By setting the degree of degradation ΔT to be within this range, the transmittance can be suppressed from decreasing even when irradiated with ultraviolet rays, and the transmittance to visible light can be suppressed from decreasing.

[0082] Here, the degree of degradation in the ultraviolet irradiation test is calculated by the following formula (1).

[0083] ΔT(%)={(T0-T1) / T0}·100···(1)

[0084] The transmittance T1 in formula (1) refers to the transmittance of the surface of the glass 10 with a thickness of 1 mm under UV illumination of 50 mW / cm 2 The external transmittance of light of wavelength 470 nm of glass 10 after irradiation with ultraviolet light of wavelength 365 nm for 10 minutes. More specifically, the UV illuminance on the glass surface was adjusted to 50 mW / cm using an ultraviolet integrated light meter (manufactured by Ushio Electric Co., Ltd.: UIT-250). 2 The surface of the glass 10 is irradiated with ultraviolet rays of 365 nm for 10 minutes using a UV-LED irradiation device (manufactured by SUN ENERGY Co., Ltd.: LSS-24). The external transmittance of light of a wavelength of 470 nm is measured using a spectrophotometer (manufactured by Hitachi High-Technologies Corporation: U-4100) for the glass 10 irradiated with ultraviolet rays in this way, and the value is taken as the transmittance T1. On the other hand, the transmittance T0 in formula (1) is the transmittance of the glass 10 of a wavelength of 470 nm before ultraviolet irradiation. That is, the external transmittance of light of a wavelength of 470 nm is also measured in advance using a spectrophotometer (manufactured by Hitachi High-Technologies Corporation: U-4100) for the glass 10 before ultraviolet irradiation as described above, and the value is taken as the transmittance T0.

[0085] (Young's modulus)

[0086] The Young's modulus of the glass 10 is preferably 60 GPa or more and less than 100 GPa, more preferably 62 GPa to 95 GPa, and even more preferably 65 GPa to 90 GPa. By making the Young's modulus so high, the breakage of the glass 10 can be appropriately suppressed. It should be noted that the Young's modulus can be measured based on the propagation of ultrasonic waves using 38DLPLUS manufactured by OLYMPUS.

[0087] (Wavelength λ 70 )

[0088] Here, the wavelength at which the internal transmittance is 70% when the plate thickness (thickness) is 10 mm is referred to as wavelength λ. 70 That is, the wavelength λ 70 The wavelength of light with a transmittance of 70% for a sample with a thickness of 10 mm. The wavelength λ of glass 10 with a thickness of 10 mm 70 Preferably, the wavelength λ of the glass 10 is 455 nm or less, more preferably 445 nm or less, more preferably 435 nm or less, more preferably 430 nm or less, more preferably 425 nm or less, and further preferably 420 nm or less. 70 It is preferably 390 nm or more, more preferably 395 nm or more, and further preferably 400 nm or more.

[0089] That is, it can be said that the wavelength λ of the glass 10 70 It is preferably 390 nm to 455 nm, more preferably 395 nm to 445 nm, more preferably 400 nm to 435 nm, more preferably 400 nm to 430 nm, more preferably 400 nm to 425 nm, and further preferably 400 nm to 420 nm.

[0090] By making the wavelength λ 70 In this range, high transmittance to visible light can be achieved. 70 The internal transmittance can be calculated based on the measured values ​​of two external transmittances with different plate thicknesses and the following formula (2). It should be noted that the external transmittance refers to the transmittance including surface reflection loss. In formula (2), X is the internal transmittance of glass with a thickness of 10 mm, T1 and T2 are the external transmittances, and Δd is the difference in thickness of the sample. The external transmittance can be measured using a spectrophotometer (manufactured by Hitachi High-Technologies Corporation: U-4100) on a sample with a double-sided mirror polished to a plate thickness of 10 mm.

[0091]

[0092] (Light transmittance)

[0093] When the plate thickness (thickness) of the glass 10 is 10 mm, the internal transmittance of light of a wavelength of 440 nm is preferably 70% or more, more preferably 75% or more, more preferably 78% or more, more preferably 81% or more, more preferably 84% or more, more preferably 87% or more, more preferably 89% or more, more preferably 90% or more, more preferably 91% or more, and further preferably 92% or more.

[0094] By setting the internal transmittance of light with a wavelength of 440 nm to be within this range, a high transmittance for visible light can be achieved. The internal transmittance of glass with a thickness of 10 mm can be obtained from the measured values ​​of two types of external transmittances with different plate thicknesses and equation (2).

[0095] (Glass form)

[0096] The glass 10 involved in this embodiment is preferably an optical glass, preferably a glass plate with a thickness of 0.01mm to 2.0mm. If the thickness is 0.01mm or more, the breakage of the glass 10 during handling and processing can be suppressed. In addition, the deflection of the glass 10 due to its own weight can be suppressed. The thickness is more preferably 0.1mm or more, more preferably 0.2mm or more, and more preferably 0.3mm or more. On the other hand, if the thickness is 2.0mm or less, the optical element obtained using the glass 10 can be lightweight. The thickness is more preferably 1.5mm or less, more preferably 1.0mm or less, and more preferably 0.8mm or less.

[0097] When the glass 10 according to the present embodiment is a glass plate, the area of ​​the main surface is preferably 8 cm 2 If the area is 8cm 2 More than 30 cm2 can be used to configure a large number of optical elements, thereby improving productivity. 2 More preferably, 170 cm 2 More preferably, 300 cm 2 More than 1000cm 2 On the other hand, if the area is 6500cm 2 The area is preferably 4500 cm 2 Below, more preferably 4000cm 2 Below, more preferably 3000cm 2 Below, particularly preferably 2000cm 2 the following.

[0098] When the glass 10 according to the present embodiment is a glass plate, 25 cm of the main surface 2The LTV (Local Thickness Variation) in is preferably less than 2 μm. By having a flatness within this range, a nanostructure of a desired shape can be formed on the main surface using an imprinting technique or the like, and the desired light-guiding properties can be obtained. In particular, in the light guide, ghosting and deformation caused by differences in optical path lengths can be prevented. The LTV is more preferably less than 1.5 μm, further preferably less than 1.0 μm, and particularly preferably less than 0.5 μm.

[0099] When the glass 10 involved in this embodiment is made into a circular glass plate with a diameter of 8 inches, the warping is preferably 50 μm or less. If the warping of the glass 10 is 50 μm or less, a nanostructure of a desired shape can be formed on the main surface using an imprinting technique or the like, and the desired light-guiding properties can be obtained. When a plurality of light guides are to be obtained, light guides with stable quality are obtained. The warping of the glass 10 is more preferably 40 μm or less, further preferably 30 μm or less, and particularly preferably 20 μm or less.

[0100] In addition, when the glass 10 involved in this embodiment is made into a circular glass plate with a diameter of 6 inches, the warping is preferably 30 μm or less. If the warping of the glass 10 is 30 μm or less, a nanostructure of a desired shape can be formed on the main surface using an imprinting technique or the like, and the desired light-guiding properties can be obtained. When a plurality of light guides are to be obtained, light guides with stable quality are obtained. The warping of the glass 10 is more preferably 20 μm or less, further preferably 15 μm or less, and particularly preferably 10 μm or less.

[0101] In addition, when the glass 10 involved in the present embodiment is made into a square glass plate with each side being 6 inches, the warping is preferably 100 μm or less. If the warping of the glass 10 is 100 μm or less, a nanostructure of a desired shape can be formed on the main surface using an imprinting technique or the like, and the desired light-guiding properties can be obtained. When a plurality of light guides are to be obtained, light guides of stable quality are obtained. The warping of the glass 10 is more preferably 70 μm or less, further preferably 50 μm or less, further preferably 35 μm or less, and particularly preferably 20 μm or less.

[0102] Figure 2 The "warp" refers to the difference C between the maximum value B and the minimum value A of the distance in the vertical direction between the reference line G1D of the glass plate G1 and the center line G1C of the glass plate G1 in any cross section passing through the center of the main surface G1F of the glass plate G1 when the glass 10 involved in the present embodiment is made into the glass plate G1 and is orthogonal to the main surface G1F of the glass plate G1.

[0103] The intersection line of the above-mentioned arbitrary cross section and the main surface G1F of the glass plate G1 is set as the bottom line G1A. The intersection line of the above-mentioned arbitrary cross section and the other main surface G1G of the glass plate G1 is set as the top line G1B. Here, the center line G1C is a line connecting the center of the plate thickness direction of the glass plate G1. The center line G1C is calculated by finding the midpoint of the bottom line G1A and the top line G1B with respect to the laser irradiation direction described later.

[0104] The reference line G1D is obtained as follows. First, the bottom line G1A is calculated based on a measurement method that eliminates the influence of the dead weight. A straight line is obtained from the bottom line G1A using the least square method. The obtained straight line is the reference line G1D. As a measurement method that eliminates the influence of the dead weight, a known method can be used.

[0105] For example, the main surface G1F of the glass plate G1 is supported at three points, and the glass plate G1 is irradiated with laser light using a laser displacement meter to measure the heights of the main surface G1F and another main surface G1G of the glass plate G1 from an arbitrary reference plane.

[0106] Next, the glass plate G1 is turned over, and the other main surface G1G is supported at three points opposite to the three points supporting the one main surface G1F, and the heights of the main surface G1F and the other main surface G1G of the glass plate G1 from an arbitrary reference plane are measured.

[0107] The influence of the self-weight is eliminated by finding the average value of the heights of the measurement points before and after the inversion. For example, before inversion, the height of the main surface G1F is measured as described above. After the glass plate G1 is inverted, the height of the other main surface G1G is measured at the position corresponding to the measurement point of the main surface G1F. Similarly, before inversion, the height of the other main surface G1G is measured. After the glass plate G1 is inverted, the height of the main surface G1F is measured at the position corresponding to the measurement point of the other main surface G1G.

[0108] The warpage is measured by, for example, a laser displacement meter.

[0109] In addition, in the glass 10 involved in the present embodiment, the surface roughness Ra of the main surface is preferably less than 2 nm. By having Ra in this range, a nanostructure of a desired shape can be formed on the main surface using an imprinting technique or the like, and the desired light-guiding properties can be obtained. In particular, in the light guide, diffuse reflection at the interface is suppressed, and ghosting and deformation can be prevented. The Ra is more preferably less than 1.7 nm, further preferably less than 1.4 nm, further preferably less than 1.2 nm, and particularly preferably less than 1 nm. Here, the surface roughness Ra is the arithmetic mean roughness defined in JIS B0601 (2001). In this specification, the value is measured using an atomic force microscope (AFM) on an area of ​​10 μm×10 μm.

[0110] (Glass Manufacturing Method)

[0111] The manufacturing method of the glass 10 involved in this embodiment is not particularly limited, and for example, existing plate glass manufacturing methods such as float method, melting method and rolling method can be used. In addition, a known method such as slicing a cast glass block to cut out a glass plate can also be used. Among them, in order to suppress the deterioration of the transmittance of the glass 10 due to the mixing of impurities, it is preferred that the material of the container (crucible) into which the raw materials are placed when the raw materials are melted is Au or Au alloy.

[0112] Furthermore, for the glass 10 of the present embodiment, it is preferred that an operation of increasing the water content in the molten glass is performed in a melting process of heating and melting glass raw materials in a melting vessel to obtain molten glass. The operation of increasing the water content in the glass is not limited, and for example, a process of adding water vapor to the melting atmosphere and a process of bubbling a gas containing water vapor into the melt are considered. The operation of increasing the water content is not essential and can be performed for purposes such as increasing transmittance and improving clarity.

[0113] In addition, the glass 10 of the present embodiment containing alkali metal oxides such as Li2O and Na2O can be chemically strengthened by replacing Li ions with Na ions or K ions, and replacing Na ions with K ions. That is, if chemical strengthening treatment is performed, the strength of the optical glass can be improved.

[0114] (Effect)

[0115] As described above, the glass 10 according to the present embodiment has a refractive index of 1.94 or more, an internal transmittance of 70% or more for light of a wavelength of 440 nm when the thickness is 10 mm, and a degree of degradation ΔT of 2.2% or less in an ultraviolet irradiation test.

[0116] Here, glass with a high refractive index is sometimes required. In this regard, the glass 10 involved in the present embodiment can achieve a high refractive index by having a refractive index of 1.94 or more. In addition, the transmittance of glass to visible light sometimes decreases. For example, glass sometimes undergoes a so-called solarization effect in which it is colored and the transmittance decreases when irradiated with ultraviolet rays. In this regard, the glass 10 involved in the present embodiment can suppress the decrease in transmittance even when irradiated with ultraviolet rays by making the degree of degradation ΔT in the ultraviolet irradiation test within the above range. In addition, by making the internal transmittance within the above range, the transmittance can be kept high. In this way, according to the present embodiment, the decrease in the transmittance of visible light can be suppressed while making the glass 10 have a high refractive index.

[0117] The glass 10 according to the present embodiment preferably has a Nb2O5 content of 0% or more and less than 15% expressed in terms of mol% based on oxides. This allows the glass 10 to have a high refractive index while suppressing a decrease in the transmittance of visible light.

[0118] The glass 10 according to the present embodiment preferably has a P2O5 content of 0% to 30% and a TiO2 content of 0% to 30% expressed in terms of mol% based on oxides. This allows the glass 10 to have a high refractive index while suppressing a decrease in the transmittance of visible light.

[0119] The glass 10 according to the present embodiment preferably contains, in terms of mol% based on oxides, P2O5: 0% to 30%, TeO2: 0.1% or more and less than 40%, B2O3: 0% to 40%, Li2O: 0% to 15%, Na2O: 0% to 15%, K2O: 0% to 15%, TiO2: 0% to 30%, Ta2O5: 0% to 20%, WO3: 0% to 15%, Nb2O5: 0% to 15%, ZrO2: 0% to 20%, Bi2O3: greater than 15% and less than 45%, ZnO: 0% to 20%, SrO: 0% to 20%, La2O3: 0% to 30%, and SiO2: 0% to 30%. Thus, the glass 10 can have a high refractive index while suppressing a decrease in the transmittance of visible light.

[0120] The glass 10 according to the present embodiment preferably has a total content of Fe, Cr, and Ni of less than 4 ppm by mass. This allows the glass 10 to have a high refractive index while suppressing a decrease in the transmittance of visible light.

[0121] The glass 10 according to the present embodiment preferably has a thickness of 0.01 mm to 2.0 mm and a surface area of ​​8 cm 2 According to the present embodiment, the glass 10 having such a shape can have a high refractive index while suppressing a decrease in the transmittance of visible light.

[0122] The glass 10 involved in this embodiment is preferably used as a light guide plate. The glass 10 has a high refractive index and can improve resistance to ultraviolet rays, so it is suitable for use as a light guide plate. In particular, the light guide plate is sometimes irradiated with ultraviolet rays during the manufacturing process, so it is particularly preferable to use the glass 10 that can improve resistance to ultraviolet rays.

[0123] (Example)

[0124] Next, examples will be described. It should be noted that the embodiments may be modified as long as the effects of the invention are achieved.

[0125] In the examples, glasses having different compositions were prepared and evaluated. A more detailed description is given below.

[0126] Table 1-1 and Table 1-2 are tables showing the glass of each example. Table 1-1 and Table 1-2 show the contents of the materials used in the glass production of Examples 1 to 32 when expressed in mole % based on oxides. In addition, the total content of the 9 components refers to the total content of P2O5, TeO2, B2O3, TiO2, Ta2O5, WO3, ZrO2, Bi2O3 and ZnO when expressed in mole % based on oxides. In addition, parameters A and B refer to the values ​​described in the above embodiment. It should be noted that Examples 1 to 31 are examples, and Example 32 is a comparative example.

[0127] [Table 1-1]

[0128]

[0129] [Table 1-2]

[0130]

[0131] In the examples, a glass having a thickness of 1 mm was manufactured with the composition described in each example shown in Table 1-1. And, the glass manufactured in this way was evaluated as a sample. Specifically, the raw materials of the composition shown in Table 1-1 were uniformly mixed and melted in a gold crucible at 950°C for 2 hours to make a uniform molten glass. Next, the molten glass was poured into a carbon mold having a length × width × height = 60 mm × width 50 mm × height 30 mm. Then, after being kept at 430°C for 1 hour, it was cooled to room temperature at a temperature drop rate of about 1°C / min to obtain a glass block. Next, a cutting machine (a small cutting machine manufactured by Maruto Co., Ltd.) was used to cut the glass block into a length × width = 30 mm × 30 mm, and a grinding machine (SGM-6301 manufactured by Hidewa Kogyo Co., Ltd.) and a single-side grinder (EJ-380IN manufactured by Engis Co., Ltd.) were used to adjust the plate thickness and grind the surface to manufacture a glass plate having a length × width = 30 mm × 30 mm and a plate thickness of 1 mm.

[0132] (physical properties)

[0133] For each glass, the refractive index n for visible light was measured. d , internal transmittance at a wavelength of 440nm and the degree of degradation ΔT in the ultraviolet irradiation test.

[0134] Refractive index n d In the measurement, the refractive index n of each glass under the helium d line (wavelength 587.6nm) was measured. d . Refractive index n d The KPR-2000 manufactured by Kalnew was used for the measurement.

[0135] The internal transmittance at a wavelength of 440 nm was measured by using the method described in the above embodiment.

[0136] In measuring the degree of degradation ΔT, the degree of degradation ΔT is calculated by the method described in the above embodiment.

[0137] The measurement results of each example are shown in Table 1-2.

[0138] As shown in Table 1-2, the refractive index n d The glasses of Examples 1 to 31 (Examples) having a refractive index of 1.94 or more, a degradation degree ΔT of 2.2% or less, and an internal transmittance of 80% or more for light of a wavelength of 440 nm are high refractive index and can suppress the reduction of the transmittance of visible light. On the other hand, the glass of Example 32 (Comparative Example) which does not satisfy the condition of a degradation degree ΔT of 2.2% or less cannot suppress the reduction of the transmittance of visible light.

[0139] In addition, Young's modulus and wavelength λ showing 70% internal transmittance when the plate thickness (thickness) is 10 mm were measured. 70 In the measurement of Young's modulus, each glass was measured using 38DL PLUS manufactured by OLYMPUS Corporation based on the propagation of ultrasonic waves. Wavelength λ 70 The Young's modulus and wavelength λ are measured using the method described in the above embodiment. 70 The measurement results are also shown in Table 1-2.

[0140] Above, the embodiments of the present invention have been described, but the embodiments are not limited by the contents of the embodiments. In addition, the above-mentioned constituent elements include constituent elements that are easily assumed by those skilled in the art, substantially the same constituent elements, and constituent elements of so-called equal scope. Furthermore, the above-mentioned constituent elements can be appropriately combined. In addition, various omissions, substitutions or changes of constituent elements can be performed within the scope of the gist of the above-mentioned embodiments.

[0141] Explanation of symbols

[0142] 10. Glass

Claims

1. A glass having a refractive index of 1.94 or more, an internal transmittance of 70% or more for light of a wavelength of 440 nm when the plate thickness is 10 mm, and a degree of degradation ΔT of 2.2% or less in an ultraviolet irradiation test, in, The degree of degradation ΔT in the ultraviolet irradiation test is calculated by the following formula (1): ΔT(%)={(T0-T1) / T0}·100···(1) The transmittance T1 is the value of the UV irradiance of 50 mW / cm2 on the surface of the glass with a thickness of 1 mm. 2 The external transmittance of the glass at a wavelength of 470 nm after irradiation with ultraviolet light at a wavelength of 365 nm for 10 minutes, The transmittance T0 is the external transmittance of the glass at a wavelength of 470 nm before the ultraviolet irradiation.

2. The glass according to claim 1, wherein: The content of Nb2O5 is greater than or equal to 0% and less than 15% expressed as mol% based on oxide.

3. The glass according to claim 1, wherein: Expressed as mole % based on oxides, the content of P2O5 is 0% to 30%, and the content of TiO2 is 0% to 30%.

4. The glass according to claim 1, wherein: The parameter A defined by the formula (A) is 270 or less, expressed as mol% based on the oxide. A=c(P2O5) 2 +c(Nb2O5) 2 -c(TiO2) 2 ···(A) here, c(P2O5) is the content of P2O5 expressed as mol% based on oxide, unit is %, c(Nb2O5) is the content of Nb2O5 expressed as mol% based on oxide, unit is %, c(TiO2) is the TiO2 content when expressed as mol% based on oxide, and the unit is %.

5. The glass according to claim 4, wherein: The parameter B defined by the formula (B) is 2.5 or less, expressed as mol% based on the oxide. B=0.13455·2.7183 (0 .014912·A)···(B)。 6. The glass according to claim 1, wherein: Contains boric acid or phosphoric acid.

7. The glass according to any one of claims 1 to 6, wherein Expressed as molar % based on oxides, it contains P2O5: 0% to 30%, TeO2: 0.1% to less than 40%, B2O3: 0% to 40%, Li2O: 0% to 15%, Na2O: 0% to 15%, K2O: 0% to 15%, TiO2: 0% to 32%, Ta2O5: 0% to 20%, WO3: 0% to 15%, Nb2O5: 0% to 15%, ZrO2: 0% to 20%, Bi2O3: greater than 15% to 45%, ZnO: 0% to 20%, SrO: 0% to 20%, La2O3: 0% to 30%, SiO2: 0% to 30%.

8. The glass according to any one of claims 1 to 7, wherein The total content of Fe, Cr and Ni is less than 4 ppm by mass.

9. The glass according to any one of claims 1 to 8, wherein The thickness is 0.01mm~2.0mm, and the surface area is 8cm 2 above. 10 . The glass according to claim 1 , which is used as a light guide plate.