Ion-conductive solid and all-solid-state battery

Through the low-temperature heating treatment of the oxide solid represented by the general formula Li6+a-c-2dY1-a-b-c-dM1aM2bM3cM4dB3O9, the problem of the oxide-based solid electrolyte reacting at high temperatures is solved, and the ion conductivity and output performance of the all-solid-state battery are improved.

CN118765269APending Publication Date: 2024-10-11CANON OPTRON INC
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202380023959.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-14
Filing Date
2023-02-14
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

The high-temperature heating treatment of existing oxide-based solid electrolytes may cause the solid electrolyte to react with the electrode active material, forming a high-resistance phase, which reduces the ion conductivity and output performance of the all-solid-state battery.

Method used

The oxide represented by the general formula Li6+a-c-2dY1-a-b-c-dM1aM2bM3cM4dB3O9 is used as an ion conductive solid. Through low-temperature heating treatment, the Li+ state and charge balance in the crystal lattice are adjusted, the ion conductivity is improved, and the ion conductivity is improved through primary or secondary burning. The oxide solid is prepared in this step.

Benefits of technology

A high-ion conductivity solid prepared by low-temperature heating treatment is realized, which suppresses the reaction between the solid electrolyte and the electrode active material and improves the ion conductivity and output performance of the all-solid-state battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005012761070000211
    Figure BDA0005012761070000211
  • Figure BDA0005012761070000221
    Figure BDA0005012761070000221
Patent Text Reader

Abstract

An ion conductive solid containing an oxide represented by the general formula: Li < 6 + a-c-2d > Y < 1-a-b-c-d > M < 1 > a > M < 2 > b > M < 3 > c > M < 4 > d > B < 3 > O < 9 >. In the formula, M1 is at least one metal element selected from the group consisting of Mg, Mn, Zn, Ni, Ca, Sr, and Ba, M2 is at least one metal element selected from the group consisting of La, Pr, Nd, Sm, Eu, Gd, Tb, Dy, Ho, Er, Tm, Yb, Lu, In, and Fe, M3 is at least one metal element selected from the group consisting of Hf, Sn, and Ti, M4 is at least one metal element selected from the group consisting of Nb and Ta, and a, b, c, and d are each in specific ranges and are real numbers satisfying 0.010 < = a + b + c + d < 1.000.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to an ion conductive solid and an all-solid-state battery. Background Art

[0002] Lightweight and high-capacity lithium-ion secondary batteries have long been used in mobile devices such as smartphones and laptops, as well as in transportation equipment such as electric vehicles and hybrid electric vehicles.

[0003] However, since existing lithium-ion secondary batteries use liquids containing flammable solvents as electrolytes, there are concerns about leakage of flammable solvents and fires caused by battery short circuits. Therefore, in recent years, in order to ensure safety, secondary batteries using ion-conductive solids as electrolytes that are different from liquid electrolytes have attracted much attention. Such secondary batteries are called all-solid-state batteries.

[0004] Solid electrolytes such as oxide-based solid electrolytes and sulfide-based solid electrolytes are widely known as electrolytes used in all-solid-state batteries. Among them, oxide-based solid electrolytes do not react with moisture in the atmosphere to produce hydrogen sulfide, and are safer than sulfide-based solid electrolytes.

[0005] In addition, the all-solid-state battery has: a positive electrode containing a positive electrode active material, a negative electrode containing a negative electrode active material, an electrolyte containing an ion-conductive solid disposed between the positive electrode and the negative electrode, and a current collector as required (the positive electrode active material and the negative electrode active material are also collectively referred to as "electrode active material"). In the case of using an oxide-based solid electrolyte to make an all-solid-state battery, a heat treatment is performed to reduce the contact resistance between the particles of the oxide-based material contained in the solid electrolyte. However, the existing oxide-based solid electrolyte requires a high temperature of more than 900°C for heating treatment, so it is possible that the solid electrolyte reacts with the electrode active material to form a high resistance phase. This high resistance phase may be related to a decrease in the ion conductivity of the ion-conductive solid, which in turn leads to a decrease in the output of the all-solid-state battery.

[0006] Examples of oxide-based solid electrolytes that can be produced by heat treatment at a temperature lower than 900° C. include Li 2+x C 1-x B x O3 (Non-Patent Document 1).

[0007] In addition, it is also disclosed that relative to the above-mentioned Li 2+x C 1-x B x O3 can improve its properties by containing specific elements at a specific ratio (Patent Document 1).

[0008] Prior art literature

[0009] Non-patent literature

[0010] Non-patent document 1: Solid State Ionic 288 (2016) 248-252

[0011] Patent Literature

[0012] Patent Document 1: Japanese Patent No. 6948676 Summary of the invention

[0013] Problems to be solved by the invention

[0014] The present disclosure provides an ion conductive solid having high ion conductivity that can be produced by a heat treatment at a low temperature, and an all-solid-state battery having the ion conductive solid.

[0015] Technical solutions to solve problems

[0016] The ion-conducting solid disclosed herein is characterized in that it is a solid having a general formula Li 6+a-c-2d Y 1-a-b-c- d M1 a M2 b M3 c M4 d An ion-conductive solid of an oxide represented by B3O9.

[0017] (wherein, M1 is at least one metal element selected from the group consisting of Mg, Mn, Zn, Ni, Ca, Sr and Ba,

[0018] M2 is at least one metal element selected from the group consisting of La, Pr, Nd, Sm, Eu, Gd, Tb, Dy, Ho, Er, Tm, Yb, Lu, In and Fe,

[0019] M3 is at least one metal element selected from the group consisting of Hf, Sn and Ti, M4 is at least one metal element selected from the group consisting of Nb and Ta,

[0020] a is a real number satisfying 0.000≤a≤0.800, b is a real number satisfying 0.010≤b≤0.900, c is a real number satisfying 0.000≤c≤0.800, d is a real number satisfying 0.000≤d≤0.800, and a, b, c, d are real numbers satisfying 0.010≤a+b+c+d<1.000. )

[0021] In addition, the all-solid-state battery disclosed in the present invention is characterized in that it is an all-solid-state battery having at least a positive electrode, a negative electrode and an electrolyte, wherein:

[0022] At least one selected from the group consisting of the positive electrode, the negative electrode, and the electrolyte contains the ion-conductive solid of the present disclosure.

[0023] Effects of the Invention

[0024] According to one aspect of the present disclosure, it is possible to obtain an ion conductive solid having high ion conductivity that can be produced by a heat treatment at a low temperature, and an all-solid-state battery having the ion conductive solid. DETAILED DESCRIPTION

[0025] In the present disclosure, unless otherwise specified, the description of "XX or more and YY or less" and "XX to YY" indicating a numerical range means a numerical range including the lower limit and the upper limit as endpoints. When the numerical range is described in stages, the upper and lower limits of each numerical range can be arbitrarily combined.

[0026] Furthermore, in the present disclosure, “solid” refers to a substance having a certain shape and volume among the three states of matter, and a powder state is included in the “solid”.

[0027] The ion-conducting solid disclosed herein is a solid having a general formula Li 6+a-c-2d Y 1-a-b-c-d M1 a M2 b M3 c M4 d An ion-conductive solid of an oxide represented by B3O9.

[0028] In the formula, M1 is at least one metal element selected from the group consisting of Mg, Mn, Zn, Ni, Ca, Sr and Ba,

[0029] M2 is at least one metal element selected from the group consisting of La, Pr, Nd, Sm, Eu, Gd, Tb, Dy, Ho, Er, Tm, Yb, Lu, In and Fe,

[0030] M3 is at least one metal element selected from the group consisting of Hf, Sn and Ti, M4 is at least one metal element selected from the group consisting of Nb and Ta,

[0031] a is a real number satisfying 0.000≤a≤0.800, b is a real number satisfying 0.010≤b≤0.900, c is a real number satisfying 0.000≤c≤0.800, d is a real number satisfying 0.000≤d≤0.800, and a, b, c, d are real numbers satisfying 0.010≤a+b+c+d<1.000.

[0032] The ion-conductive solid of the present disclosure preferably has a monoclinic crystal structure.

[0033] The volume average particle size of the ion conductive solid disclosed herein is preferably 0.1 μm to 28.0 μm, more preferably 0.3 μm to 26.0 μm, and even more preferably 1.0 μm to 20.0 μm. Within the above range, the grain boundary resistance in the ion conductive solid is reduced, so that the ion conductivity is further improved.

[0034] The volume average particle size of the ion conductive solid can be controlled by pulverization or classification.

[0035] In the above general formula, a is a real number satisfying 0.000≤a≤0.800.

[0036] a is 0.000≤a≤0.800, preferably 0.000≤a≤0.600, more preferably 0.000≤a≤0.400, further preferably 0.000≤a≤0.100, particularly preferably 0.000≤a≤0.050, and very preferably 0.000≤a≤0.030.

[0037] In the above general formula, b is a real number satisfying 0.010≤b≤0.900.

[0038] b is 0.010≤b≤0.900, preferably 0.020≤b≤0.900, more preferably 0.050≤b≤0.900, further preferably 0.100≤b≤0.900, particularly preferably 0.200≤b≤0.900, and very preferably 0.300≤b≤0.900.

[0039] In the above general formula, c is a real number satisfying 0.000≤c≤0.800.

[0040] c is 0.000≤c≤0.800, preferably 0.000≤c≤0.600, more preferably 0.000≤c≤0.400, further preferably 0.000≤c≤0.100, particularly preferably 0.000≤c≤0.050, and very preferably 0.000≤c≤0.030.

[0041] In the above general formula, d is a real number satisfying 0.000≤d≤0.800.

[0042] d is 0.000≤d≤0.800, preferably 0.000≤d≤0.600, more preferably 0.000≤d≤0.400, further preferably 0.000≤d≤0.100, particularly preferably 0.000≤d≤0.050, and very preferably 0.000≤d≤0.030.

[0043] In the above formula, a+b+c+d is a real number satisfying 0.010≤a+b+c+d<1.000.

[0044] a+b+c+d is 0.010≤a+b+c+d<1.000, preferably 0.050≤a+b+c+d<1.000, more preferably 0.100≤a+b+c+d<1.000, further preferably 0.200≤a+b+c+d≤1.000, especially preferably 0.300≤a+b+c+d<1.000, and very preferably 0.500≤a+b+c+d<1.000.

[0045] Y 1-a-b-c-d 1-abcd in is preferably 0.300≤1-abcd, more preferably 0.500≤1-abcd, further preferably 0.700≤1-abcd, and further preferably 0.750≤1-abcd. The upper limit is not particularly limited, but is preferably less than 1.000, 0.950 or less, or 0.900 or less.

[0046] The ion conductive solid of the present disclosure can adopt the following embodiments, for example, but is not limited to these embodiments. (1)

[0048] a satisfies 0.010≤a≤0.100, b satisfies 0.010≤b≤0.200, c satisfies 0.000≤c≤0.200, d satisfies 0.010≤d≤0.100, and a, b, c, d satisfy 0.010≤a+b+c+d<0.300. (2)

[0050] a satisfies 0.010≤a≤0.030, b satisfies 0.030≤b≤0.100, c satisfies 0.010≤c≤0.030, d satisfies 0.010≤d≤0.030, and a, b, c, d satisfy 0.050≤a+b+c+d<0.160.

[0051] Regarding M1, M3, and M4 in the above general formula, they may be included in the formula or not. That is, at least one of a, c, and d may be 0.

[0052] In the above general formula, M1 is at least one metal element selected from the group consisting of Mg, Mn, Zn, Ni, Ca, Sr and Ba.

[0053] M1 is at least one selected from the group consisting of Mg, Mn, Zn, Ni, Ca, Sr and Ba, preferably at least one selected from the group consisting of Mg, Zn, Ca, Sr and Ba, and more preferably at least one selected from the group consisting of Mg, Ca and Sr.

[0054] In the above general formula, M2 is at least one metal element selected from the group consisting of La, Pr, Nd, Sm, Eu, Gd, Tb, Dy, Ho, Er, Tm, Yb, Lu, In and Fe.

[0055] M2 is at least one selected from the group consisting of La, Pr, Nd, Sm, Eu, Gd, Tb, Dy, Ho, Er, Tm, Yb, Lu, In and Fe, preferably at least one selected from the group consisting of La, Eu, Gd, Tb, Dy, Yb, Lu, In and Fe, and more preferably at least one selected from the group consisting of Gd, Dy, Yb, Lu, In and Fe.

[0056] In the above general formula, M3 is at least one metal element selected from the group consisting of Hf, Sn and Ti.

[0057] M3 is at least one selected from the group consisting of Hf, Sn, and Ti, preferably at least one selected from the group consisting of Hf and Sn, and more preferably Hf.

[0058] In the above general formula, M4 is at least one metal element selected from the group consisting of Nb and Ta.

[0059] M4 is at least one selected from the group consisting of Nb and Ta, and is preferably Nb.

[0060] The present inventors presume as follows the reason why the ion conductivity of the ion conductive solid containing the oxide represented by the above general formula is improved.

[0061] When a part of Y, which is a trivalent metal element, is replaced by specific elements M1, M2, M3, and M4 within a specific ratio range, the lattice constant and charge balance in the crystal lattice are adjusted. + is in excess or deficiency, so that the Li + It is easy to move within the crystal lattice, so the ion conductivity is improved.

[0062] When a part of Y is replaced by M1, Li + As a result, the mobile Li + Therefore, the ionic conductivity increases.

[0063] When a part of Y is substituted with M2, the lattice becomes smaller by substituting an element with a different ionic radius. + The distance between each other is shortened, promoting Li + The movement of ions improves the ion conductivity.

[0064] When a part of Y is replaced by M3 or M4, Li + In a defective state. As a result, if we want to fill the Li + The defect, the surrounding Li + The ion conductivity will increase.

[0065] Next, the method for producing the ion conductive solid of the present disclosure will be described.

[0066] The method for producing the ion conductive solid of the present disclosure may be as follows, but is not limited thereto.

[0067] A compound having the general formula Li 6+a-c-2d Y 1-a-b-c-d M1 a M2 b M3 c M4 d A method for producing an ion-conductive solid of an oxide represented by B3O9,

[0068] There may be a primary calcination step of heating the mixed raw materials at a temperature lower than the melting point of the oxide to obtain the oxide represented by the general formula.

[0069] In the formula, M1 is at least one metal element selected from the group consisting of Mg, Mn, Zn, Ni, Ca, Sr and Ba, M2 is at least one metal element selected from the group consisting of La, Pr, Nd, Sm, Eu, Gd, Tb, Dy, Ho, Er, Tm, Yb, Lu, In and Fe, M3 is at least one metal element selected from the group consisting of Hf, Sn and Ti, M4 is at least one metal element selected from the group consisting of Nb and Ta, a is a real number satisfying 0.000≤a≤0.800, b is a real number satisfying 0.010≤b≤0.900, c is a real number satisfying 0.000≤c≤0.800, d is a real number satisfying 0.000≤d≤0.800, and a, b, c, d are real numbers satisfying 0.010≤a+b+c+d<1.000.

[0070] The method for producing an ion conductive solid disclosed herein may include a primary firing process, wherein the raw materials are weighed and mixed, and the raw materials are subjected to a heat treatment at a temperature lower than the melting point of the oxide to produce an ion conductive solid containing the oxide to obtain an oxide represented by the above general formula. The ion conductive solid can be obtained by the primary firing process.

[0071] Furthermore, if necessary, the production method may further include a secondary calcination step of heating the ion conductive solid containing the obtained oxide at a temperature lower than the melting point of the oxide to produce a sintered body of the ion conductive solid containing the oxide.

[0072] The method for producing the ion conductive solid of the present disclosure including the primary calcination step and the secondary calcination step will be described in detail below, but the present disclosure is not limited to the following production method.

[0073] One-shot firing process

[0074] In the primary calcination process, raw materials such as Li3BO3, H3BO3, Yb2O3, ZrO2, CeO2, HfO2, etc. of chemical reagent grade are weighed and mixed according to stoichiometric quantities to form a general formula Li 6+a-c-2d Y 1-a-b-c-d M1 a M2 b M3 c M4 d B3O9 (wherein, M1 is any one or more metal elements selected from Mg, Mn, Zn, Ni, Ca, Sr or Ba, M2 is any one or more metal elements selected from La, Pr, Nd, Sm, Eu, Gd, Tb, Dy, Ho, Er, Tm, Yb, Lu, In or Fe, M3 is any one or more metal elements selected from Hf, Sn or Ti, M4 is any one or more metal elements selected from Nb or Ta, a is a real number satisfying 0.000≤a≤0.800, b is a real number satisfying 0.010≤b≤0.900, c is a real number satisfying 0.000≤c≤0.800, d is a real number satisfying 0.000≤d≤0.800, and a, b, c, d are real numbers satisfying 0.010≤a+b+c+d<1.000).

[0075] The device for mixing is not particularly limited, but for example, a pulverizing mixer such as a planetary ball mill can be used. The material and capacity of the container used during mixing, as well as the material and diameter of the ball are not particularly limited, and can be appropriately selected according to the type and usage of the raw materials used. As an example, a 45mL container made of zirconium oxide and a 5mm diameter ball made of zirconium oxide can be used. In addition, the conditions of the mixed treatment are not particularly limited, but for example, a rotation speed of 50rpm to 2000rpm and a time of 10 minutes to 60 minutes.

[0076] After the mixed powder of the above raw materials is obtained by the mixing process, the obtained mixed powder is subjected to pressure molding to form particles. As the pressure molding method, a known pressure molding method such as cold uniaxial molding method and cold hydrostatic molding method can be used. The pressure molding conditions in the primary sintering process are not particularly limited, and for example, the pressure can be 100MPa to 200MPa.

[0077] The obtained particles are calcined using a calcination device such as an atmospheric calcination device. The temperature for the first calcination and solid phase synthesis is as long as it is lower than the temperature of the general formula Li 6+a-c-2d Y 1-a-b-c-d M1 a M2 b M3 c M4 d The melting point of the ion conductive solid represented by B3O9 is not particularly limited. The temperature during the primary calcination can be, for example, less than 700°C, less than 680°C, less than 670°C, less than 660°C or less than 650°C, for example, more than 500°C. This numerical range can be combined arbitrarily. As long as the temperature is within the above range, solid phase synthesis can be fully carried out. The time of the primary calcination process is not particularly limited, but for example, it can be about 700 minutes to 750 minutes.

[0078] Through the above-mentioned one-time calcination process, a product containing the above-mentioned general formula Li 6+a-c-2d Y 1-a-b-c- d M1 a M2 b M3 c M4 d An ion conductive solid containing an oxide represented by B3O9 can also be obtained as a powder by pulverizing the ion conductive solid containing the oxide using a mortar and a mill or a planetary mill.

[0079] Secondary firing process

[0080] In the secondary calcination step, at least one selected from the group consisting of the ion conductive solid containing oxide obtained in the primary calcination step and powder of the ion conductive solid containing oxide is pressure-molded and calcined as necessary to obtain a sintered body of the ion conductive solid containing oxide.

[0081] Pressure forming and secondary sintering can be performed simultaneously using spark plasma sintering (hereinafter also referred to as "SPS"), hot pressing, etc., or after the particles are manufactured by cold unidirectional forming, secondary sintering can be performed in an air atmosphere, an oxidizing atmosphere, or a reducing atmosphere. As long as the above conditions are met, melting due to the heat treatment will not occur, and an ion conductive solid with high ion conductivity can be obtained. There are no special restrictions on the conditions for pressure forming in the secondary sintering process, and for example, the pressure can be 10MPa to 100MPa.

[0082] The temperature of the secondary sintering is lower than that of the general formula Li 6+a-c-2d Y 1-a-b-c-d M1 a M2 b M3 c M4 d The melting point of the ion conductive solid represented by B3O9. The temperature during the secondary calcination is preferably below 700°C, more preferably below 680°C, further preferably below 670°C, and particularly preferably below 660°C. The lower limit of the temperature is not particularly limited, and the lower the better, but for example, it is above 500°C. This numerical range can be combined arbitrarily, but for example, a range of above 500°C and below 700°C can be adopted. As long as it is within the above range, the melting or decomposition of the ion conductive solid containing the oxide disclosed in the secondary calcination process can be suppressed, and a fully sintered sintered body of the ion conductive solid containing the oxide disclosed in the present invention can be obtained.

[0083] The time of the secondary firing step can be appropriately changed according to the temperature and pressure of the secondary firing, but is preferably 24 hours or less, and may be 14 hours or less. The time of the secondary firing step may be, for example, 5 minutes or more, 1 hour or more, or 6 hours or more.

[0084] The method for cooling the sintered body of the ion conductive solid containing the oxide of the present disclosure obtained by the secondary calcination step is not particularly limited, and the body may be cooled naturally (cooled in a furnace), rapidly cooled, cooled more gradually than naturally, or maintained at a certain temperature during cooling.

[0085] Next, the all-solid-state battery of the present disclosure will be described.

[0086] An all-solid-state battery generally includes a positive electrode, a negative electrode, an electrolyte containing an ion-conductive solid and disposed between the positive electrode and the negative electrode, and a current collector as needed.

[0087] The all-solid-state battery disclosed herein is an all-solid-state battery having at least a positive electrode, a negative electrode and an electrolyte, wherein:

[0088] At least one selected from the group consisting of the positive electrode, the negative electrode, and the electrolyte contains the ion-conductive solid of the present disclosure.

[0089] The all-solid-state battery disclosed herein may be a bulk battery or a thin-film battery. The specific shape of the all-solid-state battery disclosed herein is not particularly limited, and examples thereof include a coin shape, a button shape, a sheet shape, and a laminate shape.

[0090] The all-solid-state battery disclosed herein has an electrolyte. In the all-solid-state battery disclosed herein, it is preferred that at least the electrolyte contains the ion-conductive solid disclosed herein.

[0091] The solid electrolyte in the all-solid-state battery disclosed in the present invention may be composed of the ion conductive solid disclosed in the present invention, may contain other ion conductive solids, and may contain ionic liquids and gel polymers. Other ion conductive solids are not particularly limited, and may contain ion conductive solids commonly used in all-solid-state batteries, such as LiI, Li3PO4, Li7La3Zr2O 12 The content of the ion conductive solid of the present disclosure in the electrolyte of the all-solid-state battery of the present disclosure is not particularly limited, but is preferably 25% by mass or more, more preferably 50% by mass or more, further preferably 75% by mass or more, and particularly preferably 100% by mass.

[0092] The all-solid-state battery disclosed in the present invention has a positive electrode. The positive electrode may contain a positive electrode active material, or may contain the positive electrode active material and the ion conductive solid disclosed in the present invention. As the positive electrode active material, a known positive electrode active material such as a sulfide containing a transition metal element, an oxide containing lithium and a transition metal element, etc. may be used without particular limitation. For example, LiNiVO4, LiCoPO4, LiCoVO4, LiMn 1.6 Ni 0.4 O4, LiMn2O4, LiCoO2, Fe2(SO4)3, LiFePO4, LiNi 1 / 3 Mn 1 / 3 Co 1 / 3 O2、LiNi 1 / 2 Mn 1 / 2 O2, LiNiO2, Li 1+x (Fe, Mn, Co) 1-x O2、LiNi 0.8 Co 0.15 Al 0.05 O2, etc.

[0093] Furthermore, the positive electrode may further contain a binder, a conductive agent, etc. Examples of the binder include polyvinylidene fluoride (PVDF), polytetrafluoroethylene, polyvinyl alcohol, etc. Examples of the conductive agent include natural graphite, artificial graphite, acetylene black, ethylene black, etc.

[0094] The all-solid-state battery disclosed in the present invention has a negative electrode. The negative electrode may contain a negative electrode active material, or may contain the negative electrode active material and the ion conductive solid disclosed in the present invention. As the negative electrode active material, inorganic compounds such as lithium, lithium alloys, and tin compounds, carbonaceous materials that can absorb and release lithium ions, and conductive polymers may be used without particular limitation. For example, Li4Ti5O 12 wait.

[0095] Furthermore, the negative electrode may further contain a binder, a conductive agent, etc. As the binder and the conductive agent, the same materials as those listed for the positive electrode can be used.

[0096] Here, the electrode "containing" an electrode active material means that the electrode has the electrode active material as a component, element, or property. For example, whether the electrode active material is contained in the electrode or the electrode active material is coated on the surface of the electrode, it is equivalent to the above-mentioned "containing".

[0097] The positive electrode and the negative electrode can be obtained by known methods such as mixing raw materials, molding, and heat treatment. It is believed that the ion conductive solid enters the gaps between the electrode active materials, making it easier to ensure the conduction path of lithium ions. Compared with the prior art, the ion conductive solid disclosed in the present invention can be produced by low-temperature heat treatment, so it is believed that the formation of a high resistance phase generated by the reaction of the ion conductive solid with the electrode active material can be suppressed.

[0098] The positive electrode and the negative electrode may also have a current collector. As the current collector, a known current collector such as aluminum, titanium, stainless steel, nickel, iron, calcined carbon, conductive polymer, conductive glass, etc. may be used. In addition, in order to improve adhesion, conductivity, oxidation resistance, etc., a material whose surface is treated with carbon, nickel, titanium, silver, etc., may be used as a current collector.

[0099] The all-solid-state battery disclosed in the present invention can be obtained, for example, by laminating, molding, and heating the positive electrode, the solid electrolyte, and the negative electrode. Compared with the prior art, the ion-conductive solid disclosed in the present invention can be produced by low-temperature heating, so it is believed that the formation of a high-resistance phase generated by the reaction of the ion-conductive solid with the electrode active material can be suppressed, and an all-solid-state battery with excellent output characteristics can be obtained.

[0100] Next, the composition and the measurement methods of various physical properties involved in the present disclosure are described.

[0101] ·Methods for identification and analysis of metal-containing

[0102] The composition analysis of the ion conductive solid is performed by wavelength dispersive X-ray fluorescence analysis (hereinafter also referred to as XRF) using a sample solidified by a pressure molding method. However, in the case where analysis is difficult due to particle size effects, the ion conductive solid can be vitrified by the glass bead method and the composition analysis can be performed by XRF. In addition, in the case of XRF, when the yttrium peak overlaps with the metal-containing peak, the composition analysis can be performed by inductively coupled plasma atomic emission spectrometry (ICP-AES).

[0103] In the case of XRF, the analysis device used was ZSX Primus II manufactured by Rigaku Corporation. The analysis conditions were: Rh was used as the anode of the X-ray tube, in a vacuum atmosphere, the analysis diameter was 10 mm, the analysis range was 17 degrees to 81 degrees, the step length was 0.01 degrees, and the scanning speed was 5 seconds / step. In addition, a proportional counter was used for light element measurement, and a scintillation counter was used for heavy element measurement.

[0104] The elements were identified based on the peak positions of the spectrum obtained by XRF, and the molar concentration ratio was calculated from the number of X-ray photons per unit time, that is, the count rate (unit: cps), to determine a, b, c, and d.

[0105] Example

[0106] Hereinafter, examples of specifically preparing and evaluating the ion conductive solid of the present disclosure will be described as examples. In addition, the present disclosure is not limited to the following examples.

[0107] [Example 1]

[0108] ·One-shot firing process

[0109] Li3BO3 (produced by Toyoshima Seisakusho, purity 99.9 mass%), H3BO3 (produced by Kanto Chemical, purity 99.5%), Y2O3 (produced by Shin-Etsu Chemical, purity 99.9 mass%), and Yb2O3 (produced by Shin-Etsu Chemical, purity 99.9 mass%) were used as raw materials, and each raw material was weighed in a stoichiometric manner so that b became the value described in Table 1, and mixed for 30 minutes at a disk speed of 300 rpm using a planetary mill P-7 manufactured by Fritsch. The planetary mill used was made of zirconium oxide. Ball and 45mL container.

[0110] After mixing, the mixed powder was cold uniaxially molded at 147 MPa using a 100 kN electric press P3052-10 manufactured by Npasystem, and sintered in an air atmosphere at a heating temperature of 650° C. and a holding time of 720 minutes.

[0111] The obtained oxide-containing ion conductive solid was pulverized by a planetary mill P-7 manufactured by Fritsch Co., Ltd. at a disc rotation speed of 230 rpm for 180 minutes to prepare a powder of the oxide-containing ion conductive solid.

[0112] Secondary firing process

[0113] The powder of the ion conductive solid containing oxide obtained above was molded and subjected to secondary sintering to produce a sintered body of the ion conductive solid containing oxide of Example 1. The powder was cold unidirectionally molded at 147 MPa using a 100 kN electric press P3052-10 manufactured by Npasystem. The secondary sintering was performed in an air atmosphere at a heating temperature of 650° C. and a holding time of 720 minutes.

[0114] [Example 2]

[0115] Li3BO3 (produced by Toyoshima Seisakusho, purity 99.9 mass%), H3BO3 (produced by Kanto Chemical, purity 99.5%), Y2O3 (produced by Shin-Etsu Chemical, purity 99.9 mass%), Yb2O3 (produced by Shin-Etsu Chemical, purity 99.9 mass%) and HfO2 (produced by New Metals, purity 99.9%) were used as raw materials, and each raw material was weighed according to chemical quantification so that b and c became the values ​​shown in Table 1. Except for this, a sintered body of an ion conductive solid containing the oxide of Example 2 was produced by the same process as Example 1.

[0116] [Example 3]

[0117] Li3BO3 (manufactured by Toyoshima Seisakusho, purity 99.9 mass%), H3BO3 (manufactured by Kanto Chemical, purity 99.5%), Y2O3 (manufactured by Shin-Etsu Chemical, purity 99.9 mass%), Yb2O3 (manufactured by Shin-Etsu Chemical, purity 99.9 mass%), SnO2 (manufactured by Mitsuwa Chemicals, purity 99.9%) and HfO2 (manufactured by New Metals, purity 99.9%) were used as raw materials, and each raw material was weighed according to chemical quantification so that b and c became the values ​​shown in Table 1. Except for this, a sintered body of an ion conductive solid containing the oxide of Example 3 was produced by the same process as Example 1.

[0118] [Example 4]

[0119] Li3BO3 (produced by Toyoshima Seisakusho, purity 99.9 mass%), H3BO3 (produced by Kanto Chemical, purity 99.5%), Y2O3 (produced by Shin-Etsu Chemical, purity 99.9 mass%), In2O3 (produced by Shinko Chemical, purity 99 mass%), HfO2 (produced by New Metals, purity 99.9%) and Nb2O5 (produced by Mitsui Mining and Smelting, purity 99.9%) were used as raw materials, and each raw material was weighed according to chemical quantification in such a way that b, c and d became the values ​​shown in Table 1. Except for this, a sintered body of an ion conductive solid containing the oxide of Example 4 was produced by the same process as Example 1.

[0120] [Example 5]

[0121] A sintered body of an ion conductive solid containing the oxide of Example 5 was produced by the same steps as in Example 1 except that the raw materials used in the above Examples were weighed stoichiometrically so that b and c would have the values ​​shown in Table 1.

[0122] [Example 6]

[0123] Li3BO3 (produced by Toyoshima Seisakusho, purity 99.9 mass%), H3BO3 (produced by Kanto Chemical, purity 99.5%), Y2O3 (produced by Shin-Etsu Chemical, purity 99.9 mass%), In2O3 (produced by Shinko Chemical, purity 99 mass%) and CaO (produced by Kanto Chemical, purity 99.0 mass%) were used as raw materials, and each raw material was weighed according to chemical quantification so that a and b became the values ​​shown in Table 1. Except for this, a sintered body of an ion conductive solid containing the oxide of Example 6 was produced by the same process as Example 1.

[0124] [Example 7]

[0125] Li3BO3 (produced by Toyoshima Seisakusho, purity 99.9 mass%), H3BO3 (produced by Kanto Chemical, purity 99.5%), Y2O3 (produced by Shin-Etsu Chemical, purity 99.9 mass%), Fe2O3 (produced by Wako Pure Chemical Industries, Ltd., purity 95.0 mass%) and TiO2 (produced by Toho Titanium, purity 99%) were used as raw materials, and each raw material was weighed according to chemical quantification in such a way that b and c became the values ​​shown in Table 1. Except for this, a sintered body of an ion conductive solid containing the oxide of Example 7 was produced by the same process as Example 1.

[0126] [Example 8]

[0127] A sintered body of an ion conductive solid containing the oxide of Example 8 was produced by the same steps as in Example 1 except that the raw materials used in the above Examples were weighed stoichiometrically so that b and c had the values ​​shown in Table 1.

[0128] [Example 9]

[0129] Li3BO3 (manufactured by Toyoshima Seisakusho, purity 99.9 mass%), H3BO3 (manufactured by Kanto Chemical, purity 99.5%), Y2O3 (manufactured by Shin-Etsu Chemical, purity 99.9 mass%), Lu2O3 (manufactured by Kojun Chemical Laboratory, purity 99.9 mass%), MgO (manufactured by Ube Materials, purity 99.0 mass%) and CaO (manufactured by Kanto Chemical, purity 97.0 mass%) were used as raw materials, and each raw material was weighed according to chemical quantification so that a and b became the values ​​shown in Table 1. Except for this, a sintered body of an ion conductive solid containing the oxide of Example 9 was produced by the same process as Example 1.

[0130] [Example 10]

[0131] A sintered body of an ion conductive solid containing the oxide of Example 10 was produced by the same steps as in Example 1, except that the raw materials used in the above Examples were weighed stoichiometrically so that a, b, and c had the values ​​shown in Table 1.

[0132] [Example 11]

[0133] A sintered body of an ion conductive solid containing the oxide of Example 11 was produced by the same steps as in Example 1, except that the raw materials used in the above Examples were weighed stoichiometrically so that a, b, and d had the values ​​shown in Table 1.

[0134] [Example 12]

[0135] Li3BO3 (manufactured by Toyoshima Seisakusho, purity 99.9 mass%), H3BO3 (manufactured by Kanto Chemical, purity 99.5%), Y2O3 (manufactured by Shin-Etsu Chemical, purity 99.9 mass%), La2O3 (manufactured by Wako Pure Chemical Industries, Ltd., purity 99.9 mass%), MgO (manufactured by Ube Materials, purity 99.0 mass%) and CaO (manufactured by Kanto Chemical, purity 97.0 mass%) were used as raw materials, and each raw material was weighed according to chemical quantification so that a and b became the values ​​shown in Table 1. Except for this, a sintered body of an ion conductive solid containing the oxide of Example 12 was prepared by the same process as Example 1.

[0136] [Example 13]

[0137] Li3BO3 (manufactured by Toyoshima Seisakusho, purity 99.9 mass%), H3BO3 (manufactured by Kanto Chemical, purity 99.5%), Y2O3 (manufactured by Shin-Etsu Chemical, purity 99.9 mass%), La2O3 (manufactured by Wako Pure Chemical Industries, Ltd., purity 99.9 mass%) and MnO (manufactured by Kanto Chemical, purity 80.0 mass%) were used as raw materials, and the raw materials used in the above examples were weighed according to stoichiometric amounts so that a and b became the values ​​shown in Table 1. Except for this, a sintered body of an ion conductive solid containing the oxide of Example 13 was prepared by the same process as Example 1.

[0138] [Example 14]

[0139] Li3BO3 (produced by Toyoshima Seisakusho, purity 99.9 mass%), H3BO3 (produced by Kanto Chemical, purity 99.5%), Y2O3 (produced by Shin-Etsu Chemical, purity 99.9 mass%), Tb2O3 (produced by Shin-Etsu Chemical, purity 99.9 mass%) and MnO (produced by Kanto Chemical, purity 80.0 mass%) were used as raw materials, and each raw material was weighed according to stoichiometry in such a way that a and b became the values ​​shown in Table 1. Except for this, a sintered body of an ion conductive solid containing the oxide of Example 14 was produced by the same process as Example 1.

[0140] [Example 15]

[0141] Li3BO3 (manufactured by Toyoshima Seisakusho, purity 99.9 mass%), H3BO3 (manufactured by Kanto Chemical, purity 99.5%), Y2O3 (manufactured by Shin-Etsu Chemical, purity 99.9 mass%), Tm2O3 (manufactured by Kojun Chemical Laboratory, purity 99.9 mass%) and CaO (manufactured by Kanto Chemical, purity 97.0 mass%) were used as raw materials, and each raw material was weighed according to stoichiometry in such a way that a and b became the values ​​shown in Table 1. Except for this, a sintered body of an ion conductive solid containing the oxide of Example 15 was produced by the same process as Example 1.

[0142] [Example 16]

[0143] Li3BO3 (manufactured by Toyoshima Seisakusho, purity 99.9 mass%), H3BO3 (manufactured by Kanto Chemical, purity 99.5%), Y2O3 (manufactured by Shin-Etsu Chemical, purity 99.9 mass%), Tm2O3 (manufactured by Kojun Chemical Research Institute, purity 99.9 mass%), SnO2 (manufactured by Mitsuwa Chemicals, purity 99.9%) and Ta2O5 (manufactured by Kanto Chemical, purity 99 mass%) were used as raw materials, and each raw material was weighed according to chemical quantification in such a way that b, c and d became the values ​​shown in Table 1. Except for this, a sintered body of an ion conductive solid containing the oxide of Example 16 was produced by the same process as Example 1.

[0144] [Example 17]

[0145] Li3BO3 (manufactured by Toyoshima Seisakusho, purity 99.9 mass%), H3BO3 (manufactured by Kanto Chemical, purity 99.5%), Y2O3 (manufactured by Shin-Etsu Chemical, purity 99.9 mass%), In2O3 (manufactured by Shinko Chemical, purity 99 mass%), Nb2O5 (manufactured by Mitsui Mining and Smelting, purity 99.9%) and Ta2O5 (manufactured by Kanto Chemical, purity 99 mass%) were used as raw materials, and each raw material was weighed according to chemical quantification in such a way that b and d became the values ​​shown in Table 1. Except for this, a sintered body of an ion conductive solid containing the oxide of Example 17 was prepared by the same process as Example 1.

[0146] [Example 18]

[0147] Li3BO3 (manufactured by Toyoshima Seisakusho, purity 99.9 mass%), H3BO3 (manufactured by Kanto Chemical, purity 99.5%), Y2O3 (manufactured by Shin-Etsu Chemical, purity 99.9 mass%), Pr2O3 (manufactured by Shin-Etsu Chemical, purity 99.9 mass%) and ZnO (manufactured by Wako Pure Chemical Industries, Ltd., purity 99 mass%) were used as raw materials, and each raw material was weighed according to chemical quantification so that a and b became the values ​​shown in Table 1. Except for this, a sintered body of an ion conductive solid containing the oxide of Example 18 was prepared by the same process as Example 1.

[0148] [Example 19]

[0149] A sintered body of an ion conductive solid containing the oxide of Example 19 was produced by the same steps as in Example 1, except that the raw materials used in the above Examples were weighed stoichiometrically so that b and d would have the values ​​shown in Table 1.

[0150] [Example 20]

[0151] Li3BO3 (manufactured by Toyoshima Seisakusho, purity 99.9 mass%), H3BO3 (manufactured by Kanto Chemical, purity 99.5%), Y2O3 (manufactured by Shin-Etsu Chemical, purity 99.9 mass%), Sm2O3 (manufactured by Wako Pure Chemical Industries, Ltd., purity 99.9 mass%), HfO2 (manufactured by New Metals, purity 99.9%) and Ta2O5 (manufactured by Kanto Chemical, purity 99 mass%) were used as raw materials, and each raw material was weighed according to chemical quantification in such a way that b, c and d became the values ​​shown in Table 1. Except for this, a sintered body of an ion conductive solid containing the oxide of Example 20 was produced by the same process as Example 1.

[0152] [Example 21]

[0153] Li3BO3 (manufactured by Toyoshima Seisakusho, Ltd., purity 99.9 mass%), H3BO3 (manufactured by Kanto Chemical, purity 99.5%), Y2O3 (manufactured by Shin-Etsu Chemical, purity 99.9 mass%), Nd2O3 (manufactured by Shin-Etsu Chemical, purity 99.9 mass%), Sm2O3 (manufactured by Wako Pure Chemical Industries, Ltd., purity 99.9 mass%) and ZnO (manufactured by Wako Pure Chemical Industries, Ltd., purity 99 mass%) were used as raw materials, and each raw material was weighed according to chemical quantification so that a and b became the values ​​shown in Table 1. Except for this, a sintered body of an ion conductive solid containing the oxide of Example 21 was produced by the same process as Example 1.

[0154] [Example 22]

[0155] Li3BO3 (manufactured by Toyoshima Seisakusho, purity 99.9 mass%), H3BO3 (manufactured by Kanto Chemical, purity 99.5%), Y2O3 (manufactured by Shin-Etsu Chemical, purity 99.9 mass%), Nd2O3 (manufactured by Shin-Etsu Chemical, purity 99.9 mass%) and NiO (manufactured by Wako Pure Chemical Industries, Ltd., purity 99.0 mass%) were used as raw materials, and each raw material was weighed according to chemical quantification so that a and b became the values ​​shown in Table 2. Except for this, a sintered body of an ion conductive solid containing the oxide of Example 22 was prepared by the same process as Example 1.

[0156] [Example 23]

[0157] Li3BO3 (manufactured by Toyoshima Seisakusho, purity 99.9 mass%), H3BO3 (manufactured by Kanto Chemical, purity 99.5%), Y2O3 (manufactured by Shin-Etsu Chemical, purity 99.9 mass%), Eu2O3 (manufactured by Shin-Etsu Chemical, purity 95 mass%), SnO2 (manufactured by Mitsuwa Chemicals, purity 99.9%) and Ta2O5 (manufactured by Kanto Chemical, purity 99 mass%) were used as raw materials, and each raw material was weighed according to chemical quantification in such a way that b, c and d became the values ​​shown in Table 2. Except for this, a sintered body of an ion conductive solid containing the oxide of Example 23 was produced by the same process as Example 1.

[0158] [Example 24]

[0159] A sintered body of an ion conductive solid containing the oxide of Example 24 was produced by the same steps as in Example 1, except that the raw materials used in the above Examples were weighed stoichiometrically so that a and b had the values ​​shown in Table 2.

[0160] [Example 25]

[0161] A sintered body of an ion conductive solid containing the oxide of Example 25 was produced by the same steps as in Example 1, except that the raw materials used in the above Examples were weighed stoichiometrically so that b and c had the values ​​shown in Table 2.

[0162] [Example 26]

[0163] Li3BO3 (manufactured by Toyoshima Seisakusho, purity 99.9 mass%), H3BO3 (manufactured by Kanto Chemical, purity 99.5%), Y2O3 (manufactured by Shin-Etsu Chemical, purity 99.9 mass%), Gd2O3 (manufactured by Shin-Etsu Chemical, purity 99.9 mass%), Dy2O3 (manufactured by Shin-Etsu Chemical, purity 95 mass%) and CaO (manufactured by Kanto Chemical, purity 99.0 mass%) were used as raw materials, and each raw material was weighed according to chemical quantification so that a and b had the values ​​shown in Table 2. Except for this, a sintered body of an ion conductive solid containing the oxide of Example 26 was produced by the same process as Example 1.

[0164] [Example 27]

[0165] A sintered body of an ion conductive solid containing the oxide of Example 27 was produced by the same steps as in Example 1, except that the raw materials used in the above Examples were weighed stoichiometrically so that a, b and c had the values ​​shown in Table 2.

[0166] [Example 28]

[0167] A sintered body of an ion conductive solid containing the oxide of Example 28 was produced by the same steps as in Example 1, except that the raw materials used in the above Examples were weighed stoichiometrically so that b and c had the values ​​shown in Table 2.

[0168] [Example 29]

[0169] A sintered body of an ion conductive solid containing the oxide of Example 29 was produced by the same steps as in Example 1, except that the raw materials used in the above Examples were weighed stoichiometrically so that b and d would have the values ​​shown in Table 2.

[0170] [Example 30]

[0171] Li3BO3 (manufactured by Toyoshima Seisakusho, purity 99.9 mass%), H3BO3 (manufactured by Kanto Chemical, purity 99.5%), Y2O3 (manufactured by Shin-Etsu Chemical, purity 99.9 mass%), Tb2O3 (manufactured by Shin-Etsu Chemical, purity 99.9 mass%), NiO (manufactured by Wako Pure Chemical Industries, Ltd., purity 99.0 mass%) and BaO (manufactured by Wako Pure Chemical Industries, Ltd., purity 90.0 mass%) were used as raw materials, and each raw material was weighed according to chemical quantification so that a and b became the values ​​shown in Table 2. Except for this, a sintered body of an ion conductive solid containing the oxide of Example 30 was produced by the same process as Example 1.

[0172] [Example 31]

[0173] Li3BO3 (manufactured by Toyoshima Seisakusho, purity 99.9 mass%), H3BO3 (manufactured by Kanto Chemical, purity 99.5%), Y2O3 (manufactured by Shin-Etsu Chemical, purity 99.9 mass%), Tb2O3 (manufactured by Shin-Etsu Chemical, purity 99.9 mass%), Ho2O3 (manufactured by Kojun Chemical Laboratories, purity 99.9 mass%) and BaO (manufactured by Wako Pure Chemical Industries, Ltd., purity 90.0 mass%) were used as raw materials, and each raw material was weighed according to stoichiometric amounts so that a and b became the values ​​shown in Table 2. Except for this, a sintered body of an ion conductive solid containing the oxide of Example 31 was prepared by the same process as Example 1.

[0174] [Example 32]

[0175] The raw materials used in the above examples were weighed according to chemical quantification so that a and b became the values ​​shown in Table 2, and the disk rotation speed during crushing was set to 300 rpm. Except for this, a sintered body of an ion conductive solid containing the oxide of Example 32 was produced by the same process as Example 1.

[0176] [Example 33]

[0177] A sintered body of an ion conductive solid containing the oxide of Example 33 was produced by the same steps as in Example 1, except that the raw materials used in the above examples were weighed stoichiometrically so that b, c and d had the values ​​shown in Table 2.

[0178] [Example 34]

[0179] Li3BO3 (manufactured by Toyoshima Seisakusho, purity 99.9 mass%), H3BO3 (manufactured by Kanto Chemical, purity 99.5%), Y2O3 (manufactured by Shin-Etsu Chemical, purity 99.9 mass%), Er2O3 (manufactured by Shin-Etsu Chemical, purity 95 mass%), Tm2O3 (manufactured by Kojun Chemical Laboratory, purity 99.9 mass%) and SrO (manufactured by Kojun Chemical Laboratory, purity 98 mass%) were used as raw materials, and each raw material was weighed according to chemical quantification so that a and b became the values ​​shown in Table 2. Except for this, a sintered body of an ion conductive solid containing the oxide of Example 34 was produced by the same process as Example 1.

[0180] [Example 35]

[0181] A sintered body of an ion conductive solid containing the oxide of Example 35 was produced by the same steps as in Example 1, except that the raw materials used in the above examples were weighed stoichiometrically so that b and c had the values ​​shown in Table 2.

[0182] [Example 36]

[0183] A sintered body of an ion conductive solid containing the oxide of Example 36 was produced by the same steps as in Example 1, except that the raw materials used in the above examples were weighed stoichiometrically so that a, b and c had the values ​​shown in Table 2.

[0184] [Example 37]

[0185] A sintered body of an ion conductive solid containing the oxide of Example 37 was produced by the same steps as in Example 1, except that the raw materials used in the above examples were weighed stoichiometrically so that b and d had the values ​​shown in Table 2.

[0186] [Example 38]

[0187] A sintered body of an ion conductive solid containing the oxide of Example 38 was produced by the same steps as in Example 1, except that the raw materials used in the above examples were weighed stoichiometrically so that b and d had the values ​​shown in Table 2.

[0188] [Example 39]

[0189] A sintered body of an ion conductive solid containing the oxide of Example 39 was produced by the same steps as in Example 1, except that the raw materials used in the above Examples were weighed stoichiometrically so that a and b had the values ​​shown in Table 2.

[0190] [Example 40]

[0191] A sintered body of an ion conductive solid containing the oxide of Example 40 was produced by the same steps as in Example 1, except that the raw materials used in the above examples were weighed stoichiometrically so that b and d had the values ​​shown in Table 2.

[0192] [Example 41]

[0193] A sintered body of an ion conductive solid containing the oxide of Example 41 was produced by the same steps as in Example 1, except that the raw materials used in the above Examples were weighed stoichiometrically so that b and d would have the values ​​shown in Table 2.

[0194] [Comparative Example 1]

[0195] A sintered body of an ion-conductive solid containing an oxide was prepared by the same process as in Example 1 except that Li3BO3 (manufactured by Toyoshima Seisakusho, purity 99.9 mass %), H3BO3 (manufactured by Kanto Chemical, purity 99.5%) and Y2O3 (manufactured by Shin-Etsu Chemical, purity 99.9 mass %) were used as raw materials.

[0196] The composition analysis was performed by the above method on the sintered bodies of the ion conductive solids containing the oxides of Examples 1 to 41. The volume average particle size of the powders of the ion conductive solids obtained in Examples 1 to 41 and Comparative Example 1 and the ion conductivity of the sintered bodies of the ion conductive solids were measured by the following method.

[0197] The methods for measuring the ion conductivity and the volume average particle size are described below. In addition, the obtained evaluation results are shown in Tables 1 and 2.

[0198] Determination of ionic conductivity

[0199] In the flat plate-shaped sintered body of the ion conductive solid containing oxide obtained by secondary sintering, two parallel and large surfaces are ground with sandpaper. The size of the flat plate-shaped sintered body of the ion conductive solid containing oxide can be, for example, 0.9 cm × 0.9 cm × 0.05 cm, but is not limited to this. Grinding starts with grinding with #500 for 15 minutes to 30 minutes, then grinding with #1000 for 10 minutes to 20 minutes, and finally grinding with #2000 for 5 minutes to 10 minutes. If there are no obvious bumps or scratches on the ground surface by visual observation, it is completed.

[0200] After grinding, a gold film was formed on the ground surface of the sintered body of the oxide-containing ion conductive solid using a sputtering device SC-701MkII ADVANCE manufactured by Sanyu-electron Co., Ltd. The film forming conditions were that the process gas was Ar, the vacuum was 2Pa to 5Pa, and the film forming time was 5 minutes. After the film was formed, the AC impedance of the sample was measured.

[0201] Impedance measurement was performed using an impedance / gain phase analyzer SI1260 and a dielectric interface system 1296 (both manufactured by Solartron Corporation). Measurement conditions were a temperature of 27° C., an amplitude of 20 mV, and a frequency of 0.1 Hz to 1 MHz.

[0202] The resistance of the sintered body of the ion conductive solid containing oxide was calculated using the Nyquist plot obtained by impedance measurement and the AC analysis software ZVIEW manufactured by Scribner. The resistance of the sintered body of the ion conductive solid containing oxide was calculated by setting an equivalent circuit equivalent to the measured sample in ZVIEW, fitting and analyzing the equivalent circuit and the Nyquist plot. The ion conductivity was calculated by the following formula using the calculated resistance and the thickness and electrode area of ​​the sintered body of the ion conductive solid containing oxide.

[0203] Ion conductivity (S / cm) = thickness of sintered body of ion conductive solid containing oxide (cm) / (resistance of sintered body of ion conductive solid containing oxide (Ω) × electrode area (cm) 2 ))

[0204] The ion conductivity (S / cm) of the sintered body of the ion conductive solid is preferably 1.00×10 -9 More preferably, 1.00×10 -8 More preferably, 1.00×10 -7 More preferably, 1.00×10 -6 More than 1.00×10 -5 The higher the conductivity, the better. The upper limit is not particularly limited, for example, 1.00×10 -2 Below, 1.00×10 -3 Below, 1.00×10 -4 the following.

[0205] ·Evaluation of volume average particle size

[0206] The particle size distribution of the powder of the ion-conductive solid containing oxide obtained by ball milling (P-7 planetary mill made by Fritsch) after primary sintering was measured using the laser diffraction / scattering particle size distribution measuring device LA-960V2 manufactured by Horiba. The refractive index was 1.8, and ethanol was used as the measuring solvent. The concentration of the sample was adjusted in such a way that the transmittance was 90 to 70%. The volume average particle size was calculated based on the obtained frequency distribution.

[0207] ·result

[0208] Tables 1 and 2 show the chemical compositions of the raw materials used to produce the sintered bodies of the ion conductive solids containing the oxides of Examples 1 to 41 and Comparative Example 1 (general formula Li 6+a-c-2d Y 1-a-b-c-d M1 a M2 b M3 c M4 d The values ​​of a, b, c and d in B3O9), volume average particle size and ion conductivity.

[0209] The results of the above composition analysis confirmed that the sintered bodies of the ion conductive solids containing the oxides of Examples 1 to 41 and Comparative Example 1 all had the stoichiometric compositions of the raw materials described in Tables 1 and 2. In addition, the sintered bodies of the ion conductive solids containing the oxides of Examples 1 to 41 were ion conductive solids that exhibited high ion conductivity even when sintered at a temperature lower than 700°C.

[0210] [Table 1]

[0211] Table 1

[0212]

[0213] [Table 2]

[0214] Table 2

[0215]

[0216] In Table 2, the ion conductivity of the ion conductive solid prepared in Example 31 is improved compared with that in Example 32. Since the compositions and substitution elements disclosed in the prior art are different, the density after firing is affected by the difference in melting points, and therefore the suitable range of particle size may be different.

Claims

1. An ion-conductive solid, characterized in that Containing the general formula Li 6+a-c-2d Y 1-a-b-c-d M1 a M2 b M3 c M4 d Oxide represented by B3O9, In the formula, M1 is at least one metal element selected from the group consisting of Mg, Mn, Zn, Ni, Ca, Sr and Ba, M2 is at least one metal element selected from the group consisting of La, Pr, Nd, Sm, Eu, Gd, Tb, Dy, Ho, Er, Tm, Yb, Lu, In and Fe, M3 is at least one metal element selected from the group consisting of Hf, Sn and Ti, M4 is at least one metal element selected from the group consisting of Nb and Ta, a is a real number satisfying 0.000≤a≤0.800, b is a real number satisfying 0.010≤b≤0.900, c is a real number satisfying 0.000≤c≤0.800, d is a real number satisfying 0.000≤d≤0.800, and a, b, c, d are real numbers satisfying 0.010≤a+b+c+d<1.

000.

2. The ion-conductive solid according to claim 1, characterized in that The 1-abcd is 0.300≤1-abcd.

3. The ion-conductive solid according to claim 1 or 2, characterized in that The 1-abcd is 0.500≤1-abcd.

4. The ion-conductive solid according to any one of claims 1 to 3, characterized in that The a is 0.000≤a≤0.

400.

5. The ion-conductive solid according to any one of claims 1 to 4, characterized in that The b is 0.300≤b≤0.

900.

6. The ion-conductive solid according to any one of claims 1 to 5, characterized in that The c is 0.000≤c≤0.

400.

7. The ion-conductive solid according to any one of claims 1 to 6, characterized in that The d is 0.000≤d≤0.

400.

8. The ion-conductive solid according to any one of claims 1 to 7, characterized in that The volume average particle size is 0.1 μm or more and 28.0 μm or less.

9. An all-solid-state battery, comprising at least a positive electrode, a negative electrode and an electrolyte, characterized in that: At least one selected from the group consisting of the positive electrode, the negative electrode, and the electrolyte contains the ion-conductive solid according to any one of claims 1 to 8.

10. The all-solid-state battery according to claim 9, characterized in that: At least the electrolyte contains the ion-conductive solid.

Citation Information

Patent Citations

  • Method for preparing single-crystal cubic sesquioxides and uses thereof

    CN102791910A

  • Lithium ion conductor and lithium ion battery using the same

    JP2017091953A

  • Ion conductive solid and all-solid-state battery

    WO2021124812A1