Composition
By specifically combining and processing the composition of tetrafluoroethylene-based polymer and boron nitride particles, the problem of insufficient dispersion of the composition during melt mixing was solved, and high thermal conductivity, excellent bending resistance and adhesiveness were achieved. , suitable for formed products of sheets or films.
Patent Information
- Application Number
- CN202380023699.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-02-28
- Filing Date
- 2023-02-22
- Publication Date
- 2024-10-11
AI Technical Summary
The composition of a tetrafluoroethylene polymer and boron nitride particles has a high melt viscosity when melted and mixed, making it difficult to improve the dispersibility of the boron nitride particles, resulting in insufficient electrical properties, thermal conductivity, and adhesiveness of the molded product.
A composition of tetrafluoroethylene-based polymer particles within a specific range, spherical boron nitride particles with an average particle diameter of 5 μm or more and 40 μm or less, and non-spherical boron nitride particles with an average particle diameter of less than 15 μm is used, and subjected to a shearing process Mixing with the stirring mechanism ensures excellent dispersion of non-spherical boron nitride particles.
Forming molded products and laminates with low linear expansion coefficient, dielectric constant and dielectric loss tangent and excellent thermal conductivity, bending resistance and adhesion. In particular, the bending resistance and bending resistance of sheets or films are also improved. Significant improvement.
Abstract
Description
Technical Field
[0001] The present invention relates to a specific composition comprising tetrafluoroethylene polymer particles, spherical boron nitride particles, and non-spherical boron nitride particles. Background Art
[0002] In recent years, in order to cope with the higher speed and higher frequency of mobile communication devices such as mobile phones, the materials of the printed circuit boards of communication devices need to have high thermal conductivity, low linear expansion coefficient, low dielectric constant and low dielectric loss tangent. Tetrafluoroethylene-based polymers with low dielectric constant and low dielectric loss tangent have attracted much attention. In order to obtain materials with better physical properties, compositions of tetrafluoroethylene polymers and other components are being studied. Patent Document 1 proposes a powder composition of tetrafluoroethylene polymer particles and two types of boron nitride particles having different particle sizes. Prior art literature Patent Literature
[0003] Patent Document 1: Japanese Patent Application Publication No. 2016-098301 Summary of the invention Technical problem to be solved by the invention
[0004] Tetrafluoroethylene polymers have low surface tension and low affinity with other components. Therefore, in a molded product formed from a composition whose other component is inorganic particles such as boron nitride particles, the physical properties of each component may not be fully exhibited. The present inventors have found that the composition of the above-mentioned Patent Document 1 has a high melt viscosity during melt mixing and is difficult to improve the dispersibility of the boron nitride particles. Therefore, it is difficult to obtain a composition that can form a shaped product such as a sheet having excellent electrical properties and thermal conductivity, bending resistance and adhesion to a substrate (peel strength). The present inventors have discovered that a composition comprising particles of a tetrafluoroethylene polymer and spherical and non-spherical boron nitride particles having a specific average particle size within a specific range has excellent dispersibility even if the average particle size is small, and that the linear expansion coefficient, dielectric constant and dielectric loss tangent of the molded product thereof are low and that the thermal conductivity, bending resistance and adhesion are excellent. In particular, even if the molded product is a thin sheet or film, the bending resistance, bending resistance and other bending properties are excellent, thereby completing the present invention. An object of the present invention is to provide such a composition and a method for producing the same, a method for producing a sheet and a laminate obtained from the composition, and such a laminate. Solutions to technical problems
[0005] The present invention has the following aspects. [1] A composition comprising particles of a tetrafluoroethylene polymer, spherical boron nitride particles having an average particle size of 5 μm or more and 40 μm or less, and non-spherical boron nitride particles having an average particle size of less than 15 μm, wherein the mass ratio of the non-spherical boron nitride particles to the total mass of the spherical boron nitride particles and the non-spherical boron nitride particles is less than 30%. [2] The composition according to [1], wherein the tetrafluoroethylene polymer is a hot-melt tetrafluoroethylene polymer. [3] The composition according to [1] or [2], wherein the tetrafluoroethylene polymer is a tetrafluoroethylene polymer having an oxygen-containing polar group. [4] The composition as described in any one of [1] to [3], wherein the average particle size of the tetrafluoroethylene polymer particles is smaller than either the average particle size of the spherical boron nitride particles or the average particle size of the non-spherical boron nitride particles. [5] The composition according to any one of [1] to [4], wherein the average particle size of the non-spherical boron nitride particles is smaller than the average particle size of the spherical boron nitride particles. [6] The composition according to any one of [1] to [5], wherein the ratio of the average particle size of the spherical boron nitride to the average particle size of the non-spherical boron nitride particles is 2.5 or more. [7] The composition as described in any one of [1] to [6], wherein the mass ratio of the tetrafluoroethylene polymer particles to the total mass of the tetrafluoroethylene polymer particles, the spherical boron nitride particles, and the non-spherical boron nitride particles is 20% or more and 80% or less. [8] The composition according to any one of [1] to [7], wherein the total content of the tetrafluoroethylene polymer particles, the spherical boron nitride particles, and the non-spherical boron nitride particles in the composition is 50% or more. [9] The composition according to any one of [1] to [8], further comprising a liquid dispersion medium.
[10] A method for producing a composition as described in [9], wherein particles of a tetrafluoroethylene polymer, spherical boron nitride particles having an average particle size of 5 μm or more and 40 μm or less, non-spherical boron nitride particles having an average particle size of less than 15 μm, and a liquid dispersion medium are subjected to a shear treatment.
[11] The method for producing a composition according to
[10] , wherein the shearing treatment is performed by mixing in a tank equipped with a stirring mechanism that is performed by swirling of a thin film or a stirring mechanism that is performed by rotation and revolution.
[12] A method for producing a sheet, comprising extruding the composition according to any one of [1] to [9] to obtain a sheet comprising the tetrafluoroethylene polymer, the spherical boron nitride particles, and the non-spherical boron nitride particles.
[13] A method for producing a laminate, wherein the composition described in any one of [1] to [9] is applied to the surface of a substrate and heated to form a polymer layer comprising the tetrafluoroethylene polymer and the spherical boron nitride particles and the non-spherical boron nitride particles, thereby obtaining a laminate having a substrate layer composed of the substrate and the polymer layer.
[14] A laminate comprising a substrate layer and a polymer layer formed from the composition according to any one of [1] to [9] and comprising the tetrafluoroethylene polymer, the spherical boron nitride particles, and the non-spherical boron nitride particles.
[15] The laminate according to
[14] , wherein the thickness of the polymer layer is 20 μm or more and 100 μm or less. Effects of the Invention
[0006] According to the present invention, provide the composition of the excellent dispersibility of the particle that comprises tetrafluoroethylene polymer with specific range and spherical and non-spherical boron nitride particles with specific average grain diameter.Can form formed article and laminated body that linear expansion coefficient, dielectric constant and dielectric loss tangent are low and thermal conductivity, bending resistance and adhesiveness are excellent by said composition.Even if the formed article obtained by this composition is particularly thin formed article such as sheet or film, its bending resistance, bending resistance and bending properties are also excellent. DETAILED DESCRIPTION
[0007] The following terms have the following meanings. The “average particle size (D50)” is the volume-based cumulative 50% diameter of the particles obtained by the laser diffraction scattering method. That is, the particle size distribution is measured by the laser diffraction scattering method, and the cumulative curve is obtained with the total volume of the particle group as 100%, and the particle size at the point where the cumulative volume reaches 50% on the cumulative curve. The D50 of the particles is determined by dispersing the particles in water and analyzing them by a laser diffraction / scattering method using a laser diffraction / scattering particle size distribution analyzer (LA-920 analyzer manufactured by Horiba, Ltd.). The "melting temperature" is the temperature corresponding to the maximum of the melting peak of a polymer as measured by differential scanning calorimetry (DSC). The “glass transition temperature (Tg)” is a value measured by analyzing a polymer using a dynamic viscoelasticity measurement (DMA) method. The "viscosity" was determined by measuring the composition using a B-type viscometer at 25° C. and a rotation speed of 30 rpm. The measurement was repeated 3 times, and the average of the 3 measured values was taken. The "thixotropic ratio" is a value calculated by dividing the viscosity η1 of the composition measured at a rotation speed of 30 rpm by the viscosity η2 measured at a rotation speed of 60 rpm. Each viscosity measurement was repeated 3 times, and the average of the 3 measured values was taken. The "unit" in a polymer refers to an atomic group based on a monomer formed by polymerization of the monomer. The unit may be a unit formed directly by a polymerization reaction, or a unit in which a part of the unit is converted into another structure by treating the polymer. Hereinafter, the unit based on monomer a is also referred to as "monomer a unit".
[0008] The composition of the present invention (hereinafter also referred to as "the present composition") comprises particles (hereinafter also referred to as "F particles") of a tetrafluoroethylene polymer (hereinafter also referred to as "F polymer"), spherical boron nitride particles having an average particle size of 5 μm or more and 40 μm or less (hereinafter also referred to as "spherical BN particles"), and non-spherical boron nitride particles having an average particle size of less than 15 μm (hereinafter also referred to as "non-spherical BN particles"), wherein the mass ratio of the non-spherical boron nitride particles to the total mass of the spherical boron nitride particles and the non-spherical boron nitride particles is less than 30%.
[0009] The composition has excellent dispersibility, and can form a molded product having high physical properties of F polymer and boron nitride particles, low linear expansion coefficient, dielectric constant and dielectric loss tangent, and excellent thermal conductivity, bending resistance and adhesion. In particular, even if it is a thin molded product such as a sheet or film, it is easy to form a molded product with excellent bending resistance, bending resistance, etc. The reason is not necessarily clear, but it is considered as follows.
[0010] If spherical boron nitride particles with a small average particle size are mixed into a resin alone for the purpose of improving physical properties such as thermal conductivity, there is a tendency that the melt viscosity of the composition increases and the formability decreases, or the thermal conductivity decreases and it is difficult to fully present its physical properties in the molded product. In the case of mixing non-spherical boron nitride particles such as flat or flaky boron nitride particles alone, since they are oriented along the flow direction during melt molding, the thermal conductivity in the surface direction of the resulting molded product such as a sheet tends to be worse than the thermal conductivity in the length direction. In the case of using spherical boron nitride particles and non-spherical boron nitride particles and mixing them into a resin, these tendencies are expected to be improved, but on the other hand, the morphology and molding conditions of the composition are easily restricted.
[0011] The present composition contains two types of boron nitride particles, spherical BN particles and non-spherical BN particles, each of which has an average particle size within a specific range. As a result, in the interior of a molded product made from the present composition, the non-spherical BN particles are easily sandwiched between two or more spherical BN particles. In other words, the non-spherical BN particles cover the surface of the spherical BN particles and promote the formation of an inter-particle network, which improves the thermal conductivity in the surface direction when the composition is made into a sheet or a film.
[0012] In particular, the present composition contains non-spherical BN particles less than a prescribed ratio relative to the total amount of spherical BN particles and non-spherical BN particles. It is believed that the non-spherical BN particles contained in this excessively small ratio have excellent dispersibility and are not easy to agglomerate, which promotes the uniform dispersion of F particles and spherical BN particles. Furthermore, when the present composition is processed and formed, it is easy to form a dense and stable filling of spherical BN particles that are excessively contained as boron nitride particles, which is believed to promote the highly oriented configuration of non-spherical BN particles in the formed product. In other words, this promotes the formation of a heat conduction path by non-spherical BN particles in the formed product, and helps to improve the bending resistance of the formed product. As a result, it is believed that the physical properties of the F polymer and the boron nitride particles are highly possessed, and specifically, the composition can provide a thin formed product, such as a sheet or film, having low linear expansion coefficient, dielectric constant and dielectric loss tangent and excellent thermal conductivity, bending resistance and adhesiveness. In addition, in this specification, "sheet" is used as a general term for both sheets and films.
[0013] The F polymer in the present invention is a polymer containing units (hereinafter also referred to as "TFE units") based on tetrafluoroethylene (hereinafter also referred to as "TFE"). The polymer F may be heat-fusible or non-heat-fusible. Here, a heat-fusible polymer refers to a polymer having a temperature at which a melt flow rate is 1 to 1000 g / 10 minutes under a load of 49 N. A non-heat-fusible polymer refers to a polymer having no temperature at which a melt flow rate is 1 to 1000 g / 10 minutes under a load of 49 N. The melting temperature of the heat-melting F polymer is preferably 180° C. or higher, more preferably 200° C. or higher, and further preferably 260° C. or higher. The melting temperature of the F polymer is preferably 325° C. or lower, more preferably 320° C. or lower. The melting temperature of the F polymer is preferably 180 to 320° C. Within this range, the processability of the present composition is likely to be excellent, and the heat resistance of the molded product formed from the present composition is likely to be excellent.
[0014] The glass transition temperature of the F polymer is preferably 50° C. or higher, more preferably 75° C. or higher. The glass transition temperature of the F polymer is preferably 150° C. or lower, more preferably 125° C. or lower. The fluorine content of the F polymer is preferably 70% by mass or more, more preferably 72 to 76% by mass. The F polymer with a high fluorine content has low affinity with inorganic particles mainly composed of boron nitride particles, but a composition (present composition) having excellent dispersibility can be obtained according to the present invention through the above-mentioned mechanism of action. The surface tension of the F polymer is preferably 16 to 26 mN / m. The surface tension of the F polymer can be measured by placing a drop of a mixed solution for a wetting tension test specified in JIS K6768 (manufactured by Wako Pure Chemical Industries, Ltd.) on a flat plate made of the F polymer.
[0015] As the F polymer, polytetrafluoroethylene (PTFE), a polymer containing TFE units and ethylene-based units, a polymer containing TFE units and propylene-based units, a polymer containing TFE units and perfluoro(alkyl vinyl ether) (PAVE)-based units (PAVE units) (PFA), a polymer containing TFE units and hexafluoropropylene-based units (FEP), more preferably PFA and FEP, and further preferably PFA. These polymers may also contain units based on other comonomers. As PAVE, CF2=CFOCF3, CF2=CFOCF2CF3 and CF2=CFOCF2CF2CF3 (hereinafter also referred to as PPVE) are preferred, and PPVE is more preferred.
[0016] The F polymer preferably has an oxygen-containing polar group. As the oxygen-containing polar group, a hydroxyl-containing group or a carbonyl-containing group is preferred, and a carbonyl-containing group is more preferred. In this case, the F particles easily interact with the spherical BN particles and the non-spherical BN particles, and the present composition is easy to have excellent dispersibility. In addition, the present composition can easily obtain a molded product having low linear expansion coefficient, dielectric constant and dielectric loss tangent and excellent thermal conductivity and adhesiveness. The hydroxyl-containing group is preferably an alcoholic hydroxyl-containing group, more preferably -CF2CH2OH and -C(CF3)2OH. As the carbonyl-containing group, preferred are a carboxyl group, an alkoxycarbonyl group, an amide group, an isocyanate group, a carbamate group (-OC(O)NH2), an acid anhydride residue (-C(O)OC(O)-), an imide residue (-C(O)NHC(O)-, etc.), a formyl group, a haloformyl group, a carbamate group (-NHC(O)O-), a carbamoyl group (-C(O)-NH2), a urea group (-NH-C(O)-NH2), an oxalyl group (-NH-C(O)-C(O)-NH2) and a carbonate group (-OC(O)O-), and an acid anhydride residue is more preferred. In the case where the F polymer has an oxygen-containing polar group, the number of oxygen-containing polar groups in the F polymer is preferably 1×10 6The number of main chain carbon atoms is 10 to 5000, and more preferably 100 to 3000. In addition, the number of oxygen-containing polar groups in the F polymer can be quantified based on the composition of the polymer or the method described in International Publication No. 2020 / 145133.
[0017] The oxygen-containing polar group may be contained in the monomer-based unit in the F polymer or in the terminal group of the F polymer main chain, and the former form is preferred. As the latter form, an F polymer having an oxygen-containing polar group as a terminal group derived from a polymerization initiator, a chain transfer agent, etc., and an F polymer obtained by subjecting the F polymer to plasma treatment or ionizing radiation treatment can be exemplified. The monomer having a carbonyl group is preferably itaconic anhydride, citraconic anhydride, and 5-norbornene-2,3-dicarboxylic anhydride (hereinafter also referred to as NAH), and more preferably NAH.
[0018] The F polymer is preferably a polymer having a carbonyl group containing a TFE unit and a PAVE unit, more preferably a polymer comprising a TFE unit, a PAVE unit, and a unit based on a monomer having a carbonyl group and containing 90 to 99 mol%, 0.99 to 9.97 mol%, and 0.01 to 3 mol% of these units in order relative to all units. As a specific example of such a F polymer, a polymer described in International Publication No. 2018 / 16644 can be cited.
[0019] The F particles in the present invention are particles of F polymers, preferably non-hollow particles. The D50 of the F particles is preferably above 0.01 μm, more preferably above 0.3 μm, and further preferably above 1 μm. The D50 of the F particles is preferably below 10 μm, more preferably below 8 μm. In this case, the dispersibility and processability of the present composition are excellent. Moreover, it is easy to obtain a molded product having low linear expansion coefficient, dielectric constant and dielectric loss tangent and excellent thermal conductivity and adhesion (adhesion to substrate) by the present composition. The specific surface area of the F particles is preferably 1 to 25 m 2 / g. From the viewpoint of dispersion stability of the present composition, the bulk density of the F particles is preferably 0.05 g / mL or more, more preferably 0.08 g / mL or more. The bulk density of the F particles is preferably 0.5 g / mL or less, more preferably 0.4 g / mL or less.
[0020] One or more F particles may be used. The F particles are preferably particles of at least a heat-melting F polymer, and more preferably particles of a heat-melting F polymer having an oxygen-containing polar group with a melting temperature of 180 to 320° C. In this case, the interaction between the F particles and the spherical BN particles and the non-spherical BN particles in the above-mentioned mechanism of action is enhanced, the aggregation of each particle is also easily suppressed, and the dispersibility of the present composition is easily improved.
[0021] When using two or more F particles, the F particles are preferably a mixture of particles of a heat-fusible F polymer and particles of a non-heat-fusible F polymer. In this case, the agglomeration inhibition of the particles of the heat-fusible F polymer and the retention effect produced by the fibrillation of the non-heat-fusible F polymer reach a balance, and the dispersibility of the present composition is easily improved. Moreover, in the molded product thus obtained, the electrical properties of the non-heat-fusible F polymer are highly exhibited, and it is particularly easy to obtain a molded product with a low dielectric loss tangent. As the particles of the hot-melt F polymer, particles of the hot-melt F polymer having a melting temperature of 180 to 320° C. are preferred, and particles of the hot-melt F polymer having an oxygen-containing polar group having a melting temperature of 180 to 320° C. are more preferred. The preferred form of the hot-melt F polymer having an oxygen-containing polar group in the hot-melt F polymer particles is the same as the preferred form of the F polymer having an oxygen-containing polar group described above. As the particles of the non-thermally fusible F polymer, particles of non-thermally fusible PTFE are preferred. The proportion of the heat-meltable F polymer particles in the total mass of the two or more F particles is preferably 50% by mass or less, more preferably 40% by mass or less. The above proportion is preferably 5% by mass or more, more preferably 10% by mass or more. In addition, it is preferred that the D50 of the heat-fusible F polymer particles is 1 to 4 μm and the D50 of the non-heat-fusible F polymer particles is 0.1 to 1 μm.
[0022] The F particles may further contain a resin or inorganic compound other than the F polymer, or may form a core-shell structure with the F polymer as the core and the resin or inorganic compound other than the F polymer as the shell, or may form a core-shell structure with the F polymer as the shell and the resin or inorganic compound other than the F polymer as the core. Here, as the resin other than the F polymer, there may be mentioned aromatic polyester, polyamideimide, polyimide, and maleimide, and as the inorganic compound, there may be mentioned silicon dioxide and boron nitride.
[0023] The spherical BN particles contained in the present composition are approximately spherical. Here, approximately spherical means that when the inorganic particles are observed by a scanning electron microscope (SEM), the proportion of particles with a short diameter to long diameter ratio of 0.7 or more is 95% or more. The aspect ratio of the spherical BN particles is preferably 1 to 5, more preferably 1 to 2. The spherical BN particles may be used alone or in combination. However, when the spherical BN particles are used in combination in combination in combination in combination in combination, the present composition is likely to be excellent in dispersibility and processability. Furthermore, the present composition is likely to provide a molded product having excellent thermal conductivity or electrical properties. Spherical BN particles can be produced by the method described in, for example, Japanese Patent Application Publication No. 2012-056818 or Japanese Patent No. 5305656. The average particle size (D50) of the spherical BN particles is 5 μm or more and 40 μm or less, preferably 10 μm or more, and more preferably 15 μm or more. The spherical BN particles may be spherical aggregate particles of primary particles of boron nitride. In this case, aggregates of primary particles of boron nitride in a flat plate shape such as a scale or a plate are preferred.
[0024] The non-spherical BN particles included in the present composition refer to all boron nitride particles not included in the above-mentioned spherical BN particles, and their shapes can be any of needle-like (fibrous), flaky, plate-like, etc., and are more preferably flaky. In this case, the dispersibility and processability of the present composition are easily excellent. Moreover, it is easy to obtain a molded product with excellent electrical properties from the present composition. The average particle size (D50) of the non-spherical BN particles is less than 15 μm, preferably 12 μm or less, and more preferably 10 μm or less. The D50 of the non-spherical BN particles is preferably 1 μm or more, and more preferably 3 μm or more. The aspect ratio of the non-spherical BN particles is preferably greater than 5, more preferably greater than 10. The aspect ratio of the non-spherical BN particles is preferably 10,000 or less. The non-spherical BN particles are preferably plate-shaped or flaky. Such non-spherical BN particles can be produced industrially, and examples thereof include "UHP" series (manufactured by Showa Denko K.K.), "GP" and "HGP" grades of the "Denka Boron Nitride" series (manufactured by Denka K.K.).
[0025] The present composition comprises F particles, spherical BN particles and non-spherical BN particles, wherein the mass ratio of the non-spherical BN particles to the total mass of the spherical BN particles and the non-spherical BN particles is less than 30%. The mass ratio of the non-spherical BN particles to the total mass of the spherical BN particles and the non-spherical BN particles is preferably 25% or less, more preferably 20% or less. The ratio is preferably 1% or more, more preferably 5% or more. In the present composition, it is preferred that the D50 of the F particles is smaller than either the D50 of the spherical BN particles or the D50 of the non-spherical BN particles. In the present composition, the D50 of the non-spherical BN particles is preferably smaller than the D50 of the spherical BN particles. The ratio of D50 of the spherical BN particles to D50 of the non-spherical BN particles is preferably 2.5 or more, more preferably 4 or more. In addition, the above ratio is preferably 8 or less.
[0026] In the present composition, the mass ratio of the F particles to the total mass of the F particles, the spherical BN particles, and the non-spherical BN particles is preferably 20% or more and 80% or less. The mass ratio of the F particles to the total mass of the F particles, the spherical BN particles, and the non-spherical BN particles is more preferably 35% or more, and further preferably 40% or more. The ratio is more preferably 70% or less, and further preferably 60% or less. The total content of the F particles, spherical BN particles, and non-spherical BN particles in the present composition is preferably 50% by mass or more. When the content, content ratio, and D50 relationship of the F particles, spherical BN particles, and non-spherical BN particles are within the above ranges, the composition has excellent dispersibility due to the above mechanism of action. In addition, it is preferred from the viewpoint of obtaining a sheet having low linear expansion coefficient, dielectric constant, and dielectric loss tangent and excellent thermal conductivity, bending resistance, and adhesion from the composition.
[0027] In the present composition, the surfaces of the spherical BN particles and the non-spherical BN particles are preferably surface-treated with a silane coupling agent. The silane coupling agent may partially react and may also form a polysiloxane skeleton. Specific products of the silane coupling agent include, for example, "KBM-573", "KBM-403", "KBM-903", "KBE-903", "KBM-1403", "X-12-967C", "X-12-1214A", "X-12-984S", "X-12-1271A", "KBP-90", "KBM-6803", "X-12-1287A", "KBM-402", "KBE-402", "KBE-403", "KR-516", "KBM-303", "KBM-4803", "KBM-3063", and "KBM-13" (all of which are manufactured by Shin-Etsu Chemical Co., Ltd.).
[0028] As a method for surface treating the surface of spherical BN particles and non-spherical BN particles with a silane coupling agent, a method of mixing a solution containing a silane coupling agent with spherical BN particles or non-spherical BN particles and drying them can be cited. During the mixing process, the mixture of the solution and the spherical BN particles or non-spherical BN particles can be heated or water can be added to promote the reaction of the silane coupling agent. In addition, the reaction of the silane coupling agent can be promoted by a reaction catalyst. Furthermore, after drying, the spherical BN particles or non-spherical BN particles surface treated with a silane coupling agent can be crushed or classified. Alternatively, the spherical BN particles and the non-spherical BN particles used in the present composition may be mixed in advance and then surface treated with the silane coupling agent at once.
[0029] The present composition may further contain other inorganic particles different from the spherical BN particles and the non-spherical BN particles within the scope of not impairing the effect of the present invention. The shape of the other inorganic particles may be any one of spherical, needle-shaped, fibrous or plate-shaped. As inorganic compounds of other inorganic particles, for example, carbon fiber, glass, aluminum nitride, beryllium oxide, silicon dioxide, wollastonite, talc, cerium oxide, aluminum oxide, magnesium oxide, zinc oxide or titanium oxide may be cited. When the present composition further contains other inorganic particles, the content thereof is preferably 1 to 20% by mass based on the entire composition.
[0030] The present composition may further contain another resin different from polymer F. The other resin may be contained in the present composition in the form of particles, or, when the present composition further contains a liquid dispersion medium described below, may be contained in the present composition by being dissolved or dispersed in the liquid dispersion medium. As other resins, polyester resins such as liquid crystalline aromatic polyesters, polyimide resins, polyamideimide resins, epoxy resins, maleimide resins, polyurethane resins, polyphenylene ether resins, polyphenylene ether resins and polyphenylene sulfide resins may be mentioned. As the other resin, an aromatic polymer is preferred, and at least one aromatic imide polymer selected from aromatic polyimide, aromatic polyamic acid, aromatic polyamideimide and a precursor of aromatic polyamideimide is more preferred. The aromatic polymer is preferably contained in the present composition in the form of a varnish dissolved in a liquid dispersion medium. When the present composition further contains other resins, the content thereof is preferably 0.1 to 5% by mass based on the entire composition.
[0031] The present composition may be in powder form, or may be in liquid form (dispersion liquid form, slurry form) or kneaded powder form by further containing a liquid dispersion medium. In addition, the present composition in powder form may be further melted to obtain the present composition in granular form. The present composition preferably further comprises a liquid dispersion medium and is in a liquid state (dispersed liquid state, slurry state). When the present composition is in a liquid state, in addition to the excellent dispersibility of the F particles, spherical BN particles, and non-spherical BN particles, the above-mentioned action mechanism based on the spherical BN particles and non-spherical BN particles is more likely to be manifested, and a sheet having excellent thermal conductivity and bending resistance is easily obtained. The liquid dispersion medium is a compound that is liquid at 25° C. under atmospheric pressure, preferably a compound with a boiling point of 50 to 240° C. One liquid dispersion medium may be used, or two or more liquid dispersion media may be used. When two liquid dispersion media are used, the two liquid dispersion media are preferably miscible with each other.
[0032] The liquid dispersion medium is preferably a compound selected from water, amides, ketones and esters. Examples of the amide include N-methyl-2-pyrrolidone, N,N-dimethylformamide, N,N-dimethylacetamide, N,N-dimethylpropionamide, 3-methoxy-N,N-dimethylpropionamide, 3-butoxy-N,N-dimethylpropionamide, N,N-diethylformamide, hexamethylphosphoric triamide and 1,3-dimethyl-2-imidazolidinone. The ketone may, for example, be acetone, methyl ethyl ketone, methyl isopropyl ketone, methyl isobutyl ketone, methyl n-amyl ketone, methyl isoamyl ketone, 2-heptanone, cyclopentanone, cyclohexanone or cycloheptanone. Examples of the ester include methyl acetate, ethyl acetate, butyl acetate, methyl lactate, ethyl lactate, methyl pyruvate, ethyl pyruvate, methyl methoxypropionate, ethyl ethoxypropionate, ethyl 3-ethoxypropionate, γ-butyrolactone and γ-valerolactone.
[0033] When the present composition contains a liquid dispersion medium, the content of the liquid dispersion medium is preferably in the range of 10 to 70% by mass based on the entire present composition. When the present composition includes a liquid dispersion medium, the solid content concentration in the present composition is preferably 30% by mass or more, more preferably 40% by mass or more, and further preferably 50% by mass or more. The solid content concentration is preferably 90% by mass or less, and more preferably 60% by mass or less. Here, the solid content refers to the total amount of substances that form the solid content in a formed product such as a sheet formed from the present composition. Specifically, F particles, spherical BN particles, and non-spherical BN particles are solid components. When the present composition contains other resins or other inorganic particles, these other resins or other inorganic particles are also solid components, and the total mass ratio of these components is the solid content concentration in the present composition.
[0034] When the present composition contains a liquid dispersion medium, the present composition preferably further contains a surfactant from the viewpoint of improving dispersion stability. The surfactant is preferably a nonionic surfactant. Specific examples of nonionic surfactants include: "Ftergent" series (manufactured by Neos Co., Ltd.), "Surflon" series (manufactured by AGC Seimi Chemical Co., Ltd.), "MEGA FACE" series (manufactured by DIC Corporation), "Unidyne" series (manufactured by Daikin Industries, Ltd.), "BYK-347", "BYK-349", "BYK-378", "BYK-3450", "BYK-3451", "BYK-3455", "BYK-3456" (manufactured by BYK Chemical Japan Co., Ltd.), "KF-6011", "KF-6043" (manufactured by Shin-Etsu Chemical Co., Ltd.), and "Tergitol" series (manufactured by The Dow Chemical Company, "Tergitol TMN-100X", etc.). When the present composition contains a nonionic surfactant, the content of the nonionic surfactant in the present composition is preferably 0.1 to 10% by mass based on the entire present composition.
[0035] The present composition may further include a silane coupling agent as required. As the silane coupling agent, the same silane coupling agent as that used for the surface treatment of spherical BN particles and non-spherical BN particles may be cited. When the present composition includes a silane coupling agent, the content of the silane coupling agent in the present composition is preferably 0.1 to 10% by mass relative to the overall composition.
[0036] The composition may further include additives such as thixotropy imparting agents, viscosity modifiers, defoaming agents, dehydrating agents, plasticizers, weathering agents, antioxidants, heat stabilizers, lubricants, antistatic agents, whitening agents, colorants, conductive agents, mold release agents, surface treatment agents other than the above-mentioned silane coupling agents, and flame retardants.
[0037] When the present composition contains a liquid dispersion medium and is in liquid form, the viscosity is preferably 10 mPa·s or more, more preferably 100 mPa·s or more. The viscosity of the present composition is preferably 10000 mPa·s or less, more preferably 3000 mPa·s or less. When the present composition contains a liquid dispersion medium and is in a liquid state, the thixotropic ratio thereof is preferably 1.0 to 3.0. When the present composition contains water as a liquid dispersion medium, from the viewpoint of improving long-term storage properties, the pH value is more preferably 8 to 10. The pH value of the present composition can be adjusted by a pH adjuster (amine, ammonia, citric acid, etc.) or a pH buffer (tris(hydroxymethyl)aminomethane, ethylenediaminetetraacetic acid, ammonium bicarbonate, ammonium carbonate, ammonium acetate, etc.).
[0038] The present composition can be obtained by mixing F particles, spherical BN particles, and non-spherical BN particles with other resins, other inorganic particles, a liquid dispersion medium, a surfactant, a silane coupling agent, additives, and the like as needed. The present composition can be obtained by mixing F particles, spherical BN particles and non-spherical BN particles together, or by mixing them separately in sequence, or by making a masterbatch of these materials in advance and then mixing them with the remaining components. There is no particular restriction on the order of mixing, and the mixing method can be a one-time mixing or a multiple mixing. Examples of the mixing device for obtaining the present composition include stirring devices equipped with blades such as Henschel mixers, pressure kneaders, Banbury mixers and planetary mixers; pulverizing devices equipped with media such as ball mills, crushers, basket mills, sand mills, sand mills, DYNO mills, DISPERMAT dispersers, SC mills, Spike mills and stirred mills; and dispersing devices equipped with other mechanisms such as microfluidizers, nanometers, Ultimaizer dispersers, ultrasonic homogenizers, dissolvers, dispersers, high-speed impeller dispersers, thin film gyratory high-speed mixers, rotational revolution stirrers and V-type mixers. A planetary mixer is a stirring device with two stirring blades that rotate and revolve around each other. A thin film gyratory high-speed mixer is a stirring device that spreads F particles and liquid dispersion medium on the inner wall of a cylindrical stirring tank in a thin film shape and rotates, mixing while applying centrifugal force.
[0039] As an example of a method for producing the present composition comprising a liquid dispersion medium, a method for producing the present composition can be exemplified by adding F particles, spherical BN particles, non-spherical BN particles and a liquid dispersion medium preferably together and performing a shearing treatment. In this case, it is preferred to mix in a tank having a stirring mechanism performed by a thin film rotation or a stirring mechanism performed by rotation and revolution to perform the above-mentioned shearing treatment, and it is preferred to perform the shearing treatment in a thin film rotation type high-speed mixer, a planetary mixer or a rotation and revolution mixer. In addition, as another example of the manufacture method of the present composition comprising a liquid dispersion medium, it is possible to cite a method of pre-mixing a portion of F particles, spherical BN particles, non-spherical BN particles and a liquid dispersion medium to obtain a mixed material, and then adding the mixed material to the remaining liquid dispersion medium to obtain the manufacture method of the present composition. The liquid dispersion medium used during mixing and adding can be the same liquid dispersion medium or a different liquid dispersion medium. Spherical BN particles, non-spherical BN particles, other resins, other inorganic particles, surfactants, silane coupling agents, additives can be mixed during mixing or mixed during addition. The mixing during mixing is preferably carried out in a planetary mixer or a rotation and revolution mixer.
[0040] The kneaded material obtained by kneading may be in a paste state (such as a paste having a viscosity of 1,000 to 100,000 mPa·s) or in a wet powder state (such as a wet powder having a viscosity of 10,000 to 100,000 Pa·s as measured by capillary rheology). The viscosity measured by capillary rheology refers to the viscosity of a capillary with a capillary length of 10 mm and a capillary radius of 1 mm in a furnace with a diameter of 9.55 mm, a load cell capacity of 2 t, a temperature of 25 ° C, and a shear rate of 1 s. -1 The value measured under the conditions of .
[0041] The composition can be subjected to a molding method such as extrusion to obtain a molded product such as a sheet. When the present composition contains a liquid dispersion medium and is in liquid form, the present composition is preferably extruded into a sheet. The extruded sheet can be further cast by press forming, calendaring, etc. The sheet is preferably further heated to remove the liquid dispersion medium and calender the F polymer. When the present composition is in powder form, it is preferred to melt-extrude the present composition. Extrusion molding can be performed using a single-screw extruder, a multi-screw extruder, or the like. Alternatively, the present composition may be injection molded to obtain a molded product. When forming a molded product, the present composition may be directly melt-extruded or injection-molded, or the present composition may be melt-kneaded to form pellets and the pellets may be melt-extruded or injection-molded to obtain a molded product such as a sheet.
[0042] The thickness of the sheet obtained from the present composition is preferably 20 μm or more and 100 μm or less. Due to the above-mentioned action mechanism of the present composition, the sheet is excellent in bending resistance, bending resistance and other bending properties even if it is thin. The linear expansion coefficient of the sheet is preferably 100 ppm / °C or less, more preferably 80 ppm / °C or less. The lower limit of the linear expansion coefficient of the sheet is 1 ppm / °C. In addition, the linear expansion coefficient refers to a value obtained by measuring the linear expansion coefficient of a test piece in the range of 25°C or more and 260°C or less according to the measurement method specified in JIS C 6471:1995. The thermal conductivity of the sheet in the in-plane direction is preferably 1.0 W / m·K or more, and more preferably 3.0 W / m·K or more. The upper limit of the thermal conductivity of the sheet is 100 W / m·K.
[0043] The sheet material is stacked on the substrate to form a laminate. As a method for manufacturing the laminate, there can be exemplified a method of extruding the composition together with the raw materials of the substrate using a coextruder as the above-mentioned extruder, a method of extruding the composition on the above-mentioned substrate, a method of thermocompression bonding the sheet material to the above-mentioned substrate, etc. Examples of the substrate include metal substrates (metal foils of copper, nickel, aluminum, titanium, alloys thereof, etc.), heat-resistant resin films (heat-resistant resin films such as polyimide, polyamide, polyetheramide, polyphenylene sulfide, polyallyl ether ketone, polyamideimide, liquid crystalline polyester, tetrafluoroethylene polymers, etc.), prepreg substrates (precursors of fiber-reinforced resin substrates), ceramic substrates (ceramic substrates such as silicon carbide, aluminum nitride, silicon nitride, etc.), and glass substrates.
[0044] The shape of the substrate may be a flat surface, a curved surface, a concave-convex shape, etc. The substrate may be in any of a foil shape, a plate shape, a film shape, and a fiber shape. The ten-point average roughness of the substrate surface is preferably 0.01 to 0.05 μm. The substrate surface can be surface treated with a silane coupling agent or plasma treated. As the silane coupling agent, preferably a silane coupling agent having a functional group such as 3-aminopropyltriethoxysilane, vinyltrimethoxysilane, 3-mercaptopropyltrimethoxysilane, 3-glycidyloxypropylmethyldiethoxysilane, 3-methacryloxypropyltriethoxysilane, 3-isocyanatepropyltriethoxysilane, etc. The peel strength between the sheet and the substrate is preferably 2 kN / m or more, more preferably 2.5 kN / m or more. The peel strength is preferably 10 kN / m or less.
[0045] Furthermore, the present composition is applied to the surface of a substrate and heated to form a polymer layer containing F polymer and spherical BN particles and non-spherical BN particles, thereby obtaining a laminate having a substrate layer composed of a substrate and a polymer layer. The polymer layer is preferably formed by placing the present composition containing a liquid dispersion medium on the surface of the substrate, heating to remove the dispersion medium, and further heating to calcine the F polymer. As the substrate, there may be mentioned the same substrates as those which may be laminated with the above-mentioned sheet, and the preferred embodiments thereof are also the same.
[0046] The method for disposing the present composition may, for example, be a coating method, a droplet discharging method or a dipping method, and preferably a roll coating method, a knife coating method, a bar coating method, a die coating method or a spraying method. The heating for removing the liquid dispersion medium is preferably performed at 100 to 200° C. for 0.1 to 30 minutes. During the heating at this time, the liquid dispersion medium does not need to be completely removed, as long as the layer formed by the filler of F particles, spherical BN particles and non-spherical BN particles can maintain a self-supporting film. In addition, air can be blown during heating to promote the removal of the liquid dispersion medium by air drying. The heating during calcination of the F polymer is preferably performed at a temperature equal to or higher than the calcination temperature of the F polymer, more preferably at 360 to 400° C. for 0.1 to 30 minutes. As the heating device in each heating, an oven or a ventilated drying furnace can be mentioned. The heat source in the device can be a contact heat source (hot air, a heating plate, etc.) or a non-contact heat source (infrared rays, etc.). In addition, each heating may be performed under normal pressure or under reduced pressure. In addition, the atmosphere during each heating may be any of an air atmosphere and an inert gas (helium, neon, argon, nitrogen, etc.) atmosphere.
[0047] The polymer layer is formed by the arrangement and heating steps of the present composition. These steps can be performed one by one or more times. For example, the present composition can be arranged on the surface of a substrate and heated to form a polymer layer, and the present composition can be further arranged on the surface of the polymer layer and heated to form a second polymer layer. In addition, the present composition can be arranged on the surface of a substrate and heated to remove the liquid dispersion medium, and then the present composition can be further arranged on the surface and heated to form a polymer layer. The thickness of the polymer layer is preferably 20 μm or more and 100 μm or less, more preferably 50 μm or less, and even more preferably 50 μm or less. Due to the above-mentioned mechanism of action of the present composition, the polymer layer is excellent in bending resistance, folding resistance and other bending properties even if it is thin. The present composition may be disposed on only one surface of the substrate or on both surfaces of the substrate. In the former case, a laminate having a substrate layer and a polymer layer on one surface of the substrate layer may be obtained, and in the latter case, a laminate having a substrate layer and polymer layers on both surfaces of the substrate layer may be obtained.
[0048] Preferred specific examples of the laminate include a metal-clad laminate having a metal foil and a polymer layer on at least one surface of the metal foil, and a multilayer film having a polyimide film and polymer layers on both surfaces of the polyimide film. The preferred ranges of the linear expansion coefficient of the polymer layer, the thermal conductivity in the in-plane direction, and the peel strength between the polymer layer and the substrate layer are the same as the preferred ranges of the linear expansion coefficient, the thermal conductivity in the in-plane direction, and the peel strength between the sheet and the substrate obtained from the above-mentioned present composition.
[0049] The present composition can be used as a material for imparting insulation, heat resistance, corrosion resistance, chemical resistance, water resistance, impact resistance, and thermal conductivity. Specifically, the composition can be used for printed wiring boards, thermal interface materials, substrates for power modules, coils used in power equipment such as motors, vehicle engines, heat exchangers, vials, syringes (Syringe), ampoules, medical wires, secondary batteries such as lithium-ion secondary batteries, primary batteries such as lithium batteries, free radical batteries, solar cells, fuel cells, lithium-ion capacitors, hybrid capacitors, capacitors (capacitors), capacitors (condensers) (aluminum electrolytic capacitors, tantalum electrolytic capacitors, etc.), electrochromic elements, electrochemical conversion elements, electrode adhesives, electrode separators, electrodes (positive and negative electrodes). In addition, the composition can also be used as an adhesive for bonding parts. Specifically, the composition can be used for bonding ceramic parts, bonding metal parts, bonding IC chips and resistors, capacitors and other electronic parts on the substrate of semiconductor elements or module parts, bonding circuit substrates and heat sinks, and bonding LED chips on substrates. In addition, the composition of the present invention can also be used for applications requiring electrical conductivity, such as the field of printed electronics, and can be used specifically to manufacture current-carrying elements such as printed circuit boards and sensor electrodes.
[0050] The molded products, sheets and laminates formed from the present composition can be used as antenna parts, printed circuit boards, aircraft parts, automobile parts, sports equipment, food industry products, heat dissipation parts and the like. Specifically, it can be used as wire coating materials (such as wires for aircraft), enameled wire coating materials used in motors of electric vehicles, etc., electrical insulating tapes, insulating tapes for oil drilling, oil pipelines, hydrogen tanks, printed circuit board materials, separation membranes (precision filtration membranes, ultrafiltration membranes, reverse osmosis membranes, ion exchange membranes, dialysis membranes, gas separation membranes, etc.), electrode adhesives (for lithium secondary batteries, fuel cells, etc.), copy rollers, covers for furniture, automobile dashboards, home appliances, etc., sliding parts (load bearings, yaw bearings, sliding shafts, valves, bearings, Bushings, seals, thrust washers, mounting rings, pistons, slide switches, gears, cams, belt conveyors, food conveyor belts), tension ropes, wear pads, wear strips, tube lights, test sockets, wafer guides, wear parts of centrifugal pumps, chemical and water supply pumps, tools (shovels, files, chisels, saws), boilers, hoppers, pipes, ovens, baking molds, chutes, racket strings, molds, toilets, container covering materials, heat dissipation substrates for power devices, heat dissipation components of wireless communication devices, transistors, thyristors, rectifiers, transformers, power MOS FETs, CPUs, heat sinks, metal heat sinks, blades of windmills or wind power generation equipment or aircraft, computer or display housings, electronic device materials, automotive interior and exterior trim, processing machines or vacuum furnaces that perform heat treatment under low oxygen, sealing materials for plasma processing devices, heat dissipation components in processing units such as sputtering or various dry etching devices, and electromagnetic wave shielding bodies. The molded products, sheets and laminates formed from the present composition can be particularly used as electronic substrate materials such as flexible printed circuit boards and rigid printed circuit boards for automotive electronics such as LED headlights, power control units or electrical control units, heat sinks or heat dissipation substrates, and heat dissipation substrates for automobiles. When a molded product, sheet or laminate formed from the present composition is used as a heat dissipation component, it can be directly adhered to a substrate such as the molded product, sheet or laminate, or it can be bonded to the substrate via an adhesive layer such as a silicone adhesive layer.
[0051] As mentioned above, although this composition, the manufacturing method of this composition, the manufacturing method of a sheet material, the manufacturing method of a laminated body, and a laminated body were demonstrated, this invention is not limited to the structure of the said embodiment. For example, this composition and laminate can add other arbitrary structures in the formation of the above-mentioned embodiment, and can also be replaced by any structure that plays the same function. In addition, the manufacture method of this composition, sheet material or laminate can add other arbitrary processes in the formation of the above-mentioned embodiment respectively, and can also be replaced by any process that produces the same effect. Example
[0052] Hereinafter, the present invention will be described in detail by way of examples, but the present invention is not limited thereto. 1. Preparation of Ingredients [F polymer] F particles 1: each containing 97.9 mol%, 0.1 mol%, and 2.0 mol% of TFE units, NAH units, and PPVE units, respectively. 6 Particles of tetrafluoroethylene polymer (melting temperature: 300°C) having 1000 carbonyl groups in the main chain (D50: 2.1 μm) [Boron nitride particles] Boron nitride particles 1: Spherical boron nitride particles (D50: 12 μm) Boron nitride particles 2: Spherical boron nitride particles (D50: 45 μm) Boron nitride particles 3: non-spherical (scaly) boron nitride particles (D50: 4 μm) Boron nitride particles 4: non-spherical (scaly) boron nitride particles (D50: 15 μm) [Liquid dispersion medium] NMP: N-methyl-2-pyrrolidone
[0053] 2. Preparation Example of Composition [Example 1] F particles 1, boron nitride particles 1, boron nitride particles 3 and NMP were kneaded in a planetary mixer to obtain a wet powdered kneaded powder 1, and NMP was added several times and stirred to obtain a liquid composition 1 containing F particles 1 (30 parts by mass), boron nitride particles (30 parts by mass, boron nitride particles 1: boron nitride particles 3 = 80:20 (mass ratio) and NMP (40 parts by mass). [Example 2] In the same manner as in Example 1, except that the mass ratio of the boron nitride particles 1 to the boron nitride particles 3 was changed, a liquid composition 2 comprising the F particles 1 (30 parts by mass), the boron nitride particles (30 parts by mass, the boron nitride particles 1: the boron nitride particles 3 = 75:25 (mass ratio) and NMP (40 parts by mass) was obtained.
[0054] [Example 3] In the same manner as in Example 1, except that the boron nitride particles 1 were replaced with the boron nitride particles 2, a liquid composition 3 comprising the F particles 1 (30 parts by mass), the boron nitride particles (30 parts by mass, the boron nitride particles 2: the boron nitride particles 3 = 70:30 (mass ratio) and NMP (40 parts by mass) was obtained. [Example 4] In the same manner as in Example 1, except that the boron nitride particles 3 were replaced with boron nitride particles 4, a liquid composition 4 comprising F particles 1 (30 parts by mass), boron nitride particles (30 parts by mass, boron nitride particles 1:boron nitride particles 4=70:30 (mass ratio) and NMP (40 parts by mass) was obtained. [Example 5] F particles 1, boron nitride particles 1 and NMP are kneaded in a planetary mixer to obtain a wet powdered kneaded powder 1, and NMP is added in multiple portions and stirred to obtain a liquid composition 5 containing F particles 1 (30 parts by mass), boron nitride particles (30 parts by mass) and NMP (40 parts by mass).
[0055] 3. Manufacturing of laminated body The composition 1 was applied on the surface of the long copper foil by a bar coater to form a wet film. Then, the copper foil formed with the wet film was dried in a drying furnace at 110° C. for 5 minutes to form a dry film. Then, the copper foil with the dry film was heated in a nitrogen oven at 380° C. for 3 minutes. Thus, a laminate 1 having a copper foil and a polymer layer with a thickness of 100 μm containing a molten sintered product of F particles 1 and boron nitride particles 1 and boron nitride particles 3 on the surface thereof was prepared. Laminates 2 to 5 were prepared from compositions 2 to 5 in the same manner as for the laminate 1 .
[0056] 4. Evaluation of laminated body 4-1. Peel strength of laminate A rectangular test piece (100 mm long and 10 mm wide) was cut from each laminate. Then, the test piece was fixed at a position 50 mm away from one end in the longitudinal direction, and the copper foil and the polymer layer were peeled off from one end in the longitudinal direction at 90° relative to the test piece at a tensile speed of 50 mm / min. Then, the maximum load applied at this time was measured as peel strength (N / cm), and evaluated according to the following criteria. [Evaluation criteria] ○: 2kN / m or more △: 1kN / m or more and less than 2kN ×: less than 1kN / m
[0057] 4-2. Bendability Each laminate was etched with an aqueous solution of ferric chloride to remove the copper foil of the laminate, thereby producing a sheet of a single polymer layer. A 5 mm square test piece was cut from the produced sheet, bent 180° at a curvature radius (300 μm), and folded back after applying a load (50 mN, 1 minute) from above. The appearance of the test piece was evaluated according to the following criteria. [Evaluation criteria] ○: No abnormality in appearance was observed at the crease. △: Whitening is observed at the crease. ×: Broken at the crease position.
[0058] 4-3. Thermal conductivity A 10 mm×10 mm square test piece was cut out from the center of each sheet obtained in the same manner as in 4-2, and the thermal conductivity (W / m·K) in the in-plane direction was measured and evaluated according to the following criteria. [Evaluation criteria] ○: greater than 2W / m·K △: 1W / m·K or more and 2W / m·K or less ×: less than 1W / m·K The above evaluation results are summarized in Table 1.
[0059] Table 1 Laminated body number 1 2 3 4 5 Peel strength ○ ○ ○ × △ Bendability ○ △ × ○ △ Thermal conductivity ○ △ △ × × Industrial Applicability
[0060] The above results show that the present composition has excellent dispersion stability, and the laminate formed from the present composition highly exhibits the physical properties of the F polymer and the boron nitride particles, has excellent peel strength (adhesion) and thermal conductivity, and also has excellent bending resistance.
[0061] The entire contents of the specification, claims, and abstract of Japanese Patent Application No. 2022-030107 filed on February 28, 2022 are cited herein and are incorporated herein as a disclosure of the specification of the present invention.
Claims
1. A composition comprising particles of a tetrafluoroethylene polymer, spherical boron nitride particles having an average particle size of 5 μm or more and 40 μm or less, and non-spherical boron nitride particles having an average particle size of less than 15 μm, wherein the mass ratio of the non-spherical boron nitride particles to the total mass of the spherical boron nitride particles and the non-spherical boron nitride particles is less than 30%.
2. The composition according to claim 1, wherein The tetrafluoroethylene polymer is a hot-melt tetrafluoroethylene polymer.
3. The composition according to claim 1 or 2, wherein The tetrafluoroethylene polymer is a tetrafluoroethylene polymer having an oxygen-containing polar group.
4. The composition according to claim 1 or 2, wherein The average particle size of the tetrafluoroethylene-based polymer particles is smaller than either the average particle size of the spherical boron nitride particles or the average particle size of the non-spherical boron nitride particles.
5. The composition according to claim 1 or 2, wherein The average particle size of the non-spherical boron nitride particles is smaller than the average particle size of the spherical boron nitride particles.
6. The composition according to claim 1 or 2, wherein The ratio of the average particle size of the spherical boron nitride to the average particle size of the non-spherical boron nitride particles is greater than 2.
5.
7. The composition according to claim 1 or 2, wherein The mass ratio of the tetrafluoroethylene polymer particles to the total mass of the tetrafluoroethylene polymer particles, the spherical boron nitride particles, and the non-spherical boron nitride particles is 20% or more and 80% or less.
8. The composition according to claim 1 or 2, wherein The total content of the tetrafluoroethylene polymer particles, the spherical boron nitride particles, and the non-spherical boron nitride particles in the composition is 50% or more.
9. The composition according to claim 1 or 2, wherein A liquid dispersion medium is also included.
10. The method for producing the composition according to claim 9, wherein: Particles of tetrafluoroethylene polymer, spherical boron nitride particles having an average particle size of 5 μm or more and 40 μm or less, non-spherical boron nitride particles having an average particle size of less than 15 μm, and a liquid dispersion medium are subjected to a shear treatment.
11. The method for producing a composition according to claim 10, wherein: The shear treatment is performed by mixing in a tank equipped with a stirring mechanism that is performed by the rotation of the film or a stirring mechanism that is performed by rotation and revolution.
12. A method for producing a sheet material, wherein: The composition according to claim 1 or 2 is extruded to obtain a sheet comprising the tetrafluoroethylene polymer, the spherical boron nitride particles, and the non-spherical boron nitride particles.
13. A method for producing a laminate, wherein: The composition according to claim 1 or 2 is applied to the surface of a substrate and heated to form a polymer layer containing the tetrafluoroethylene polymer, the spherical boron nitride particles and the non-spherical boron nitride particles, thereby obtaining a laminate having a substrate layer composed of the substrate and the polymer layer. 14 . A laminate comprising a substrate layer and a polymer layer formed from the composition according to claim 1 or 2 and containing the tetrafluoroethylene polymer, the spherical boron nitride particles, and the non-spherical boron nitride particles.
15. The laminate according to claim 14, wherein The polymer layer has a thickness of 20 μm or more and 100 μm or less.