All-solid-state battery and manufacturing method thereof
By using flat active material particles in the negative electrode layer of an all-solid-state lithium-ion battery and forming a dense coating layer, the problem of interface peeling caused by lithium ion conduction and expansion and contraction is solved, and the battery capacity and charge and discharge characteristics are improved.
Patent Information
- Application Number
- CN202280092685.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-03-10
- Filing Date
- 2022-12-08
- Publication Date
- 2024-10-11
AI Technical Summary
In existing all-solid-state lithium-ion batteries, when granulated particles formed by stacking multiple graphite flakes are used as negative electrode active materials, it is easy to hinder the conduction of lithium ions, resulting in a reduction in battery capacity, and is caused by expansion and contraction during charging and discharging. The peeling problem further reduces battery performance.
By using a flat -shaped active substance particles with multiple graphite small sheets in the negative layer, and forming a dense layer composed of solid electrolyte in its long shaft direction, ensuring that the conduction path of lithium ions is not blocked, and the power is charged and the power is charged. It can alleviate the stress caused by expansion and contraction and reduce the interface peeling between the negative electrode layer and the solid electrolyte layer.
It effectively suppresses the reduction of battery capacity, improves the conduction efficiency of lithium ions, and enhances the charge and discharge characteristics and durability of the battery, especially under high-rate charge and discharge conditions.
Smart Images

Figure CN118765450A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to an all-solid-state battery and a method for manufacturing the same, and in particular to an all-solid-state battery using a positive electrode layer, a negative electrode layer and a solid electrolyte layer and a method for manufacturing the same. Background Art
[0002] In recent years, due to the lightweight and wireless development of electronic devices such as personal computers and mobile phones, there is a demand for the development of reusable secondary batteries. Secondary batteries include nickel-cadmium batteries, nickel-metal hydride batteries, lead-acid batteries, lithium-ion batteries, etc. Among them, lithium-ion batteries have attracted attention due to their characteristics such as light weight, high voltage, and high energy density.
[0003] In the automotive field such as electric vehicles and hybrid vehicles, the development of secondary batteries with high battery capacity is also receiving attention, and the demand for lithium-ion batteries is tending to increase.
[0004] Lithium-ion batteries are composed of a positive electrode layer, a negative electrode layer, and an electrolyte disposed therebetween. The electrolyte uses an electrolyte or solid electrolyte made by dissolving a supporting salt such as lithium hexafluorophosphate in an organic solvent. At present, widely used lithium-ion batteries are flammable because they use an electrolyte containing an organic solvent. Therefore, materials, structures, and systems are needed to ensure the safety of lithium-ion batteries. In contrast, by using a non-flammable solid electrolyte as an electrolyte, it is expected that the above-mentioned materials, structures, and systems can be simplified, and it is believed that an increase in energy density, a reduction in manufacturing costs, and an increase in productivity can be achieved. Hereinafter, batteries using solid electrolytes such as lithium-ion batteries using solid electrolytes that conduct lithium (Li) ions are referred to as "all-solid-state batteries."
[0005] Solid electrolytes can be roughly divided into organic solid electrolytes and inorganic solid electrolytes. In addition, as inorganic solid electrolytes, oxide-based solid electrolytes, sulfide-based solid electrolytes and halide-based solid electrolytes are generally used. Here, sulfide-based solid electrolytes and halide-based solid electrolytes have smaller grain boundary resistance than oxide-based solid electrolytes, so they have the characteristics of being able to obtain good properties only by compression molding of powders without using a sintering process. In the development of all-solid-state batteries for further large-scale and high-capacity, research on large-scale coated all-solid-state batteries using sulfide-based solid electrolytes has been popular in recent years.
[0006] As a method for manufacturing an all-solid-state battery, Patent Document 1 discloses a method for producing a negative electrode layer by pressure-molding a mixture of negative electrode active material particles and solid electrolyte particles.
[0007] Prior art literature
[0008] Patent Literature
[0009] Patent Document 1: Japanese Patent Application Laid-Open No. 8-138724 Summary of the invention
[0010] An all-solid-state battery of one embodiment of the present invention comprises a positive electrode collector, a positive electrode layer comprising a positive electrode active material and a first solid electrolyte, a solid electrolyte layer comprising a third solid electrolyte, a negative electrode layer comprising a negative electrode active material and a second solid electrolyte, and a negative electrode collector stacked in sequence, the negative electrode active material comprising a plurality of flat active material particles, the flat active material particles having a structure formed by stacking a plurality of small graphite flakes, the negative electrode layer having an active material orientation region in which two or more of the plurality of flat active material particles are adjacently arranged in a cross section of the negative electrode layer cut along the thickness direction of the negative electrode layer, and in the cross section, the major axis directions of the two or more flat active material particles respectively form an angle of 0° or more and 30° or less with respect to the thickness direction of the negative electrode layer.
[0011] In addition, a method for manufacturing an all-solid-state battery according to one embodiment of the present invention is the method for manufacturing the all-solid-state battery described above, wherein the manufacturing process of the negative electrode layer includes a mixing process of the negative electrode active material and the second solid electrolyte, wherein the mixing process uses a negative electrode active material comprising a plurality of active material particles, wherein the active material particles are non-spherical shapes having a long axis direction and a short axis direction, and are formed by stacking and granulating a plurality of graphite flakes, and wherein the mixing process includes a step of forming a coating layer composed of a second solid electrolyte and covering the ends of two or more of the plurality of active material particles in the long axis direction. BRIEF DESCRIPTION OF THE DRAWINGS
[0012] Figure 1 It is a schematic diagram showing a cross section of an all-solid-state battery in an embodiment.
[0013] Figure 2 It is a schematic diagram for explaining the method for manufacturing an all-solid-state battery in an embodiment.
[0014] Figure 3 This is a flowchart showing a method for producing a negative electrode mixture in an embodiment.
[0015] Figure 4 This is a flow chart showing a method for producing a negative electrode mixture in a comparative example.
[0016] Figure 5 It is a schematic diagram for explaining the change in the state of the negative electrode active material and the solid electrolyte in the comparative example.
[0017] Figure 6 It is a schematic diagram for explaining the change in the state of the negative electrode active material and the solid electrolyte in the embodiment.
[0018] Figure 7 This is an electron microscope image showing the appearance of the negative electrode mixture in the embodiment.
[0019] Figure 8 This is an electron microscope image showing a cross section of a negative electrode layer in the embodiment.
[0020] Fig. 9 It is a schematic diagram for explaining the change in the state of the negative electrode active material and the solid electrolyte in the mixing step in the embodiment. DETAILED DESCRIPTION
[0021] (Process of obtaining one embodiment of the present invention)
[0022] The present inventors have found that the conventional all-solid-state battery described in the “Background Art” column has the following problems.
[0023] Generally, in order to stabilize the battery manufacturing process and improve the fluidity of the active material, it is mainstream to treat the active material as granulated particles formed by forming a plurality of small pieces into particles. However, in the method disclosed in Patent Document 1, when granulated particles formed by stacking a plurality of small pieces of graphite are used as negative electrode active material particles, the following two problems arise.
[0024] The first problem is that the granulated particles hinder the conduction of lithium ions. Specifically, when the negative electrode active material particles and the solid electrolyte particles are mixed and then put into a mold for pressurization, the granulated particles used for the negative electrode active material are flattened to become flat active material particles. In the negative electrode layer, such flat active material particles are easy to hinder the conduction of lithium ions in the thickness direction of the negative electrode layer due to their flat shape, and the battery capacity is reduced. In particular, when charging and discharging at a high rate, the battery capacity is easy to reduce.
[0025] Here, the flat active material particles refer to active material particles having a non-spherical shape formed by randomly stacking and granulating a plurality of graphite flakes, and then pressing and flattening them, whereby the graphite flakes are compressed into an oriented and stacked shape, and are hereinafter referred to as "flat active material particles".
[0026] The second problem is that the flat active material particles of the negative electrode active material in the negative electrode layer expand and shrink due to charging and discharging, thereby causing peeling in the negative electrode layer and at the interface between the negative electrode layer and the solid electrolyte layer. If peeling occurs, the ion conduction path is reduced, so the battery capacity is reduced.
[0027] Therefore, in view of the above problems, the present invention provides an all-solid-state battery or the like capable of suppressing a decrease in battery capacity even when a negative electrode active material containing flat active material particles is used.
[0028] (Overview of the Invention)
[0029] An overview of one embodiment of the present invention is as follows.
[0030] An all-solid-state battery in one embodiment of the present invention comprises a positive electrode collector, a positive electrode layer comprising a positive electrode active material and a first solid electrolyte, a solid electrolyte layer comprising a third solid electrolyte, a negative electrode layer comprising a negative electrode active material and a second solid electrolyte, and a negative electrode collector stacked in sequence, the negative electrode active material comprising a plurality of flat active material particles, the flat active material particles having a structure in which a plurality of graphite flakes are stacked, the negative electrode layer having an active material orientation region in which two or more of the plurality of flat active material particles are adjacently arranged in a cross section of the negative electrode layer cut along the thickness direction of the negative electrode layer, and in the cross section, the major axis directions of the two or more flat active material particles respectively form an angle of 0° or more and 30° or less with respect to the thickness direction of the negative electrode layer.
[0031] Thus, there is an active material orientation region where flat active material particles are arranged at a small angle relative to the thickness direction, so the conduction of lithium ions is not easily hindered by the flat active material particles, and the conduction path of lithium ions in the thickness direction can be ensured in the negative electrode layer. Therefore, the reduction of battery capacity can be suppressed.
[0032] In addition, for example, the above-mentioned negative electrode layer may further have a solid electrolyte region in the above-mentioned cross-section, and the above-mentioned solid electrolyte region is located at a position adjacent to the above-mentioned active material orientation region, has an area greater than 1.5 times the average area of the above-mentioned two or more flat active material particles, contains the above-mentioned second solid electrolyte but does not contain the above-mentioned negative electrode active material.
[0033] Thus, the stress from the expansion and contraction of the negative electrode active material during charge and discharge can be relieved by the solid electrolyte region. As a result, delamination in the negative electrode layer and at the interface between the negative electrode layer and the solid electrolyte layer can be suppressed.
[0034] Furthermore, for example, in the cross section, the aspect ratio of the length in the major axis direction to the length in the minor axis direction of at least one of the two or more flat active material particles may be 3 times or more.
[0035] As a result, lithium ions can easily penetrate into graphite constituting the flat active material particles on the surface of the flat active material particles, and the negative electrode active material is effectively utilized, thereby improving the battery capacity.
[0036] For example, the volume ratio of the negative electrode active material in the negative electrode layer to the total volume of the negative electrode active material and the second solid electrolyte may be 46% to 96%, or 56% to 75%.
[0037] This makes it easy to ensure both the lithium ion conduction path performed by the solid electrolyte and the electron conduction path performed by the negative electrode active material in the negative electrode layer.
[0038] In addition, for example, the concentration of the solvent contained in the negative electrode layer may be 50 ppm or less.
[0039] Thus, the negative electrode layer does not substantially contain a solvent, and thus degradation of the material of the negative electrode layer is suppressed.
[0040] In addition, a method for manufacturing an all-solid-state battery in one embodiment of the present invention is the method for manufacturing an all-solid-state battery mentioned above, wherein the manufacturing process of the negative electrode layer includes a mixing process of the negative electrode active material and the second solid electrolyte, and the mixing process uses a negative electrode active material comprising a plurality of active material particles, and the active material particles are non-spherical shapes having a long axis direction and a short axis direction, and are formed by stacking and granulating a plurality of small graphite flakes, and the mixing process includes a step of forming a coating layer composed of a second solid electrolyte and covering the ends of two or more active material particles in the long axis direction among the plurality of active material particles.
[0041] Thus, the coating layer covers the ends of the non-spherical active material particles, and the coating layer serves as a support to suppress the active material particles from falling in the negative electrode layer, thereby making it possible to easily manufacture an all-solid-state battery having the active material orientation region.
[0042] Furthermore, for example, the mixing step may be a step of mixing the negative electrode active material and the second solid electrolyte while applying a compressive force and a shearing force to the negative electrode active material and the second solid electrolyte.
[0043] Thereby, a dense coating layer composed of the second solid electrolyte can be formed on the end portions of the granulated active material particles of the negative electrode active material in the long axis direction.
[0044] Hereinafter, the all-solid-state battery in the embodiment is described in detail. It should be noted that the embodiments described below all represent general or specific examples. The numerical values, shapes, materials, constituent elements, configuration positions and connection forms of constituent elements, steps and processes shown in the following embodiments are examples and do not limit the subject matter of the present invention. In addition, the constituent elements in the following embodiments that are not recorded in the independent technical solutions for which protection is requested are described as arbitrary constituent elements.
[0045] In the present specification, terms such as parallel that indicate the relationship between elements, terms such as rectangle that indicate the shape of elements, and numerical ranges are not strictly defined but include substantially equivalent ranges, for example, differences of several percent.
[0046] In addition, each figure is a schematic diagram that appropriately emphasizes, omits, or adjusts the ratio in order to illustrate the present invention, and is not necessarily strictly illustrated, and sometimes differs from the actual shape, positional relationship, and ratio. In each figure, the same symbols are marked for substantially the same structure, and repeated descriptions are sometimes omitted or simplified.
[0047] In addition, in this specification, terms such as "upper" and "lower" in the structure of the all-solid-state battery do not refer to the upper direction (vertically above) and the lower direction (vertically below) in absolute spatial identification, but are used as terms defined by relative positional relationships based on the stacking order in the stacking structure.
[0048] In addition, in this specification, a cross-sectional view is a view showing a cross section when the center portion of the all-solid-state battery is cut along the stacking direction. In addition, in this specification, the stacking direction is consistent with the thickness direction of each layer of the all-solid-state battery and the normal direction of the main surface of each layer of the all-solid-state battery.
[0049] (Implementation Method)
[0050] <Composition>
[0051] [A. All-solid-state battery]
[0052] First, use Figure 1 The outline of the all-solid-state battery in this embodiment will be described. Figure 1Schematic diagram showing a cross section of an all-solid-state battery 100 in the present embodiment. The all-solid-state battery 100 in the present embodiment includes a positive electrode collector 7, a negative electrode collector 8, a positive electrode layer 20 formed on the surface of the positive electrode collector 7 close to the negative electrode collector 8 and including a positive electrode active material 2 and a solid electrolyte 1, a negative electrode layer 30 formed on the surface of the negative electrode collector 8 close to the positive electrode collector 7 and including a negative electrode active material 3 and a solid electrolyte 4, and a solid electrolyte layer 10 disposed between the positive electrode layer 20 and the negative electrode layer 30 and including a solid electrolyte 5. That is, the all-solid-state battery 100 has a structure in which the positive electrode collector 7, the positive electrode layer 20, the solid electrolyte layer 10, the negative electrode layer 30, and the negative electrode collector 8 are stacked in order.
[0053] In addition, the negative electrode active material 3 in this embodiment includes a plurality of flat active material particles. Each of the plurality of flat active material particles has a structure in which a plurality of graphite flakes are stacked. In this specification, the particle is flat in shape, for example, when the ratio of the length of the long axis direction of the particle (the so-called long diameter) to the length of the short axis direction (the so-called short diameter) is 2 times or more.
[0054] The negative electrode layer 30 has an active material orientation region 14 in which two or more of the plurality of flat active material particles are arranged adjacent to each other in the main surface direction of the negative electrode layer 30 (a direction orthogonal to the thickness direction of the negative electrode layer 30) in a cross section of the negative electrode layer 30 cut along the thickness direction of the negative electrode layer 30 (in other words, the stacking direction of the all-solid-state battery 100). Hereinafter, the cross section obtained by cutting the negative electrode layer 30 along the thickness direction of the negative electrode layer 30 is sometimes referred to as a "negative electrode layer cross section". In the negative electrode layer cross section, the angle formed by the long axis directions of the two or more flat active material particles arranged in the active material orientation region 14 relative to the thickness direction of the negative electrode layer 30 is 0° or more and 30° or less. This angle is a smaller angle among the angles formed by the long axis direction and the thickness direction. In the active material orientation region 14, the two or more flat active material particles are arranged, for example, along the short axis direction of the flat active material particles. In addition, from the viewpoint that lithium ions easily penetrate into graphite constituting the flat active material particles, the aspect ratio of at least one of the two or more flat active material particles present in the active material orientation region 14 may be 3 times or more. Alternatively, the aspect ratio may be, for example, 10 times or less.
[0055] In this specification, the length of the major axis direction is the longest distance between the distances of two parallel lines that are connected to the outline of the particle in the cross-sectional view such as the figure of the cross section of the negative electrode layer. The major axis direction is the direction orthogonal to the two parallel lines in the case of the longest distance. In addition, the length of the minor axis direction is the distance in the direction orthogonal to the major axis direction in the distance between the two parallel lines that are connected to the outline of the particle in the cross-sectional view such as the figure of the cross section of the negative electrode layer. The minor axis direction is the direction orthogonal to the major axis direction.
[0056] In the present embodiment, the solid electrolyte 5 is an example of a third solid electrolyte. The solid electrolyte 1 is an example of a first solid electrolyte. The solid electrolyte 4 is an example of a second solid electrolyte.
[0057] The all-solid-state battery 100 in the present embodiment is formed, for example, by the following method. A positive electrode layer 20 formed on a positive electrode collector 7 composed of a metal foil, a negative electrode layer 30 formed on a negative electrode collector 8 composed of a metal foil, and a solid electrolyte layer 10 arranged between the positive electrode layer 20 and the negative electrode layer 30 are formed. Then, the positive electrode collector 7 and the negative electrode collector 8 are pressed from the outside in the stacking direction, thereby making the all-solid-state battery 100. The pressing pressure is, for example, greater than 100 MPa and less than 1000 MPa. By pressing, the filling rate of at least one layer of the solid electrolyte layer 10, the positive electrode layer 20 and the negative electrode layer 30 is greater than 60% and less than 100%. It should be noted that the detailed manufacturing method of the all-solid-state battery 100 is described later.
[0058] By making the filling rate 60% or more, the voids in the solid electrolyte layer 10, the positive electrode layer 20 or the negative electrode layer 30 are reduced, so that more ion conduction and electron conduction are performed, and good charge and discharge characteristics can be obtained. It should be noted that the filling rate refers to the proportion of the volume occupied by the material other than the voids between the materials in the total volume.
[0059] The pressed all-solid-state battery 100 is mounted with terminals and housed in a case. The case of the all-solid-state battery 100 may be made of, for example, stainless steel (SUS), iron or aluminum, a resin, or an aluminum laminate bag.
[0060] Hereinafter, the solid electrolyte layer 10 , the positive electrode layer 20 , and the negative electrode layer 30 of the all-solid-state battery 100 in the present embodiment will be described in detail.
[0061] [B. Solid electrolyte layer]
[0062] First, the solid electrolyte layer 10 will be described. The solid electrolyte layer 10 in the present embodiment includes a solid electrolyte 5 and may further include a binder.
[0063] [B-1. Solid electrolyte]
[0064] The solid electrolyte 5 in this embodiment is described. As the solid electrolyte material used in the solid electrolyte 5, inorganic solid electrolytes such as sulfide solid electrolytes, halide solid electrolytes, and oxide solid electrolytes, which are generally known materials, can be cited. The solid electrolyte material has, for example, lithium ion conductivity. As the solid electrolyte material, any of a sulfide solid electrolyte, a halide solid electrolyte, and an oxide solid electrolyte can be used. The type of the sulfide solid electrolyte in this embodiment is not particularly limited. As the sulfide solid electrolyte, Li 2 S-SiS 2 、LiI-Li 2 S-SiS 2 、LiI-Li 2 SP 2 S 5 、LiI-Li 2 SP 2 O 5 、LiI-Li 3 PO 4 -P 2 S 5 , Li 2 SP 2 S 5 In particular, from the viewpoint of excellent lithium ion conductivity, the sulfide-based solid electrolyte may contain Li, P, and S. In addition, since the reactivity with the binder is high and the bonding property with the binder is high, the sulfide-based solid electrolyte may contain P. 2 S 5 It should be noted that the above “Li 2 SP 2 S 5 " refers to the use of Li 2 S and P 2 S 5 The sulfide-based solid electrolyte is composed of raw materials, and the same is true for other records.
[0065] In this embodiment, the sulfide-based solid electrolyte material includes, for example, Li 2 S and P 2 S 5 Sulfide glass ceramics, about Li 2 S and P 2 S 5 The ratio, in molar terms, of Li 2 S:P 2 S 5It may be in the range of 70:30 to 80:20, or in the range of 75:25 to 80:20. 2 S and P 2 S 5 The ratio of can form a crystal structure with high lithium ion conductivity while maintaining the lithium (Li) concentration that affects battery characteristics. 2 S and P 2 S 5 The ratio of P to the binder is thus easy to ensure 2 S 5 The amount.
[0066] The solid electrolyte 5 is composed of, for example, a plurality of particles. The average particle size of the solid electrolyte 5 is, for example, smaller than the average particle size of the negative electrode active material 3 (described later). This makes it easy to ensure a contact area with the negative electrode active material 3 in the negative electrode layer 30 .
[0067] In addition, the average particle size of the solid electrolyte 5 is, for example, 0.2 μm or more and 10 μm or less. Thus, the contact surface with the negative electrode active material 3 in the negative electrode layer 30 is ensured, and the particle interface in the solid electrolyte layer 10 is reduced, and the resistance component of the particle interface is reduced, thereby suppressing the reduction of the lithium ion conductivity of the solid electrolyte layer 10 as a whole.
[0068] [B-2. Binder]
[0069] The binder in the present embodiment is described. The binder is an adhesive material that does not have lithium ion conduction and electron conduction, and is responsible for bonding the materials in the solid electrolyte layer 10 to each other and bonding the solid electrolyte layer 10 to other layers. The binder in the present embodiment may include a thermoplastic elastomer introduced with a functional group that improves the adhesion strength, and the functional group may be a carbonyl group. From the perspective of improving the adhesion strength, the carbonyl group may be maleic anhydride. The oxygen atoms of maleic anhydride react with the solid electrolyte 5, and the solid electrolytes 5 are bonded to each other with the aid of the binder, forming a structure in which a binder is arranged between the solid electrolyte 5 and the solid electrolyte 5, resulting in improved adhesion strength.
[0070] As thermoplastic elastomers, for example, styrene-butadiene-styrene (SBS), styrene-ethylene-butadiene-styrene (SEBS), etc. are used. This is because they have high adhesion strength and high durability in the cycle characteristics of the battery. Hydrogenated (hereinafter referred to as hydrogenated) thermoplastic elastomers can also be used. By using hydrogenated thermoplastic elastomers, reactivity and adhesion are improved, and solubility in the solvent used when forming the solid electrolyte layer 10 is improved.
[0071] The addition amount of the binder is, for example, more than 0.01 mass % and less than 5 mass %, can be more than 0.1 mass % and less than 3 mass %, can also be more than 0.1 mass % and less than 1 mass %. By setting the addition amount of the binder to more than 0.01 mass %, it is easy to combine with the aid of the binder, and it is easy to obtain sufficient adhesion strength. In addition, by setting the addition amount of the binder to less than 5 mass %, it is difficult to cause the reduction of battery characteristics such as charge-discharge characteristics, in addition, for example, in low temperature regions, even if the physical properties such as the hardness, tensile strength, and tensile elongation of the binder change, the charge-discharge characteristics are also difficult to reduce.
[0072] [C. Positive electrode layer]
[0073] Next, the positive electrode layer 20 in this embodiment is described. The positive electrode layer 20 in this embodiment includes a solid electrolyte 1 and a positive electrode active material 2. The positive electrode layer 20 may also contain a conductive additive and a binder such as acetylene black and Ketjen black (registered trademark) to ensure electron conductivity as needed, but if the amount added is large, the battery performance is affected, so it is preferably a small amount that does not affect the battery performance.
[0074] The weight ratio of the positive electrode active material 2 to the solid electrolyte 1 is, for example, in the range of 50:50 to 95:5, or may be in the range of 70:30 to 90:10.
[0075] The volume ratio of the positive electrode active material 2 to the solid electrolyte 1 is, for example, in the range of 60:40 to 90:10, or 70:30 to 85:15. This volume ratio makes it easy to ensure both the lithium ion conduction path and the electron conduction path in the positive electrode layer 20.
[0076] The positive electrode current collector 7 is made of, for example, a metal foil. As the metal foil, for example, a metal foil of SUS, aluminum, nickel, titanium, copper, or the like is used.
[0077] [C-1. Solid electrolyte]
[0078] The solid electrolyte material used in the solid electrolyte 1 is, for example, at least one of the solid electrolyte materials listed in [B-1. Solid electrolyte] above. In addition, there is no particular limitation on the selection of materials. For example, a combination of materials is selected within the range where the interface between the positive electrode active material 2 and the solid electrolyte 1 and the interface between the solid electrolyte 1 and the solid electrolyte 5 do not significantly impair the lithium ion conductivity. The solid electrolyte 1 is, for example, composed of a plurality of particles.
[0079] [C-2. Binder]
[0080] Since it is the same as the above-mentioned adhesive, it is omitted.
[0081] [C-3. Positive electrode active material]
[0082] The positive electrode active material 2 in this embodiment is described. As the material of the positive electrode active material 2 in this embodiment, for example, a lithium-containing transition metal oxide is used. Examples of lithium-containing transition metal oxides include LiCoO 2 、LiNiO 2 、LiMn 2 O 4 、LiCoPO 4 、LiNiPO 4 、LiFePO 4 、LiMnPO 4 , compounds obtained by replacing the transition metals of these compounds with one or two different elements, etc. As compounds obtained by replacing the transition metals of the above compounds with one or two different elements, LiNi is used. 1 / 3 Co 1 / 3 Mn 1 / 3 O 2 、LiNi 0.8 Co 0.15 Al 0.05 O 2 、LiNi 0.5 Mn 1.5 O 2 The material of the positive electrode active material 2 may be used alone or in combination of two or more.
[0083] The positive electrode active material 2 is composed of a plurality of particles. Each particle of the positive electrode active material 2 is a granulated particle in which a plurality of primary particles containing the above-mentioned material are gathered. In this specification, the granulated particles are referred to as particles of the positive electrode active material 2.
[0084] The average particle size of the positive electrode active material 2 is not particularly limited, and is, for example, 1 μm to 10 μm. The particle size distribution of the positive electrode active material 2 is, for example, a distribution in which 80% or more of all particles exist within a particle size range of ±30% relative to the average particle size.
[0085] [D. Negative electrode layer]
[0086] Next, the negative electrode layer 30 in the present embodiment is described. The negative electrode layer 30 in the present embodiment includes a solid electrolyte 4 and a negative electrode active material 3. The negative electrode layer 30 may further include a conductive additive and a binder such as acetylene black and ketjen black to ensure electronic conductivity as needed, but if the amount added is large, the battery performance will be affected, so it is preferably a small amount that does not affect the battery performance. Regarding the ratio of the negative electrode active material 3 to the solid electrolyte 4, for example, in terms of weight conversion, the negative electrode active material: solid electrolyte is in the range of 95:5 to 40:60, and may be in the range of 70:30 to 50:50. In addition, regarding the ratio of the negative electrode active material 3 to the solid electrolyte 4, for example, in terms of volume conversion, the negative electrode active material: solid electrolyte is in the range of 96:4 to 46:54, and may be in the range of 75:25 to 56:44. In other words, the volume ratio of the negative electrode active material 3 to the total volume of the negative electrode active material 3 and the solid electrolyte 4 is, for example, 46% or more and 96% or less, and may be 56% or more and 75% or less. By setting the volume ratio to this value, it is easy to ensure both the lithium ion conduction path performed by the solid electrolyte 4 and the electron conduction path performed by the negative electrode active material 3 in the negative electrode layer 30 .
[0087] The negative electrode current collector 8 is made of, for example, metal foil. As the metal foil, for example, a metal foil of SUS, copper, nickel, or the like is used.
[0088] [D-1. Solid electrolyte]
[0089] The solid electrolyte material used in the solid electrolyte 4 is not particularly limited, and for example, at least one of the solid electrolyte materials listed in [B-1. Solid electrolyte] may be selected arbitrarily. From the viewpoint of facilitating the formation of the coating layer 13 described later, the solid electrolyte material used in the solid electrolyte 4 may be a sulfide-based solid electrolyte or a halide-based solid electrolyte. The solid electrolyte 4 is composed of, for example, a plurality of particles.
[0090] [D-2. Binder]
[0091] Since it is the same as the above-mentioned adhesive, it is omitted.
[0092] [D-3. Negative electrode active material]
[0093] The negative electrode active material 3 in the present embodiment is described. As the material of the negative electrode active material 3 in the present embodiment, a carbon material (active material particles) in which a plurality of small graphite pieces are granulated in a stacked state is used. That is, the negative electrode active material 3 contains a plurality of granulated active material particles. As the granulated active material particles, known materials and granulation methods are used. The granulated active material particles are, for example, non-spherical shapes having a major axis direction and a minor axis direction. The details will be described later, and the granulated active material particles are pressed into flat active material particles during the manufacturing process of the all-solid-state battery 100.
[0094] In addition, the negative electrode active material 3 may further contain SiO x , lithium, indium, tin, silicon and other known materials of negative electrode active materials.
[0095] In addition, the average particle size of the granulated active material particles is not particularly limited, and is, for example, 1 μm or more and 15 μm or less. Here, the particle size refers to the maximum Feret diameter obtained by finding the maximum value of the length of the side of a rectangle circumscribing each active material particle when drawing a rectangle circumscribing each active material particle in a top view image of each active material particle. In addition, the average particle size refers to the number average particle size obtained by finding the number average of the particle sizes found by the above method.
[0096] <Method for manufacturing all-solid-state batteries>
[0097] Next, use Figure 2 A method for manufacturing the all-solid-state battery 100 in the present embodiment will be described. Specifically, a method for manufacturing the all-solid-state battery 100 including the solid electrolyte layer 10 , the positive electrode layer 20 , and the negative electrode layer 30 will be described. Figure 2 It is a schematic cross-sectional view for explaining a method for manufacturing the all-solid-state battery 100 .
[0098] The manufacturing method of the all-solid-state battery 100 includes, for example, a negative electrode layer film forming step, a positive electrode layer film forming step, a solid electrolyte layer film forming step, a lamination step, and a pressing step. The negative electrode layer film forming step is an example of a manufacturing step of the negative electrode layer 30. In the negative electrode layer film forming step ( Figure 2 In (a)), the negative electrode layer 30 is formed on the negative electrode current collector 8. In the positive electrode layer film forming step ( Figure 2 In (b)), the positive electrode layer 20 is formed on the positive electrode current collector 7. In the solid electrolyte layer film forming step ( Figure 2 In (c) and (d)), the solid electrolyte layer 10 is prepared. Figure 2In (e) and (f)), the positive electrode layer 20 formed on the positive electrode collector 7, the negative electrode layer 30 formed on the negative electrode collector 8, and the prepared solid electrolyte layer 10 are stacked together in a manner such that the solid electrolyte layer 10 is arranged between the positive electrode layer 20 and the negative electrode layer 30, and pressed from the outside of the positive electrode collector 7 and the negative electrode collector 8. The details of each step are described below.
[0099] [E. Negative Electrode Layer Film Forming Step]
[0100] As the film forming step of the negative electrode layer 30 (negative electrode layer film forming step) in the present embodiment, for example, there are two methods: the following method (1) and method (2).
[0101] (1) As a film-forming method for the negative electrode layer 30 in the present embodiment, for example, a method of manufacturing by a film-forming process including a mixture preparation process, a coating process and a coating pressing process can be cited. Specifically, in the mixture preparation process, for example, the negative electrode active material 3 and the solid electrolyte 4 are subjected to preliminary preparations of stirring and mixing as described in detail below, and the obtained mixed powder is dispersed in an organic solvent, and further, as needed, a binder and a conductive aid (not shown) are dispersed in the organic solvent to prepare a slurry-formed negative electrode mixture. Then, in the coating process, the obtained negative electrode mixture is applied to the surface of the negative electrode collector 8, and the organic solvent is removed by heating and drying the obtained coating, and then drying and / or firing is performed. Next, in the coating pressing process, the dried coating formed on the negative electrode collector 8 is pressed. The negative electrode layer 30 is manufactured by such a film-forming process.
[0102] The coating method of the slurry is not particularly limited, and examples thereof include a knife coater, a gravure coater, a dip coater, a reverse coater, a roll knife coater, a wire bar coater, a slot die coater, an air knife coater, a curtain coater, an extrusion coater, or a known coating method such as a combination thereof.
[0103] Examples of the organic solvent used for slurry formation include heptane, xylene, toluene, etc., but the invention is not limited thereto, and a solvent that does not chemically react with the negative electrode active material 3 and the solid electrolyte 4 may be appropriately selected.
[0104] In the drying and / or calcining, there is no particular limitation as long as the coating can be formed and the organic solvent can be removed, and a known drying method or calcining method using a heater etc. can be adopted. There is no particular limitation on the pressing method in the coating pressing step, and a known pressing method using a press etc. can be adopted.
[0105] (2) In addition, as other methods for forming the film of the negative electrode layer 30 in the present embodiment, for example, a method of manufacturing by a film forming process including a mixture preparation process, a powder stacking process and a powder pressing process can be cited. In the mixture preparation process, a powdered (unslurried) negative electrode active material 3 and a solid electrolyte 4 are prepared, and a binder and a conductive aid (not shown) are further prepared as needed. The prepared materials are stirred and mixed while applying appropriate compression and shear forces to prepare a negative electrode mixture in which the negative electrode active material 3 and the solid electrolyte 4 are uniformly dispersed. The details of the stirring and mixing will be described later. In the powder stacking process, the obtained powdered negative electrode mixture is uniformly stacked on the negative electrode collector 8 using, for example, a scraper to obtain a stacked body. In the powder pressing process, the stacked body obtained in the powder stacking process is pressed to form a film.
[0106] When manufactured in the form of a negative electrode mixture in a stacked powder state, there is an advantage that a drying process is not required and the manufacturing cost is reduced. In addition, no solvent that affects the battery performance of the all-solid-state battery 100 will remain in the negative electrode layer 30 after film formation. For example, the material will not deteriorate due to the residual solvent during the charge and discharge of the all-solid-state battery 100, so the reduction in battery characteristics can be suppressed. In addition, in the manufacturing process, since there is no solvent, the material degradation caused by the solvent will not occur. Therefore, the battery performance can be improved. In the case of manufacturing the all-solid-state battery 100 in the form of a negative electrode mixture in a stacked powder state, for example, the concentration of the solvent contained in the negative electrode layer 30 is less than 50 ppm, and the negative electrode layer 30 does not substantially contain a solvent component.
[0107] Here, in the above-mentioned methods (1) and (2), as a preparation for film formation, a mixing step of stirring and mixing the negative electrode active material 3 and the solid electrolyte 4 in a dry process is important. Here, stirring and mixing means a method of mixing while applying compression force and shear force when mixing the negative electrode active material 3 and the solid electrolyte 4, and there is no special limitation. In addition, the purpose of the mixing step of stirring and mixing is to form a coating formed by densely compacting the particles constituting the solid electrolyte 4 on a part of the surface of the negative electrode active material 3. In particular, the shape of the granulated active material particles contained in the negative electrode active material 3 is not a perfect spherical shape, and the granulated active material particles have a long direction (i.e., the major axis direction) and a short direction (i.e., the minor axis direction) of the length of the particle shape. It is preferred to intentionally form a large amount of the above-mentioned coating near the front end of the major axis direction of the granulated active material particles.
[0108] Hereinafter, in the stage of manufacturing the all-solid-state battery, this densely compacted coating film is referred to as a coating layer 13 .
[0109] The specific mixing procedure will be described later.
[0110] [F. Positive Electrode Layer Film Forming Step]
[0111] The film forming step of the positive electrode layer 20 (positive electrode layer film forming step) of this embodiment is basically the same as the film forming step of the negative electrode layer 30 described in the above [E. Negative electrode layer film forming step] except that the material used is changed to that for the positive electrode layer 20 .
[0112] The manufacturing method of the positive electrode layer 20 may be, for example, a method in which a positive electrode mixture obtained by mixing and slurrying a solid electrolyte 1, a positive electrode active material 2, and a binder and a conductive aid (not shown) as required is applied to a positive electrode collector 7 and then dried (i.e., the same method as method (1) in [E. Negative electrode layer film forming process]). In addition, the manufacturing method of the positive electrode layer 20 may be, for example, a method in which a non-slurried powdered positive electrode mixture is layered on a positive electrode collector 7 (i.e., the same method as method (2) in [E. Negative electrode layer film forming process]). In addition, in the film forming process of the positive electrode layer 20, a mixing process of stirring and mixing may be performed, or a mixing process of stirring and mixing may not be performed.
[0113] In the case of manufacturing by stacking a powdered positive electrode mixture, there is an advantage that a drying step is not required, the manufacturing cost is reduced, and in addition, no solvent that contributes to the capacity of the all-solid-state battery remains in the positive electrode layer 20 after film formation. That is, the same effect as the case of manufacturing the above-mentioned negative electrode layer 30 by method (2) can be obtained.
[0114] [G. Solid Electrolyte Layer Film Forming Step]
[0115] The solid electrolyte layer 10 in this embodiment can be prepared by the same method as in the above-mentioned [E. Negative electrode layer film forming step], except that the solid electrolyte 5 and the binder as required are dispersed in an organic solvent to prepare a slurry, and the obtained slurry is applied to the positive electrode layer 20 and / or the negative electrode layer 30 prepared above. In addition, the material of the solid electrolyte layer 10 in a powder state can also be used for film formation in the same manner as in method (2).
[0116] exist Figure 2 In the examples shown in (c) and (d), the solid electrolyte layer 10 is formed on the positive electrode layer 20 and the negative electrode layer 30, but it is not limited thereto, and the solid electrolyte layer 10 may be formed on either the positive electrode layer 20 or the negative electrode layer 30. In addition, the solid electrolyte layer 10 may be produced by the above method on a substrate such as a polyethylene terephthalate (PET) film, and the obtained solid electrolyte layer 10 may be stacked on the positive electrode layer 20 and / or the negative electrode layer 30.
[0117] [H. Lamination process and pressing process]
[0118] In the stacking process and the pressing process, the positive electrode layer 20 formed on the positive electrode collector 7, the negative electrode layer 30 formed on the negative electrode collector 8 and the solid electrolyte layer 10 obtained by each film forming process are stacked in a manner such that the solid electrolyte layer 10 is arranged between the positive electrode layer 20 and the negative electrode layer 30 (stacking process), and then pressed from the outside of the positive electrode collector 7 and the negative electrode collector 8 (pressing process) to obtain an all-solid-state battery 100.
[0119] The purpose of pressing is to increase the density of the positive electrode layer 20, the negative electrode layer 30 and the solid electrolyte layer 10. By increasing the density, the lithium ion conductivity and the electron conductivity in the positive electrode layer 20, the negative electrode layer 30 and the solid electrolyte layer 10 can be improved, and an all-solid-state battery 100 with good battery characteristics can be obtained.
[0120] <Method for producing negative electrode layer>
[0121] Below, a detailed example of a method for manufacturing the negative electrode layer 30 of the all-solid-state battery 100 of the present embodiment is described, but it is not limited to these examples of manufacturing methods. It should be noted that, unless otherwise specified, each process is performed in a glove box or a drying room where the dew point is managed to be below -45°C. In addition, below, a method for manufacturing the negative electrode layer 30 using the above-mentioned method (2) is described, but the same negative electrode layer 30 can also be manufactured when using method (1).
[0122] First, the materials used in the negative electrode layer 30 will be described. In the manufacture of the negative electrode layer 30, for example, a negative electrode mixture including a negative electrode active material 3 and a solid electrolyte 4 is used.
[0123] The material of the negative electrode active material 3 is selected from the materials listed in [D-3. Negative electrode active material] in the configuration of the all-solid-state battery in the present embodiment. The material of the solid electrolyte 4 is selected from the materials listed in [B-1. Solid electrolyte].
[0124] In addition, the size of the material used is described in detail. For example, the negative electrode active material 3 uses a material with an average particle size of 8.0 μm, and more than 80% of the total particles fall within the range of ±30% of the average particle size. In addition, the solid electrolyte 4 uses a particulate material with an average particle size of 0.5 μm or more and 1.0 μm or less.
[0125] Here, the amount of solid electrolyte 4 added is appropriately selected within the range of the overall mixing ratio of negative electrode active material 3 and solid electrolyte 4 , and the mixing ratio of negative electrode active material 3 and solid electrolyte 4 is, for example, 75:25 to 56:44 in volume ratio and 70:30 to 50:50 in weight ratio.
[0126] In the manufacture of the negative electrode layer 30, it is important to prepare the negative electrode mixture through a mixing step of stirring and mixing as described above. Thus, in the process of manufacturing the negative electrode layer 30 finally formed, when the active material particles of the negative electrode active material 3 present in the negative electrode layer 30 are flat active material particles, a plurality of adjacent flat active material particles can be formed in which the angle formed by the long axis direction of the flat active material particles with respect to the thickness direction of the negative electrode layer 30 is within a range of 0° or more and 30° or less.
[0127] The method for producing the negative electrode layer 30 , such as the mixing step in preparing the negative electrode mixture, will be described in detail below while comparing the embodiment and the comparative example.
[0128] (I) Method for producing negative electrode layer in embodiment
[0129] First, a method for producing a negative electrode layer in the embodiment will be described. Figure 3 This is a flowchart showing a method for producing a negative electrode mixture in an embodiment.
[0130] In the manufacture of the negative electrode mixture in the embodiment, as a mixing process, the particles of the negative electrode active material 3 and the particles of the solid electrolyte 4 are stirred and mixed (step S11). In addition, in the mixing process, a negative electrode active material 3 containing a plurality of active material particles of a non-spherical shape is used. Here, stirring and mixing refers to mixing while applying compression and shearing forces to the materials. For example, the negative electrode active material 3 and the solid electrolyte 4 are put into a stirring and mixing device, and they are stirred and mixed by the stirring and mixing device. As a stirring and mixing device, for example, a device is used in which a rotating blade for stirring and mixing is provided in a container in which materials are put. For example, a prescribed space is provided between the inner wall of the container of the stirring and mixing device and the rotating blade, and compression and shearing forces are applied to the materials in the space by the rotation of the rotating blade. Stirring and mixing is not limited to stirring and mixing using such a stirring and mixing device, as long as it is mixing in which compression and shearing forces are applied to the mixed materials.
[0131] By stirring and mixing the negative electrode active material 3 and the solid electrolyte 4, a dense coating layer 13 composed of the solid electrolyte 4 can be formed at the end of the granulated active material particles in the long axis direction of the negative electrode active material 3. The details of the coating layer 13 will be described later. Through such a mixing step, a negative electrode mixture containing active material particles of the negative electrode active material 3 with the coating layer 13 formed on the surface can be obtained.
[0132] Next, the negative electrode mixture thus prepared is used to form the negative electrode layer 30 by, for example, the method described in the method (2) of the above-mentioned [E. Negative electrode layer film forming step]. In addition, the all-solid-state battery 100 in the embodiment is manufactured by the above-mentioned method using the negative electrode layer 30. Here, in the manufacturing process, there are no particular limitations except for the mixing step of the negative electrode mixture.
[0133] (II) Method for producing negative electrode layer in comparative example
[0134] Next, a method for producing the negative electrode layer 30 in the comparative example will be described. Figure 4 This is a flow chart showing a method for producing a negative electrode mixture in a comparative example.
[0135] In the manufacturing method of the negative electrode mixture of the comparative example, the particles of the negative electrode active material 3 and the particles of the solid electrolyte 4 are mixed (step S51). In the mixing in step S51, it is different from step S11 in that the compression force and the shear force are not substantially applied to the negative electrode active material 3 and the solid electrolyte 4. Thus, the negative electrode mixture is obtained. In the negative electrode mixture of the comparative example, since the materials of the negative electrode mixture are not stirred and mixed, the coating layer 13 is not formed on the surface of the active material particles of the negative electrode active material 3.
[0136] Next, the negative electrode mixture thus prepared is used to form a negative electrode layer 30, for example, by the method described in the method (2) of the above [E. Negative electrode layer film forming step]. In addition, the all-solid-state battery in the comparative example is manufactured by the above method using the negative electrode layer 30. Here, in the manufacturing process, there are no particular limitations except for the mixing step of the negative electrode mixture.
[0137] (III) Structure of Negative Electrode Mixture and Negative Electrode Layer
[0138] Next, the structure of the negative electrode mixture in the embodiment and the comparative example and the negative electrode layer 30 formed using the negative electrode mixture will be described. Figure 5 and Figure 6 The change in the state of the negative electrode active material 3 and the solid electrolyte 4 including active material particles having a non-perfect spherical shape in the major axis direction and the minor axis direction will be described. Figure 5 It is a schematic diagram for explaining the change in the state of the negative electrode active material 3 and the solid electrolyte 4 in the comparative example. Figure 6 Schematic diagram for explaining the change in the state of the negative electrode active material 3 and the solid electrolyte 4 in the embodiment. Figure 5 (a) and Figure 6 (a) are schematic diagrams showing the range of several particle amounts of the negative electrode active material 3 in the negative electrode mixture before the powder pressing step and after mixing or stirring. Figure 5 (b) and Figure 6(b) are Figure 5 (a) and Figure 6 (a) is a schematic diagram of the negative electrode mixture during the pressing process in the powder pressing step. Figure 5 (c) and Figure 6 (c) are schematic diagrams showing the state of the negative electrode active material 3 in the negative electrode layer 30 after the powder pressing step.
[0139] In the negative electrode mixture of the comparative example, Figure 5 As shown in (a), the active material particles of the negative electrode active material 3 and the particles of the solid electrolyte 4 having the long axis direction and the short axis direction exist in a uniformly dispersed state. Here, the particle size of the solid electrolyte 4 is smaller than the particle size of the negative electrode active material 3, so the solid electrolyte 4 (for example, Figure 5 The particles within the dotted line portion 24 in (a) are stacked in a state with a low stacking density, that is, a state with a large amount of space.
[0140] Next, during the pressing process in the powder pressing step, the space between the solid electrolyte 4 particles in the dotted line portion 24 is compressed while the negative electrode layer 30 is pressed in the thickness direction. Figure 5 As shown in (b), when pressurized, the solid electrolyte 4 in the dotted line portion 24 cannot support the negative electrode active material 3, and the active material particles of the negative electrode active material 3 are Figure 5 The negative electrode layer 30 is tilted laterally, that is, greatly tilted relative to the thickness direction of the negative electrode layer 30, while being pressed. As a result, Figure 5 As shown in (c), the negative electrode layer 30 is pressurized in a state of being inverted in the plane direction (direction perpendicular to the thickness direction of the negative electrode layer 30). In addition, by pressurizing, the non-spherical active material particles are compressed in the short axis direction of the active material particles and deformed into a flat shape, thereby becoming flat active material particles.
[0141] In contrast, in the negative electrode mixture according to the embodiment, Figure 6 As shown in (a), a coating layer 13 formed by compacting the particles of the solid electrolyte 4 is formed on at least a portion of the surface of the active material particles of the negative electrode active material 3, especially near the ends of two or more adjacent active material particles in the long axis direction. The solid electrolyte 4 (for example, Figure 6 The particles (in the dotted line portion 25) in (a) are stacked in a state with a high stacking density, that is, with less space.
[0142] Next, if Figure 6As shown in (b), during the pressing process in the powder pressing step, the coating layers 13 support each other, and even if the negative electrode layer 30 is pressed in the thickness direction, the active material particles of the negative electrode active material 3 are prevented from tilting and falling with respect to the thickness direction of the negative electrode layer 30. Figure 6 As shown in (c), in the negative electrode layer 30 finally formed after the powder pressing step, the active material particles of the negative electrode active material 3 are not easy to fall over. As a result, the flat active material particles formed by compressing the active material particles in the short axis direction are arranged in a form in which the long axis direction of the flat active material particles is oriented in the longitudinal direction (the thickness direction of the negative electrode layer 30).
[0143] Here, use Figure 7 and Figure 8 The observation results of the negative electrode mixture and the negative electrode layer actually produced by the above-mentioned method will be described. Figure 7 : is an electron microscope image showing the appearance of the negative electrode mixture in the embodiment. Figure 7 Shown in Figure 6 The observation results of the negative electrode mixture in the state shown in (a). Figure 8 FIG. 1 is an electron microscope image showing a cross section of the negative electrode layer 30 in the embodiment. Figure 8 It is shown that the Figure 7 The cross section of the negative electrode layer 30 formed by the negative electrode mixture shown in FIG. Figure 7 and Figure 8 In the example, the use of Figure 6 The states of the negative electrode active material 3 and the solid electrolyte 4 are described.
[0144] like Figure 7 As shown, it can be seen that by the method for manufacturing the negative electrode mixture in this embodiment, a coating layer 13 in which the particles of the solid electrolyte 4 are compressed and densified is formed on the surface of the negative electrode active material 3. In addition, a part of the solid electrolyte 4 exists in the state of particles without densification, but it can also be used in a manner that can play a role. Figure 6 The effect described in the above is present within the scope. Figure 8 As shown in FIG. 1 , it can be seen that by using the negative electrode mixture produced by the manufacturing method in this embodiment, an active material orientation region 14 is formed in the negative electrode layer 30, where two or more flat active material particles of the negative electrode active material are arranged adjacent to each other in the main surface direction of the negative electrode layer 30. In addition, in the active material orientation region 14, the angles formed by the major axis directions of the two or more flat active material particles of the negative electrode active material with respect to the thickness direction of the negative electrode layer 30 are 0° or more and 30° or less. In addition, as shown in FIG. Figure 8 As shown, the negative electrode layer 30 may have a plurality of active material orientation regions 14 .
[0145] In addition, the negative electrode layer 30 has a solid electrolyte region 15 adjacent to the active material orientation region 14 and containing a solid electrolyte 4 but not containing a negative electrode active material 3 in the negative electrode layer cross section. That is, a solid electrolyte region 15 in which no negative electrode active material 3 is present is formed in the negative electrode layer 30. The solid electrolyte 4 of the solid electrolyte region 15 comes from the coating layer 13, for example. Here, in any negative electrode layer cross section of the negative electrode layer 30, the area occupied by the solid electrolyte region 15 is, for example, 1.5 times or more of the average value of the area occupied by each of two or more flat active material particles of the negative electrode active material 3 in the active material orientation region 14, and may be 2.0 times or more. It should be noted that the solid electrolyte region 15 may not be formed in the negative electrode layer 30.
[0146] Next, the intentional production Figure 6 (a) and Figure 7 The negative electrode mixture described in the above description is a structure in which a coating layer 13 formed by compacting particles of a solid electrolyte 4 is formed on at least a portion of the surface of the active material particles of the negative electrode active material 3, especially near the end of the active material particles in the long axis direction. Specifically, using Fig. 9 right Figure 3 The state of the mixing process of the negative electrode active material 3 and the solid electrolyte 4 during the stirring and mixing shown will be described. Fig. 9 It is a schematic diagram for explaining the change in the state of the negative electrode active material 3 and the solid electrolyte 4 in the mixing step in the embodiment.
[0147] like Fig. 9 As shown in (a), the negative electrode active material 3 and the solid electrolyte 4 are prepared, and stirring and mixing are started while applying compression and shearing forces. When stirring and mixing are started, Fig. 9 As shown in (b), the solid electrolyte 4 present near the end 16 of the active material particle in the long axis direction of the negative electrode active material 3 is compressed and sheared between the active material particles of the adjacent negative electrode active material 3 and flattened to form a coating layer 13. Next, as Fig. 9 As shown in (c), since the material is stirred as a whole, the active material particles of the negative electrode active material 3 rotate, and the axis in the long axis direction is offset, so that the compression and shear force applied to the end 16 disappears sharply, and the densified coating layer 13 from the solid electrolyte 4 is fixed near the end 16. This can be dealt with by adjusting the factors from the material during stirring and mixing (particle size, material and shape, etc.) and process conditions (amount of input material, method of applying compression and shear force, temperature, etc.). It should be noted that, except for forming a densified coating layer 13 from the solid electrolyte 4 near the end 16 of the active material particles in the long axis direction of the negative electrode active material 3, the method for making the negative electrode mixture is not particularly limited.
[0148] <Example>
[0149] Next, the results of evaluating the battery characteristics of the all-solid-state battery 100 in the present invention are described using examples, but the present invention is not limited to the examples. Specifically, all-solid-state batteries in Example 1 and Comparative Example 1 were manufactured, and the battery characteristics of the manufactured all-solid-state batteries were evaluated.
[0150] [Production of all-solid-state batteries]
[0151] (I) Embodiment 1
[0152] The negative electrode layer 30 was formed by the method described in the above-mentioned "(I) Method for producing the negative electrode layer in the embodiment". At this time, the mixing ratio of the negative electrode active material 3 and the solid electrolyte 4 was 70:30 in terms of volume ratio.
[0153] Then, the all-solid-state battery 100 in Example 1 was manufactured through the positive electrode layer forming step, solid electrolyte layer forming step, lamination step, and pressing step described in the above-mentioned <Method for Manufacturing All-Solid-State Battery>.
[0154] (II) Comparative Example 1
[0155] The all-solid-state battery in Comparative Example 1 was manufactured by the same method as the all-solid-state battery in Example 1, except that the negative electrode layer was formed by the method described in the above “(II) Method for preparing the negative electrode layer in Comparative Example”. At this time, the mixing ratio of the negative electrode active material 3 and the solid electrolyte 4 was 70:30 by volume ratio.
[0156] [Evaluation of battery capacity]
[0157] Next, the battery characteristics of the all-solid-state batteries in Example 1 and Comparative Example 1 prepared above are evaluated. Specifically, as a battery characteristic that becomes an indicator of battery capacity, the results of evaluating the charge and discharge efficiency are shown in Table 1. In the evaluation of the charge and discharge efficiency, two conditions of low-rate discharge and high-rate discharge are implemented. In addition, in the evaluation of the charge and discharge efficiency, charging is implemented under the conditions of a termination voltage of 3.7V, a current rate of 0.05C, and a temperature of 25°C. In addition, discharging is implemented under the conditions of a termination voltage of 1.9V, a charging rate of 0.05C at a low rate, a charging rate of 1C at a high rate, and a temperature of 25°C. In addition, in the evaluation of the charge and discharge efficiency, from the start of charging, the ratio (%) of the discharge capacity to the charging capacity is calculated as the charge and discharge efficiency.
[0158] [Table 1]
[0159] Comparative Example 1 Example 1 Charge and discharge efficiency in low rate discharge 99% 99% Charge and discharge efficiency during high rate discharge 33% 64%
[0160] As shown in Table 1, it can be seen that the all-solid-state battery 100 in Example 1 has improved charge and discharge efficiency compared with the all-solid-state battery in Comparative Example 1. In Example 1, the charge and discharge efficiency in high-rate discharge is improved compared with Comparative Example 1. It is believed that this shows that the all-solid-state battery 100 is manufactured by intentionally forming a coating layer 13 near the end 16 of the active material particles in the long axis direction of the negative electrode active material 3, thereby improving the battery characteristics. Specifically, it is believed that this is because the conduction of lithium ions in the thickness direction of the negative electrode layer 30 is hindered by the flat active material particles in the state where the long axis direction of the flat active material particles in the negative electrode layer 30 is greatly tilted (that is, toward the direction along the main surface direction). In the all-solid-state battery 100 in the embodiment, by forming an active material orientation region 14 in which two or more flat active material particles of the negative electrode active material 3 are oriented in a manner along the thickness direction of the negative electrode layer 30, it is easy to ensure the conduction path of lithium ions in the thickness direction of the negative electrode layer 30 even at a high rate of discharge.
[0161] In addition, by the presence of the active material orientation region 14 in which the long axis direction of the flat active material particles is not greatly tilted in the negative electrode layer 30, the stress caused by the expansion and contraction of the negative electrode active material 3 caused by charging and discharging can also be dispersed in the direction intersecting the thickness direction of the negative electrode layer 30, and the effect of improving durability can be expected. In addition, in the negative electrode layer 30, by the presence of the solid electrolyte region 15 composed of the solid electrolyte 4 from the coating layer 13 and without the negative electrode active material 3, the effect of further relaxing the stress by the solid electrolyte 4 that is softer than the negative electrode active material 3 can be expected. By relaxing the stress in this way, the peeling at the interface between the negative electrode active material 3 and the solid electrolyte 4 and the peeling at the interface between the negative electrode layer 30 and the solid electrolyte layer 10 can be suppressed, and the reduction of the battery capacity can be suppressed.
[0162] In the present embodiment, as described above, the volume ratio of the negative electrode active material 3 in the negative electrode layer 30 relative to the total volume of the negative electrode active material 3 and the solid electrolyte 4 is, for example, 46% or more and 96% or less. By setting the volume ratio of the negative electrode active material 3 to be such, it is easy to obtain the effect described using the above embodiment. Specifically, by making the above volume ratio less than 96%, the coating layer 13 formed toward the end 16 of the active material particles of the negative electrode active material 3 becomes more, and the active material orientation region 14 in the negative electrode layer 30 can be increased. In addition, by making the above volume ratio more than 46%, the capacity of the battery can be further increased. In addition, from the viewpoint of further increasing the capacity of the battery during high-rate charge and discharge, the above volume ratio can be 56% or more and 75% or less.
[0163] (Other embodiments)
[0164] The all-solid-state battery of the present invention is described above based on the embodiments, but the present invention is not limited to these embodiments. As long as it does not depart from the main purpose of the present invention, various deformation methods that a person skilled in the art thinks of are implemented on the embodiments, and other methods constructed by combining some of the constituent elements in the embodiments are also included in the scope of the present invention.
[0165] For example, in the above embodiment, the example in which the ions conducted in the all-solid-state battery 100 are lithium ions is described, but the present invention is not limited thereto. The ions conducted in the all-solid-state battery 100 may be ions other than lithium ions, such as sodium ions, magnesium ions, potassium ions, calcium ions, or copper ions.
[0166] According to the all-solid-state battery and the like of one embodiment of the present invention, it is possible to suppress a decrease in the battery capacity of the all-solid-state battery.
[0167] Industrial Applicability
[0168] The all-solid-state battery of the present invention is expected to be used in various batteries such as power sources for portable electronic devices and batteries for vehicles.
[0169] Description of Reference Numerals
[0170] 1, 4, 5: Solid electrolyte
[0171] 2: Positive electrode active material
[0172] 3: Negative electrode active material
[0173] 7: Positive electrode collector
[0174] 8: Negative electrode collector
[0175] 10: Solid electrolyte layer
[0176] 13: Coating layer
[0177] 14: Active material orientation area
[0178] 15: Solid electrolyte area
[0179] 16: End
[0180] 20: Positive electrode layer
[0181] 30: Negative electrode layer
[0182] 100: All-solid-state battery
Claims
1. An all-solid-state battery comprising a positive electrode collector, a positive electrode layer including a positive electrode active material and a first solid electrolyte, a solid electrolyte layer including a third solid electrolyte, A negative electrode layer including a negative electrode active material and a second solid electrolyte, and The negative electrode current collector is stacked in layers. The negative electrode active material includes a plurality of flat active material particles, and the flat active material particles have a structure in which a plurality of graphite flakes are stacked. The negative electrode layer has an active material orientation region in which two or more of the plurality of flat active material particles are arranged adjacent to each other in a cross section of the negative electrode layer cut along a thickness direction of the negative electrode layer. In the cross section, an angle formed by the major axis directions of the two or more flat active material particles with respect to the thickness direction of the negative electrode layer is 0° or more and 30° or less.
2. The all-solid-state battery according to claim 1, wherein: The negative electrode layer further has a solid electrolyte region in the cross section, The solid electrolyte region is located adjacent to the active material orientation region, has an area that is 1.5 times or more the average area of the two or more flat active material particles, contains the second solid electrolyte and does not contain the negative electrode active material.
3. The all-solid-state battery according to claim 1 or 2, wherein: In the cross section, at least one of the two or more flat active material particles has an aspect ratio, which is a ratio of the length in the major axis direction to the length in the minor axis direction, of 3 times or more.
4. The all-solid-state battery according to any one of claims 1 to 3, wherein In the negative electrode layer, a volume ratio of the negative electrode active material to a total volume of the negative electrode active material and the second solid electrolyte is 46% or more and 96% or less.
5. The all-solid-state battery according to claim 4, wherein: In the negative electrode layer, a volume ratio of the negative electrode active material to a total volume of the negative electrode active material and the second solid electrolyte is 56% or more and 75% or less.
6. The all-solid-state battery according to any one of claims 1 to 5, wherein The concentration of the solvent contained in the negative electrode layer is 50 ppm or less.
7. A method for manufacturing an all-solid-state battery, which is the method for manufacturing an all-solid-state battery according to any one of claims 1 to 6, The negative electrode layer manufacturing process includes a mixing process of the negative electrode active material and the second solid electrolyte. The mixing step uses a negative electrode active material including a plurality of active material particles, wherein the active material particles are non-spherical in shape with a long axis direction and a short axis direction, and are formed by stacking and granulating a plurality of graphite flakes. The mixing step includes forming a covering layer composed of a second solid electrolyte that covers the end portions of two or more active material particles in the longitudinal direction of the plurality of active material particles.
8. The method for manufacturing an all-solid-state battery according to claim 7, wherein: The mixing step is a step of mixing the negative electrode active material and the second solid electrolyte while applying a compressive force and a shearing force to the negative electrode active material and the second solid electrolyte.
Citation Information
Patent Citations
Manufacture of all solid lithium secondary battery
JP1996138724A