Bone repair material manufacturing method and bone repair material

By constructing a bone repair material with a cubic frame structure and a minimal curved surface structure, combined with a shape memory alloy and a selective laser melting process, the problem of difficult reusability and small space implantation of bone implants is solved, achieving high strength and reliability. Regulatory, bone repair effect that adapts to complex needs.

CN118767207AActive Publication Date: 2024-10-15BEIJING INST OF TECH

Patent Information

Application Number
CN202410770933.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-14
Publication Date
2024-10-15
Estimated Expiration
2044-06-14

AI Technical Summary

Technical Problem

Existing bone implants are difficult to reuse and difficult to implant in small spaces, and cannot effectively cope with the complex needs of bone defects.

Method used

Using bone repair materials formed by cellular structure, by constructing a cubic frame structure, using minimal surface structure and shape memory alloy for 3D printing, combined with selective laser melting process, the stiffness and strength of the material can be controlled to achieve the controllability of the material. After implantation, the material is heated to return to its prototype to adapt to the needs of different implanted objects.

Benefits of technology

It achieves high specific strength and reusability of bone repair materials, can be effectively implanted and fused in a small space, improves the fusion effect with the bone, avoids the stress shielding effect, and meets the complex needs of implant adaptation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118767207A_ABST
    Figure CN118767207A_ABST
Patent Text Reader

Abstract

The invention provides a bone repair material manufacturing method and a bone repair material, and relates to the technical field of metamaterials. The bone repair material is formed by a cell element structure, the outline of the cell element structure is a cube, the cube is provided with two opposite surfaces and four side faces arranged between the two surfaces in a surrounding mode, and the cell element structure is formed by a plurality of first beams and second beams; the manufacturing method of the bone repair material comprises the steps that a first cell structure model is constructed, and a first beam and a second beam of a first cell structure are straight rods; forming the first beam and the second beam by using a minimum curved surface structure to obtain a third cell element structure model; performing space array on the third cell element structure model to obtain an array structure model; and manufacturing based on an additive manufacturing process according to the array structure model to obtain the bone repair material. The bone repair material prepared by the manufacturing method of the bone repair material can be effectively matched with a bone implantation object.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of metamaterials, and in particular to a method for manufacturing a bone repair material and a bone repair material. Background Art

[0002] Bone defect is one of the most common injuries in clinical practice, with a high disability rate and strong destructiveness to human health. With the increase of age, human bones inevitably suffer from bone aging, osteoporosis and even necrosis, resulting in bone defects. In addition, due to traffic accidents and orthopedic diseases, a large number of patients also face the problem of bone defects. When the bone defect exceeds the critical threshold, osteoblasts are insufficient to repair it.

[0003] In the related art, bone implants are used to replace damaged or missing bones of patients. Generally, bone implants should have an elastic modulus similar to that of human bones to avoid stress shielding effects, and existing bone implants lack reusability. Summary of the invention

[0004] The purpose of the present invention is to provide a method for manufacturing a bone repair material and a bone repair material to solve the technical problem that bone implants are difficult to reuse.

[0005] In order to achieve the above object, the present invention provides the following technical solutions:

[0006] In a first aspect, the present invention provides a method for manufacturing a bone repair material, wherein the bone repair material is formed by a cell structure, wherein the outline of the cell structure is a cube, wherein the cube has two opposite surfaces and four side surfaces arranged between the two surfaces, and wherein the cell structure is formed by a plurality of first beams and second beams; the manufacturing method comprises:

[0007] Constructing a first cellular structure model, wherein the first beam and the second beam of the first cellular structure are both straight bars;

[0008] The first beam and the second beam are formed by using a minimal surface structure to obtain a third cell structure model;

[0009] Performing spatial arraying on the third cell structure model to obtain an array structure model;

[0010] The array structure model is manufactured using an additive manufacturing process to obtain a bone repair material.

[0011] According to at least one embodiment of the present invention, before the first beam and the second beam are formed using a minimal surface structure to obtain a third cell structure model, the method further includes:

[0012] The first beam and the second beam in the first cellular structure model are replaced by at least a portion of a semicircular arc rod to obtain a second cellular structure model.

[0013] According to at least one embodiment of the present invention, in the second cell structure model, the first beam is a semicircular arc-shaped first beam, and the arc shape of the second beam is a quarter-circular arc shape.

[0014] According to at least one embodiment of the present invention, the first beam and the second beam are formed using a minimal surface structure to obtain a third cell structure model, including:

[0015] The cell structure cube is divided into a plurality of sub-cubes, each of the sub-cubes is filled with a lattice of a minimal surface structure, and the intersection of the lattice in each of the sub-cubes and the first beam and the second beam of the cell structure is obtained by Boolean operation.

[0016] According to at least one embodiment of the present invention, the additive manufacturing process comprises a selective laser melting process.

[0017] According to at least one embodiment of the present invention, the laser power of the selective laser melting process is 130W to 150W, the thickness of the powder layer is 20μm to 40μm, and the hatch scanning interval is 70μm to 90μm.

[0018] According to at least one embodiment of the present invention, the scanning speed of the selective laser melting process is negatively correlated with the austenite transformation peak temperature of the bone repair material.

[0019] According to at least one embodiment of the present invention, the austenite transformation peak temperature of the bone repair material ranges from 36°C to 42°C.

[0020] According to at least one embodiment of the present invention, the shape memory alloy includes one of a copper-based shape memory alloy, an iron-based shape memory alloy, and a nickel-titanium-based shape memory alloy.

[0021] According to at least one embodiment of the present invention, the copper-based shape memory alloy includes one of Cu-Zn, Cu-Zn-Al, Cu-Zn-Sn, Cu-Zn-Si, Cu-Zn-Ga, and Cu-Sn alloys.

[0022] According to at least one embodiment of the present invention, the iron-based shape memory alloy includes one of Fe-Pt, Fe-Mn-Si, Fe-Ni-Co-Ti, Fe-Mn-Al-Ni, and Fe-C-Mn-Si-Cr-Ni alloys.

[0023] According to at least one embodiment of the present invention, the nickel-titanium-based shape memory alloy includes one of Ni-Ti-Cu, Ni-Ti-Co, Ni-Ti-Fe, and Ni-Ti-Nb alloys.

[0024] According to at least one embodiment of the present invention, the stiffness and strength of the bone repair material can be controlled based on changes in ambient temperature.

[0025] According to at least one embodiment of the present invention, when the temperature is raised to 42° C., the recovery rate of the bone repair material under cyclic static compression is at least 98%.

[0026] According to at least one embodiment of the present invention, both the first beam and the second beam are formed by minimal curved surface structures.

[0027] According to at least one embodiment of the present invention, the cross section of the second beam is circular.

[0028] According to at least one embodiment of the present invention, a cellular structure for bone repair, wherein the outline of the cellular structure is a cube, wherein the cube has two opposite surfaces and four side surfaces arranged between the two surfaces, each of the surfaces has a first node located at the center of the surface and four third nodes located at the vertices of the cube, each of the side surfaces has a second node located at the center of the side surface, and the cube further has a fourth node located at the center of the cube;

[0029] The cell structure further includes a plurality of semicircular arc-shaped first beams and circular arc-shaped second beams.

[0030] Each of the side surfaces is formed by two of the first beams, and in the same side surface, the arc tops of the two first beams are connected to the second node, and both ends of each of the first beams are respectively connected to the two third nodes of the same surface;

[0031] Each of the surfaces is formed by two of the first beams, and in the same surface, the arc tops of the two first beams are connected to the first node, and both ends of each of the first beams form the third node respectively;

[0032] Each of the second nodes is connected to the first node via the second beam;

[0033] The second nodes of two adjacent side surfaces are connected by the second beam;

[0034] The first beam and the second beam are both formed by minimal curved surface structures.

[0035] According to at least one embodiment of the present invention, the arc shape of the second beam is a quarter arc shape.

[0036] According to at least one embodiment of the present invention, an arc top of each of the second beams connected between the first node and the second node is close to the fourth node.

[0037] According to at least one embodiment of the present invention, the arc top of each of the second beams connected between the second nodes of two adjacent side surfaces is close to the fourth node.

[0038] According to at least one embodiment of the present invention, both the first beam and the second beam are formed by a Gyroid three-periodic minimal surface structure.

[0039] According to at least one embodiment of the present invention, the outer contour of the unit cell of the Gyroid three-periodic minimal surface structure is located within the sub-cube structure.

[0040] According to at least one embodiment of the present invention, the cross section of the second beam is circular.

[0041] The metamaterial for bone repair of the present invention is formed by a plurality of cell structure arrays, wherein the cell structure is the cell structure described in the first aspect;

[0042] In the two fitted cellular structures, the corresponding two second beams in different cellular structures are arranged in a semicircular shape.

[0043] According to at least one embodiment of the present invention, the stiffness, porosity and pore size of the metamaterial are decoupled.

[0044] According to at least one embodiment of the present invention, the diameter of the second beam and the wall thickness of the Gyroid unit cell are positively correlated with the stiffness of the metamaterial; and / or,

[0045] The size of the Gyroid unit cell is negatively correlated with the stiffness of the metamaterial.

[0046] Among the one or more technical solutions provided in the exemplary embodiments of the present invention, at least one of the following beneficial effects can be achieved.

[0047] The cellular structure in the bone repair material of the exemplary embodiment of the present invention is a cubic frame structure as a whole, including two opposite surfaces and four sides arranged between the two surfaces, each surface and each side is formed by two first beams, and in the same side, the arc tops of the two first beams are connected to the second node (the center point of the surface of the side), and the connecting sections of each first beam are respectively connected to the two third nodes of the same surface; in the same surface, the arc tops of the two first beams are connected to the first node (the center point of the surface), and the two ends of each first beam form a third node (the vertex of the cube), and the cube also has a fourth node (the center point of the cube). Each second node is connected to the first node and the second nodes of the two adjacent sides are connected by a second beam. The cellular structure is arranged in a face-centered cubic shape as a whole, and has the characteristics of high specific strength. Compared with setting the first beam and the second beam as a straight rod structure, setting the first beam as a semicircular arc structure and the second beam as a circular arc structure, the overall stiffness and strength of the cellular structure are further improved.

[0048] Furthermore, the first beam and the second beam are both formed of a minimal surface structure, which is integrated with a macroscopic cellular structure, so that the stiffness, porosity and pore size of the cellular structure are decoupled. Through the controllability of the material, the implant for bone repair can cope with the complex needs of various implant objects to improve the fusion effect with the bone.

[0049] Furthermore, the metamaterial formed by the cellular structure is produced by 3D printing of shape memory alloy, and the phase change temperature of the shape memory alloy is controlled at a preset temperature. The bone repair material is compressed and shaped before implantation, and the structure is pre-programmed. After implantation, the temperature is increased using heating technology without damaging the human body, so that the structure returns to its original shape, thereby allowing the bone repair material to be implanted in a small space. BRIEF DESCRIPTION OF THE DRAWINGS

[0050] The accompanying drawings illustrate exemplary embodiments of the present invention and together with the description serve to explain the principles of the present invention, and these drawings are included to provide a further understanding of the present invention and are incorporated in and constitute a part of this specification;

[0051] Figure 1 is an axonometric structural schematic diagram of a cell structure according to an embodiment of the present invention;

[0052] Figure 2 is a schematic diagram of the main structure of a cell structure according to an embodiment of the present invention;

[0053] Figure 3 is a schematic diagram of the design principle of a cell structure according to an embodiment of the present invention;

[0054] Figure 4is a stress-strain curve before and after macro-scale optimization of the cell structure according to an embodiment of the present invention;

[0055] Figure 5 is a stress-strain curve of a metamaterial with different rod diameters according to an embodiment of the present invention;

[0056] Figure 6 is a stress-strain curve of a metamaterial with different wall thicknesses according to an embodiment of the present invention;

[0057] Figure 7 is a stress-strain curve of a metamaterial with different microscopic cell sizes according to an embodiment of the present invention;

[0058] Figure 8 is the stiffness value of the metamaterial with different geometric parameters according to the embodiment of the present invention;

[0059] Fig. 9 is a CCK-8 count diagram of human bone marrow mesenchymal stem cells under different extraction liquid volume fractions of the metamaterial according to an embodiment of the present invention;

[0060] Fig.10 is a graph showing the results of an osteoblast alizarin red staining experiment of a metamaterial according to an embodiment of the present invention;

[0061] Fig.11 1 is a graph showing the results of a vascular endothelial cell migration and invasion experiment of a metamaterial according to an embodiment of the present invention, wherein (a) is the migration rate and (b) is the invasion rate;

[0062] Fig.12 is a differential thermal scanning analysis curve of a metamaterial according to an embodiment of the present invention;

[0063] Fig.13 is a metamaterial recovery rate-time curve at 42° C. of a metamaterial according to an embodiment of the present invention;

[0064] Fig.14 is a stress-strain curve under cyclic compression of a metamaterial according to an embodiment of the present invention;

[0065] Fig.15 is a stress-strain curve of a metamaterial at different temperatures according to an embodiment of the present invention;

[0066] Fig.16 : are experimental results of (a) osteogenic gene ALP and (b) RUNX2 gene expression of the metamaterial according to an embodiment of the present invention;

[0067] Fig.17 is a schematic flow chart of a method for manufacturing a bone repair material according to an embodiment of the present invention;

[0068] Fig.18 is a graph showing the results of a vascular endothelial cell scratch test of a bone repair material according to an embodiment of the present invention;

[0069] Fig.19 3 is a diagram showing the experimental results of vascular endothelial cell lumen formation of the bone repair material according to an embodiment of the present invention.

[0070] Reference numerals: 10, surface; 20, side; 31, first node; 32, second node; 33, third node; 34, fourth node; 41, first beam; 42, second beam. DETAILED DESCRIPTION

[0071] In order to make the technical problems, technical solutions and beneficial effects to be solved by the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention.

[0072] Bone defect is one of the most common injuries in clinical practice, with a high disability rate and strong destructiveness to human health. With the increase of age, human bones inevitably suffer from bone aging, osteoporosis and even necrosis, resulting in bone defects. In addition, due to traffic accidents and orthopedic diseases, a large number of patients also face the problem of bone defects. When the bone defect exceeds the critical threshold, osteoblasts are insufficient to repair it.

[0073] Bone transplantation is a way to repair bone defects. Existing bone implants cannot cope with small spaces and are difficult to implant.

[0074] In view of the above problems, the bone repair material manufacturing method provided by the exemplary embodiment of the present invention adopts a multi-bionic strategy of combining two bionic structures when constructing a model. The Octet lattice structure is improved by combining the U-shaped arch in the tortoise shell structure. The beams forming the Octet lattice structure are formed by a minimal curved surface structure with biocompatibility, so that the stiffness, pore size, and porosity of the metamaterial can be decoupled, and the bone of the metamaterial adapted to the implantation site can be regulated separately. Furthermore, the metamaterial formed by the cellular structure is made of shape memory alloy, and the phase change temperature of the shape memory alloy is controlled at a preset temperature. The bone repair material is compressed and shaped before implantation, and the structure is pre-programmed. After implantation, the temperature is increased by heating technology without damaging the human body, so that the structure returns to the original shape, thereby allowing the bone repair material to be implanted in a small space.

[0075] Figure 1 is an axonometric structural schematic diagram of a cell structure according to an embodiment of the present invention; Figure 2 is a schematic diagram of the main structure of the cell structure according to an embodiment of the present invention. Figure 1 and Figure 2As shown, in the cell structure provided by the exemplary embodiment of the present invention, the outline of the cell structure is a cube, the cube has two opposite surfaces 10 and four side surfaces 20 surrounded by the two surfaces 10, each surface 10 has a first node 31 located at the center of the surface 10 and four third nodes 33 located at the vertices of the cube, each side surface 20 has a second node 32 located at the center of the side surface 20, and the cube also has a fourth node 34 located at the center of the cube; the cell structure also includes a plurality of semicircular first beams 41 and circular second beams 42, each side surface 20 is formed by two first beams 41, In the same side surface 20, the arc tops of the two first beams 41 are connected to the second node 32, and the two ends of each first beam 41 are respectively connected to the two third nodes 33 of the same surface 10; each surface 10 is formed by two first beams 41, and in the same surface 10, the arc tops of the two first beams 41 are connected to the first node 31, and the two ends of each first beam 41 form the third node 33 respectively; each second node 32 is connected to the first node 31 through the second beam 42; the second nodes 32 of two adjacent side surfaces 20 are connected through the second beam 42; the first beam 41 and the second beam 42 are both formed by a minimal curved surface structure.

[0076] Exemplarily, the two first beams 41 on the side 20 are arranged in a manner that their openings are away from each other, that is, the opening of each first beam 41 faces the surface 10 adjacent thereto, and the two ends are respectively connected to the two third nodes 33 on the adjacent surface 10. The two first beams 41 located on the surface 10 are also arranged in a manner that their openings are away from each other, and the four ends of the two first beams 41 on the same surface 10 are respectively connected to the four third nodes 33 on the surface 10. The arrangement of the first beams 41 on the two surfaces 10 may be the same or different. When the arrangement is different, the ends of the first beams 41 on one surface 10 are respectively connected to the third nodes 33 located on two opposite side surfaces 20, and the ends of the first beams 41 on the other surface 10 are respectively connected to the third nodes 33 located on the other two opposite side surfaces 20.

[0077] Exemplarily, the first nodes 31 are connected to the second nodes 32 respectively through the second beams 42, and the openings of the eight second beams 42 are all facing the periphery of the macro cube. Exemplarily, two adjacent second nodes 32 are connected through the second beams 42, and the openings of the four second beams 42 are all facing the periphery of the macro cube.

[0078] Figure 3 Schematic diagram of the design principle of the cell structure according to an embodiment of the present invention. Figure 3As shown, the design idea of ​​the cell structure provided by the exemplary embodiment of the present invention is that the lattice includes a macro cell, the general outline of the macro cell is a cube, and the lattice structure is roughly a metal atom face-centered cubic arrangement structure, and the lattice structure has the characteristics of high specific strength. The macro cell includes eight vertices of the virtual cube, that is, eight third nodes 33, and also includes six face center points, that is, the first nodes 31 of the two surfaces 10 and the second nodes 32 of the four side surfaces 20, and also includes a fourth node located at the center of the virtual cube. The first beam 41 and the second beam 42 between each node are straight rods before macro-scale optimization, based on the U-shaped arch in the tortoise shell structure, and are arc-shaped rods after macro-scale optimization, wherein the first beam 41 is a semicircular arc rod, and the second beam 42 is a rod smaller than a semicircular arc, for example, the second beam 42 is a quarter-circular arc rod.

[0079] Figure 4 The stress-strain curves of the cell structure before and after macro-scale optimization of the embodiment of the present invention are shown. Figure 4 As shown, the above macro-size optimization can further improve the stiffness and strength of the lattice structure.

[0080] When the second beam 42 is a quarter-circular arc-shaped rod, after the cell structure forms a metamaterial, the two adjacent cell structures are at the second node 32 of the side 20. Since the openings of the second beam 42 are all facing the periphery of the macroscopic cube, when the two cell structures are spliced, the corresponding second beams 42 in the two different cell structures present a U-shaped arch setting, so that the formed metamaterial structure is a U-shaped arch structure both on the cube surface and inside, thereby increasing the stiffness and strength of the metamaterial.

[0081] Fig.17 FIG. 1 is a schematic flow chart of a method for manufacturing a bone repair material according to an embodiment of the present invention. Fig.17 As shown, the manufacturing method comprises the following steps:

[0082] Step 101: construct a first cellular structure model, wherein the first beam 41 and the second beam 42 of the first cellular structure are both straight bars.

[0083] For example, the first cell structure is a macroscopic cubic frame structure, which is constructed based on the Octet lattice structure. Then, the first beam 41 and the second beam 42 are structurally optimized based on the U-shaped arch in the tortoise shell structure, for example, the first beam 41 is a semicircular arc rod, and the second beam 42 is a quarter-circular arc rod, to obtain the second cell structure model.

[0084] Step 102: The first beam 41 and the second beam 42 are formed using a minimal surface structure to obtain a third cell structure model.

[0085] like Figure 3As shown, after the macroscopic scale optimization of the cell structure, the microscopic scale optimization is also performed, for example, using a minimal surface structure to form each beam, so that the cell structure has excellent biocompatibility.

[0086] A minimal surface refers to a surface with zero average curvature. There are many forms of minimal surface structures, such as Costa series minimal surfaces - single period, Cobogo House minimal surfaces - double period, FRD(r)Surface - three period, etc.

[0087] For example, the first beam 41 and the second beam 42 in the cell structure provided by the exemplary embodiment of the present invention are both formed by a Gyroid three-periodic minimal surface structure. When the Gyroid three-periodic minimal surface structure is integrated with the macro cell, the size of the macro cube and the size of the micro cube are selected, wherein the macro cube contains a plurality of micro virtual sub cubes, the Gyroid lattice is filled in the micro virtual cube, and the micro structure is filled in the macro cell structure, thereby forming a cell of a dual-scale lattice metamaterial. Figure 3 As shown, in the macroscopic structural parameters of the cell structure, the unit cell length is L, that is, the edge length of the macroscopic virtual cube is L, the rod diameter of the second beam 42 is R, that is, the virtual cross-sections of the second beam 42 and the first beam 41 are both circular, and R is the diameter of the circle; in the microscopic structural parameters, the unit cell length of the Gyroid lattice is c, and the wall thickness is h. It should be noted that after the macroscopic cell structures of the first beam 41 are bonded together to form a metamaterial, the cross-section after the combination is also circular.

[0088] Step 103: spatially array the third cell structure model to obtain an array structure model.

[0089] An exemplary embodiment of the present invention further provides a metamaterial for bone repair, which is formed by an array of multiple cellular structures, wherein the cellular structure is the cellular structure in the above-mentioned embodiment; in two fitted cellular structures, the corresponding two second beams 42 in different cellular structures are arranged in a semicircular shape, that is, the cellular structures are fitted together to form an array structure of the metamaterial.

[0090] Step 104: Using an additive manufacturing process to manufacture a bone repair material based on the array structure model.

[0091] The metamaterial for bone repair is integrally formed by 3D printing, and the material of the metamaterial can be a variety of alloys, for example, magnesium alloy, zinc alloy, aluminum alloy, titanium alloy, stainless steel, copper alloy, cobalt-based alloy, zirconium-based alloy, etc. Exemplarily, selective laser melting (SLM) is used for preparation.

[0092] Exemplarily, the deformable bone repair material may be one of a copper-based shape memory alloy, an iron-based shape memory alloy, and a nickel-titanium-based shape memory alloy.

[0093] For example, the copper-based shape memory alloy includes one of Cu-Zn, Cu-Zn-Al, Cu-Zn-Sn, Cu-Zn-Si, Cu-Zn-Ga, and Cu-Sn alloys; the iron-based shape memory alloy includes one of Fe-Pt, Fe-Mn-Si, Fe-Ni-Co-Ti, Fe-Mn-Al-Ni, and Fe-C-Mn-Si-Cr-Ni alloys; the nickel-titanium-based shape memory alloy includes one of Ni-Ti-Cu, Ni-Ti-Co, Ni-Ti-Fe, and Ni-Ti-Nb alloys.

[0094] Fig.12 is a differential thermal scanning analysis curve of the metamaterial according to an embodiment of the present invention. Fig.12 As shown, nickel-titanium alloy was used as the substrate and prepared using SLM 3D printing technology. The laser power was 140W, the powder layer thickness was 30μm, the hatch scanning interval was 80μm, the scanning speed was 1000-1100mm / s, and the austenite phase transformation peak temperature of the prepared sample was Ap.

[0095] Exemplarily, the austenite phase transformation peak temperature Ap of the nickel-titanium alloy substrate is regulated according to the scanning speed s, and the relationship between the two satisfies Formula 1:

[0096]

[0097] The SLM nickel-titanium alloy 3D printing process parameters include laser power of 140W, powder layer thickness of 30μm, hatch scanning spacing of 80μm, scanning speed ranging from 1000mm / s to 1100mm / s, and the regulated austenite phase transformation peak temperature of 36℃~42℃.

[0098] Fig.13 42°C is a metamaterial recovery rate-time curve according to an embodiment of the present invention. Fig.13 As shown, the bone repair material was subjected to quasi-static compression at room temperature, and a recovery experiment was carried out at 42°C after shaping. After the temperature was raised to 42°C, the shape recovery rate could reach about 98%. It can be seen that the "implantation-recovery" of the bone repair material has a high reliability.

[0099] Fig.14 is a stress-strain curve of a metamaterial under cyclic compression according to an embodiment of the present invention. Fig.14As shown, ten cycles of quasi-static compression were applied to the bone repair material. The bone repair material was compressed at room temperature before fracture occurred. After unloading, the temperature was raised to above the peak temperature of the austenite phase transformation of the nickel-titanium alloy, for example 42°C. The compression operation was repeated ten times, indicating that the bone repair material has strong mechanical stability and high recovery rate under cyclic compression, and has good reusability.

[0100] In actual applications, the bone repair material is compressed and shaped, and the structure is pre-programmed. After implantation, it is slowly heated to 42°C using nickel element ferromagnetic eddy current induction. The temperature is raised without damaging the human body, allowing the structure to return to its original shape, thereby meeting the needs of implanting bone repair materials in a small space.

[0101] Fig.15 is a stress-strain curve of the metamaterial at different temperatures according to an embodiment of the present invention. Compression experiments are performed on the metamaterial at different temperatures, such as Fig.15 As shown, the metallographic structure of nickel-titanium alloy can be adjusted by temperature to obtain different stiffness and strength. When the temperature reaches the peak temperature of austenite transformation, the higher the temperature, the greater the volume fraction of austenite, and the greater the stiffness of the bone repair material.

[0102] The following experiment will be conducted using nickel-titanium alloy as an example, which should not be construed as a limitation on the material of the metamaterial of the present invention.

[0103] For example, the length of the macro cube unit cell is L = 20 mm, and the macro geometric parameters of the metamaterial, rod diameter R, micro geometric parameters, Gyroid unit cell size c, and Gyroid wall thickness h are changed to print various samples. The name of the sample represents the value of the geometric parameter. Take the sample numbered 1 as an example. The geometric parameters of the sample named R36c30h80 are: R = 3.6 mm, c = 3.0 mm, h = 0.8 mm. The porosity and pore size of the prepared samples are shown in Table 1.

[0104] Table 1 Metamaterial samples with different geometric parameters

[0105]

[0106] As shown in Table 1, by comparing the data of sample 1 with sample 5, sample 6, and sample 8, it can be seen that the porosity and pore size are decoupled by regulating the dual-scale (macroscale and microscale) geometric parameters of the cell structure of the exemplary embodiment of the present invention.

[0107] Since the porosity of human cancellous bone is between 50% and 90%, and the pore size required for cell growth is in the range of 300μm to 600μm, it can be seen from Table 1 that the porosity of the metamaterial can be adjusted between 50% and 90% by regulating the geometric parameters of the cell structure respectively. The porosity in this range is convenient for the transmission and sufficient flow of nutrients inside the bone, and the diameter of the micropores can also be adjusted between 150μm and 700μm. When the diameter of the micropores is in the range of 300μm to 600μm, human bone cells can be easily adhered, proliferated, and differentiated on the material. It can be seen that when the metamaterial of the exemplary embodiment of the present invention is used for bone defect repair, the porosity and pore size can be regulated separately to adapt to the requirements of bone implantation and be more conducive to the growth needs of cells in different implantation sites.

[0108] Figure 5 is a stress-strain curve of a metamaterial with different rod diameters according to an embodiment of the present invention. Figure 5 As shown in the figure, the samples prepared by the metamaterial were subjected to compression tests. As the rod diameter R increased, the stiffness and strength increased.

[0109] Figure 6 ] is a stress-strain curve of a metamaterial with different wall thicknesses according to an embodiment of the present invention. Figure 6 As shown in the figure, the samples prepared by metamaterials were subjected to compression test. As the wall thickness h of the Gyroid structure increased, the stiffness and strength increased.

[0110] Figure 7 ] is a stress-strain curve of a metamaterial with different microscopic cell sizes according to an embodiment of the present invention. Figure 7 As shown in the figure, the samples prepared by the metamaterial were subjected to compression tests. As the unit cell size c of the Gyroid structure decreased, the stiffness and strength increased. Compared with the rod diameter R and the wall thickness h of the Gyroid structure, the unit cell size c of the Gyroid structure has a more significant effect on the stiffness and strength of the metamaterial.

[0111] Figure 8 is the stiffness value of the metamaterial with different geometric parameters according to the embodiment of the present invention. Figure 8As shown, samples 1 to 10 can smoothly transition from about 100 MPa to more than 1000 MPa through the changes of different geometric parameters: rod diameter R, Gyroid structure wall thickness h, Gyroid structure unit cell size c. They not only have a large adjustment range, but also can customize the stiffness value with high precision within the adjustment range. Since the porosity of human cancellous bone is 50% to 90%, the pore size required for cell growth is 300 μm to 600 μm, and the elastic modulus is 50 MPa to 800 MPa, the metamaterial of the exemplary embodiment of the present invention can be adapted to the implantation site in terms of stiffness, porosity, and pore size, achieving the decoupling of stiffness, porosity, and pore size. Under the condition of satisfying the porosity, the stiffness can also be adapted, and the stress shielding effect can be avoided. It can also be said that the pore size, stiffness, and porosity can be adjusted separately within a large range, and the most suitable pore size can be provided for the attachment, growth, and nutrient transport of the implanted cells under the premise of adapting the stiffness and strength of the implanted object and avoiding stress shielding.

[0112] The stress shielding effect means that after fracture fixation treatment, it is advocated in clinical treatment to use a plate with higher stiffness and strength to fix the fracture site. This method can provide a stable mechanical environment for the fracture tissue in the short term after surgery to prevent re-injury. It also provides solid support for the body, which is conducive to the patient's normal activities during the rehabilitation process. However, since the stiffness of the plate is much greater than that of the bone tissue, the bone tissue is at a low stress level for a long time. In the later stages of fracture rehabilitation, the bone tissue will develop symptoms such as osteoporosis due to insufficient mechanical stimulation. Fractures are often prone to recurrence after the plate is removed. Often, the longer the fixation time, the worse the mechanical properties of the bone.

[0113] In order to further illustrate the biocompatibility of the metamaterial of the exemplary embodiment of the present invention, a sample named R40c30h80 is selected as an example for testing, and the porosity, pore size and elastic modulus of the sample can adapt to the vertebrae of the human body. The sample is used to prepare an extract for cell culture, and cells are cultured and observed.

[0114] The test process is as follows: the 3D printed metamaterial sample (R40c30h80) was immersed in 75% alcohol for 1 hour for disinfection, and then referred to ISO 10993 Part 12, at an extraction ratio of 0.1g / ml, and added to the cell culture medium after immersion for 72 hours.

[0115] Human BMSC cells were cultured in a special culture medium in a constant temperature incubator with 5% CO2, 37°C and saturated humidity with a loose lid. The medium was changed every 1 to 2 days and the cells were digested and passaged when they grew to 80% confluence.

[0116] HUVEC cells were cultured in a dedicated complete culture medium in a constant temperature incubator at 5% CO2, 37°C and saturated humidity with a loose lid. The medium was changed every 1 to 2 days and the cells were digested and passaged when they grew to 80% confluence.

[0117] In all experiments, a control group was set up for culture without adding extract.

[0118] The culture medium was stained and observed under a microscope to observe and analyze the biological behavior and activity of human BMSC cells and their differentiated osteoblasts, as well as HUVEC cells.

[0119] Fig. 9 2 is a graph showing the CCK-8 count of human bone marrow mesenchymal stem cells at different extraction liquid volume fractions of the metamaterial according to an embodiment of the present invention. Fig. 9 As shown, CCK-8 was used to detect the changes in cell viability of human BMSC cells on days 1, 3, and 7.

[0120] Specifically, the metamaterial extracts were added at concentrations of 10%, 20%, 50%, and 100%, and after culturing human BMSC cells for 1 day, 3 days, and 7 days, CCK8 staining counting solution was added to each well and the absorbance of each well at a wavelength of 450nm was measured using an ELISA reader. The higher the absorbance, the more cells there are, that is, the more significant the cell proliferation behavior is, and the higher the cell activity is. The test results are as follows: Fig. 9 As shown, it is shown that the extract of the exemplary metamaterial that can be used for bone repair of the present invention is highly compatible with human BMSC cells and has no significant effect on the activity and proliferation behavior of the cells.

[0121] Fig.10 : is a graph showing the results of an osteoblast alizarin red staining experiment of a metamaterial according to an embodiment of the present invention. The osteoblasts after differentiation, culture and alizarin red staining were subjected to absorbance detection. The test results are shown in FIG. Fig.10 As shown, the absorbance of osteoblasts Alizarin Red staining increased after adding the metamaterial extract, indicating that the metamaterial extract increased the number of calcium nodules in osteoblasts, that is, the metamaterial has a promoting effect on the growth of osteoblasts.

[0122] Fig.11 The figure is a result of the experiment on the migration and invasion of vascular endothelial cells of the metamaterial according to the embodiment of the present invention. HUVEC cells were cultured to a certain number and then placed in one of the two chambers separated by a thin film so that the cells can shuttle through. After 72 hours of culture, the total number of cells that shuttled through the other chamber was counted. Fig.11 As shown in the figure, after adding the metamaterial extract, the total number of cells in the other chamber in the HUVEC cell migration and invasion experiments increased, indicating that the metamaterial has a promoting effect on the activity and proliferation of HUVEC cells.

[0123] Fig.16 : (a) osteogenic gene ALP, (b) RUNX2 gene expression experimental results of the metamaterial according to the embodiment of the present invention. Fig.16 As shown, RNA was extracted and reverse transcribed from the differentiated and cultured osteoblasts, and then quantitative polymerase chain reaction was performed to detect the expression of osteoblast genes ALP and RUNX2. After adding the metamaterial extract, the expression levels of osteoblast genes ALP and RUNX2 were significantly increased. It can be seen that the exemplary bone repair material of the present invention has a promoting effect on the growth of osteoblasts.

[0124] Fig.18 The figure is a result of the vascular endothelial cell scratch test of the bone repair material according to the embodiment of the present invention. After the HUVEC cells are cultured to a certain number, a scratch is made on the cell plate and the culture is continued. After 72 hours of culture, the growth of cells on both sides through the scratch is observed. Fig.18 It can be seen that the area and density of cells cultured in the metamaterial extract on the scratch are greater than those of the control group, and the migration rate is also higher. Therefore, the bone repair metamaterial of the present invention has a promoting effect on the activity and proliferation of HUVEC cells.

[0125] Fig.19 The figure is a result of the experiment on the formation of vascular endothelial cells lumen of the bone repair material according to the embodiment of the present invention. HUVEC cells were digested and inoculated on a specific culture medium, and the formation of tubule-like structures of endothelial cells was observed with an inverted microscope 6 hours after adding the material leaching solution. Fig.19 As shown, the number of tubules formed by cells cultured in the metamaterial extract is greater than that of the control group. Therefore, the bone repair metamaterial of the present invention has a promoting effect on the activity and proliferation of HUVEC cells.

[0126] It should be understood by those skilled in the art that the above embodiments are only for the purpose of clearly illustrating the present invention, and are not intended to limit the scope of the present invention. For those skilled in the art, other changes or modifications may be made based on the above disclosure, and these changes or modifications are still within the scope of the present invention.

Claims

1. A method for manufacturing a bone repair material, characterized in that: The bone repair material is formed by a cell structure, the outline of the cell structure is a cube, the cube has two opposite surfaces and four side surfaces surrounded by the two surfaces, and the cell structure is formed by a plurality of first beams and second beams; The manufacturing method comprises: Constructing a first cellular structure model, wherein the first beam and the second beam of the first cellular structure are both straight bars; The first beam and the second beam are formed by using a minimal surface structure to obtain a third cell structure model; Performing spatial arraying on the third cell structure model to obtain an array structure model; The array structure model is manufactured using an additive manufacturing process to obtain a bone repair material.

2. The method for producing a bone repair material according to claim 1, characterized in that: Before the first beam and the second beam are formed by using a minimal surface structure to obtain a third cell structure model, the method further includes: The first beam and the second beam in the first cellular structure model are replaced by at least a portion of a semicircular arc rod to obtain a second cellular structure model.

3. The method for producing a bone repair material according to claim 2, characterized in that: In the second cell structure model, the first beam is a semicircular arc-shaped first beam, and the arc shape of the second beam is a quarter-circular arc shape.

4. The method for producing a bone repair material according to claim 3, characterized in that: The first beam and the second beam are formed by using a minimal surface structure to obtain a third cell structure model, including: The cube of the cell structure is divided into a plurality of sub-cubes, each of the sub-cubes is filled with a lattice of a minimal surface structure, and the intersection of the lattice in each of the sub-cubes and the first beam and the second beam of the cell structure is obtained by Boolean operation.

5. The method for producing a bone repair material according to claim 4, characterized in that: The additive manufacturing process includes a selective laser melting process.

6. The method for producing a bone repair material according to claim 5, characterized in that: The laser power of the selective laser melting process is 130W to 150W, the thickness of the powder layer is 20μm to 40μm, and the hatch scanning interval is 70μm to 90μm.

7. The method for producing a bone repair material according to claim 5, characterized in that: The scanning speed of the selective laser melting process is negatively correlated with the austenite transformation peak temperature of the bone repair material.

8. The method for producing a bone repair material according to claim 5, characterized in that: The substrate for the selective laser melting process is a shape memory alloy.

9. The method for producing a bone repair material according to claim 8, characterized in that: The shape memory alloy includes one of a copper-based shape memory alloy, an iron-based shape memory alloy, and a nickel-titanium-based shape memory alloy.

10. A bone repair material, characterized in that: The bone repair material is prepared by the method for preparing the bone repair material according to any one of claims 1 to 9.

Citation Information

Patent Citations

  • Preparation method of Thiessen polygonal bionic artificial bone structure based on broken bone surface

    CN110974488A

  • Micro-nano porous functional device and additive manufacturing method and application thereof

    CN113290242A

  • Porous scaffold structure for bone repair implant and processing method of porous scaffold structure

    CN114587713A

  • Novel titanium alloy orthopedic implant based on additive manufacturing and manufacturing method thereof

    CN116833425A

  • Functionalized-mechanical superstructure unit, support and machining method

    CN117982272A

Cited By

  • High-strength 3D printing nickel-titanium-iron shape memory alloy and preparation method thereof