A catalyst for the production of green methanol from biomass syngas, its preparation method and application

The CuO-ZnO-Al2O3 nanocatalyst, promoted by highly dispersed metal oxides with multiple interfacial active sites, solved the problem of low CO2 conversion efficiency in hydrogen-rich biomass syngas, achieving efficient production of green methanol, simplifying the process and reducing costs.

CN118767924BActive Publication Date: 2026-11-17GUANGZHOU INST OF ENERGY CONVERSION CHINESE ACAD OF SCI
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202410762541.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-06-13
Publication Date
2026-11-17
Estimated Expiration
2044-06-13

AI Technical Summary

Technical Problem

Existing catalysts are inefficient at converting high concentrations of CO2 in hydrogen-rich biomass syngas into methanol. Traditional CuO-ZnO-Al2O3 catalysts have low CO2 conversion efficiency, which limits the high-value utilization of biomass organic solid waste.

Method used

A CuO-ZnO-Al2O3 nanocatalyst with highly dispersed multi-interfacial active sites was used. The specific surface area and pore volume of the catalyst were increased by surfactant-assisted co-precipitation and alkaline solution removal treatment, thereby enhancing the CO2 adsorption and activation capabilities.

Benefits of technology

It achieves efficient conversion of CO2 from hydrogen-rich biomass syngas into methanol, increases methanol yield and selectivity, simplifies the process, reduces costs, and is suitable for large-scale production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118767924B_ABST
    Figure CN118767924B_ABST
Patent Text Reader

Abstract

This invention discloses a catalyst for the preparation of green methanol from hydrogen-rich biomass syngas, its preparation method, and its application. The precursor structure of the catalyst is xCuO-yZnO-zAl2O3-mMO, where MO is one or both of CeO2 and TiO2; x, y, z, and m are 50-60%, 20-30%, 5-15%, and 5-15%, respectively. During the precipitation process, a surfactant is added to promote the dispersion of active sites at the metal interface. Alkali treatment of the catalyst reduces aluminum content, increasing the specific surface area and pore volume, and raising the oxygen vacancy concentration. This enhances the adsorption and activation of CO2 in the syngas, as well as the formation and conversion of methanol intermediates, thereby enabling the direct conversion of high-concentration CO2 in the hydrogen-rich biomass syngas into methanol with minimal decarbonization.
Need to check novelty before this filing date? Find Prior Art

Description

Technical fields:

[0001] This invention belongs to the field of green methanol synthesis, specifically relating to a catalyst for preparing green methanol from hydrogen-rich biomass syngas, its preparation method, and its application. Background technology:

[0002] Green methanol, as a safe, efficient, and renewable clean energy source, is liquid at room temperature and pressure. It exhibits unique advantages in storage and transportation, multi-functional applications, and market potential, with a safety level equivalent to gasoline. Currently, methanol production mainly utilizes three traditional feedstocks: coal, coke oven gas, and natural gas. However, traditional processes have high carbon emissions, with CO2 emissions reaching 3.5 tons per ton of methanol. Achieving large-scale, low-carbon, or zero-carbon methanol production would undoubtedly promote the green and safe development of my country's energy sector.

[0003] Biomass is the only zero-carbon renewable resource in nature, characterized by its abundance and wide distribution. Crop straw, livestock manure, and other biomass organic solid waste are among the most valuable and abundant renewable resources on Earth. my country produces 800 million tons of straw and 3.05 billion tons of livestock manure annually, but the vast majority of these resources are not effectively utilized, resulting in a significant waste of biomass resources. Currently, the production of green methanol (hereinafter referred to as green methanol) by coupling biomass syngas obtained through gasification with renewable energy power generation and water electrolysis for hydrogen production can achieve near-zero CO2 emissions, and several such facilities have been planned or are under construction. However, the typical composition of syngas obtained from the gasification of straw-based biomass is approximately 45% CO, 33% H2, and 20% CO2 (with the remaining components being CH4, N2, H2S, HCl, NH3, etc.). The (H2-CO2) / (CO+CO2) ratio is only 0.2, far less than the 1 / 2 required for methanol synthesis. This often necessitates processes such as water-gas shift conversion and decarbonization to increase the H2 content and reduce the CO2 content of the syngas to meet the requirements of methanol synthesis, inevitably resulting in significant CO2 emissions. Furthermore, these processes are complex and costly, hindering large-scale application. Our team's previous patent CN117106485A disclosed a method for producing hydrogen-rich biomass syngas by coupling biomass through catalytic cracking, steam reforming, and water-gas shift reaction. The resulting syngas contains 50-90% hydrogen, making it an ideal raw material for producing green methanol. How to efficiently convert it into methanol urgently requires in-depth research.

[0004] Traditional methanol synthesis mainly involves the hydrogenation of carbon monoxide, with a typical catalyst being the CuO-ZnO-Al2O3 catalyst. Cu / ZnO is considered the main active metal, and Al2O3 primarily serves as a structural aid. However, the traditional CuO-ZnO-Al2O3 catalyst for CO hydrogenation to methanol has low efficiency in converting CO2 to methanol, especially for syngas containing both CO and CO2, where it tends to convert CO more readily than CO2. Patent CN117282432A discloses a catalyst and its preparation method for synthesizing green methanol by combining Cu / ZnO and oxide solid solutions to couple biomass gasification with renewable energy sources. However, this type of catalyst is suitable for feed gas compositions of CO, CO2, and H2, with CO molar content of 40%–50%, CO2 molar content of 15%–25%, and H2 molar content of 25%–45%. The CO conversion rate is ≤35%, and the CO2 conversion rate is <7%, limiting its application in green methanol synthesis. For the hydrogen-rich biomass syngas (composition of 65-75% H2, 15-20% CO2, 5-10% CO, 2-5% CH4, and 1-3% other hydrocarbons) produced by catalytic cracking and steam reforming of biomass (CN117106485A), how to directly and effectively convert it into green methanol is of great significance for accelerating the high-value utilization and resource utilization of biomass organic solid waste. Summary of the Invention:

[0005] This invention provides a catalyst for the preparation of green methanol from hydrogen-rich biomass syngas, its preparation method, and its application. The hydrogen-rich biomass syngas is produced by a one-step coupling process of catalytic cracking and steam reforming of biomass, with a gas composition of 65-75% H2, 15-20% CO2, 5-10% CO, 2-5% CH4, and 1-3% other hydrocarbons. The catalyst is a CuO-ZnO-Al2O3 nanocatalyst with highly dispersed multi-interfacial active sites, which can achieve efficient conversion of CO2 in hydrogen-rich biomass syngas into methanol.

[0006] This invention is achieved through the following technical solutions:

[0007] A catalyst suitable for preparing green methanol from hydrogen-rich biomass syngas is characterized in that the hydrogen-rich biomass syngas is produced by a one-step coupled process of catalytic cracking and steam reforming of biomass (see CN117106485A), and the gas composition is 65-75% H2, 15-20% CO2, 5-10% CO, 2-5% CH4, and 1-3% other hydrocarbons; the catalyst precursor has the structural formula xCuO-yZnO-zAl2O3-mMO, where MO is a metal oxide, which is one or a mixture of two of CeO2 and TiO2; in the catalyst structural formula, x, y, z, and m represent the mass contents of CuO, ZnO, Al2O3, and the metal oxide MO, respectively, which are 50-60%, 20-30%, 5-15%, and 5-15%; when MO is a mixture of two of CeO2 and TiO2, the mixing ratio is 1:2 to 2:1.

[0008] The preparation method of the above catalyst includes the following steps:

[0009] (1) Dissolve the precursor salts of copper salt, zinc salt, aluminum salt and metal oxide MO in water to prepare solution A, and dissolve the precipitant in water to prepare solution B;

[0010] (2) Solution A and solution B are simultaneously added dropwise to a container pre-filled with a certain amount of surfactant at a temperature of 60-70℃ for co-precipitation. The pH of the solution is controlled at 9.0-9.5. The resulting suspension is aged at 80-90℃ for 3-6 hours, then filtered, washed, dried, and calcined to obtain the catalyst precursor. The calcination temperature and time are 350-500℃ and 3-10 hours, respectively.

[0011] (3) The catalyst precursor is crushed, ground and sieved to >100 mesh, and then treated with alkaline solution at 60-90℃ for 2-10 hours. After filtration, washing and drying, the catalyst is obtained.

[0012] In step (1), the copper salt is selected from one of copper nitrate, copper acetate, or copper chloride; the zinc salt is selected from one of zinc nitrate, zinc acetate, or zinc chloride; the aluminum salt is selected from one of aluminum nitrate, aluminum acetate, or aluminum chloride; the precursor salt of the metal oxide MO is selected from at least one of cerium nitrate, cerium acetate, tetrabutyl titanate, or titanium tetrachloride; the total concentration of copper salt, zinc salt, aluminum salt, and precursor salt of metal oxide MO in solution A is 0.2–1.5 mol / L; the precipitant is selected from one of a combination of sodium carbonate and sodium hydroxide, or a combination of potassium carbonate and potassium hydroxide; the concentration of the precipitant in solution B is 0.2–1.5 mol / L.

[0013] The surfactant in step (2) is selected from at least one of hexadecyltrimethylammonium bromide, hexadecyltrimethylammonium chloride, octadecyltrimethylammonium chloride, sodium dodecylbenzenesulfonate, sodium dodecyl sulfate, etc., and its molar amount is in the ratio of the total concentration of copper salt, zinc salt, aluminum salt and metal oxide MO precursor salt in solution A to 1:100 to 1:300; the drying temperature and time are 80 to 120°C and 10 to 24 h, respectively.

[0014] Preferably, attapulgite powder is added to the surfactant in step (2) at the same time, and the amount added is 5% to 20% of the theoretical mass of the xCuO-yZnO-zAl2O3-mMO catalyst after calcination.

[0015] The alkaline solution mentioned in step (3) is an aqueous solution of sodium hydroxide or potassium hydroxide. The liquid-solid mass ratio in the dealuminization process is 3:1 to 10:1, and the amount of alkali used is 5 to 20% of the catalyst mass.

[0016] The core innovation of this invention lies in its unique surfactant-assisted co-precipitation method, which utilizes traditional CuO-ZnO-Al2O3 methanol synthesis catalysts. CeO2 and / or TiO2 oxides are used as promoters to form a highly dispersed nanocatalyst with multiple interfacial active sites on CuO-ZnO-Al2O3. Alkaline solution treatment increases the catalyst's specific surface area and pore volume, thereby increasing oxygen vacancy concentration and promoting CO2 adsorption and activation to improve its conversion rate. Simultaneously, it enhances the synergistic effect of the Cu / ZnO interface and the interfaces of different metal oxides to accelerate the formation and conversion of methanol intermediates. This allows for the direct conversion of high-concentration CO2 in hydrogen-rich biomass syngas into methanol with minimal decarbonization, ultimately increasing methanol production.

[0017] This invention also provides an application of the above-mentioned catalyst in green methanol synthesis, comprising the following steps: compressing, crushing, and sieving the catalyst powder and then loading it into a fixed-bed reactor; after reduction and activation, introducing hydrogen-rich biomass syngas (see CN117106485A for hydrogen-rich biomass syngas synthesis) at a temperature of 220–300°C, a feed gas pressure of 2–8 MPa, and a volume hourly space velocity of 2000–10000 h⁻¹. -1Under certain conditions, a catalytic conversion reaction is carried out to produce green methanol, which is a mixed alcohol with methanol as the main component and a methanol selectivity of ≥80%. The biomass is selected from at least one of sugarcane bagasse, straw, bamboo shavings, wood flour, kitchen waste, and livestock and poultry manure. The main components of the hydrogen-rich biomass syngas include H2, CO2, CO, CH4, and other hydrocarbons, wherein the molar content of H2 is 65-75%, the molar content of CO2 is 15-20%, the molar content of CO is 5-10%, the molar content of CH4 is 2-5%, and the molar content of other hydrocarbons is 1-3%. The other hydrocarbons include at least one of ethylene, ethane, propylene, and propane.

[0018] Preferably, the reaction temperature is 280-300℃, the feed gas pressure is 6-8MPa, and the volume hourly space velocity is 2000-6000h. -1 .

[0019] In the above application process, the reduction and activation process of the catalyst is carried out at a temperature of 250–350°C, a pressure of 0.1–1 MPa, and a volume hourly space velocity of 500–2000 h⁻¹. -1 The catalyst is reduced using hydrogen or a mixture of hydrogen and an inert gas for 2 to 12 hours, wherein the inert gas is selected from helium, nitrogen or argon, and the hydrogen content in the mixture is 5 to 100%.

[0020] The beneficial effects of this invention are as follows:

[0021] The catalyst of this invention is a CuO-ZnO-Al2O3 catalyst promoted by metal oxides such as CeO2 and TiO2. During the precipitation process, a surfactant is added to induce metal ions to form mixed metal oxide seed crystals in the solution or on the surface of attapulgite, achieving sufficient contact and good dispersion of active sites at different metal oxide interfaces. The specific surface area and pore volume of the catalyst are improved by alkaline solution dealumination treatment, increasing the oxygen vacancy concentration and promoting the adsorption and activation of CO2 in hydrogen-rich biomass syngas, as well as the formation and conversion of methanol intermediates. This results in excellent catalytic performance in the conversion of hydrogen-rich biomass syngas with high CO2 content (15-20%) to green alcohol. Moreover, the catalyst preparation method is simple, low-cost, and easy to achieve large-scale preparation, providing an ideal choice for the large-scale production of green methanol.

[0022] Instruction manual illustrations:

[0023] Figure 1 Scanning electron microscope (SEM) image of the 50CuO-30ZnO-10Al2O3-10CeO2 catalyst prepared according to Example 1.

[0024] Figure 2Scanning electron microscope (SEM) image of the 60CuO-30ZnO-5Al2O3-5CeO2@10ATP catalyst prepared according to Example 5. Detailed implementation method:

[0025] The following is a further description of the invention, but not a limitation thereof.

[0026] According to the method disclosed in our team's patent CN117106485A, hydrogen-rich syngas was prepared from kitchen waste as raw material, referring to Example 4. The molar content of H2 was 70%, the molar content of CO2 was 20%, the molar content of CO was 4.5%, the molar content of CH4 was 3.5%, and the molar content of other hydrocarbons was 2%.

[0027] Examples 1-3 below use biomass syngas as feedstock for methanol synthesis. Example 4 uses different feedstocks to prepare biomass syngas and obtains syngas with different compositions for methanol synthesis. Example 5 compares and investigates the effect of attapulgite addition on the catalyst's performance in chlorophyll synthesis.

[0028] The micro fixed-bed reactor used in the listed embodiments has an inner diameter of 8 mm and a length of 200 mm. The gas flow rate is regulated by a mass flow meter, the system pressure is regulated by a pressure reducer and a back pressure valve, and the reactor temperature is measured and regulated by a thermocouple and a temperature controller. After the reduction process (reduction conditions: pure hydrogen or a mixture of hydrogen and an inert gas, reduction at 250–350°C for 2–12 h, pressure 0.1–1 MPa) is completed, the temperature is adjusted to the required reaction temperature, and then synthesis gas is introduced through the back pressure valve to set the system pressure and gradually increase the temperature to carry out the reaction. The feed gas is metered by a mass flow meter before entering the reactor. A cold trap separates the synthesis product and tail gas. The tail gas is released to atmospheric pressure via a back pressure valve and then enters a six-way valve. It is analyzed using an online GC 9800 gas chromatograph (Shanghai Kechuang) with Ar as the carrier gas (flow rate 30 mL / min) and detected by a thermal conductivity detector (TCD). A TDX-01 (2 m × 3 mm) carbon molecular sieve column is used. After the reaction, the liquid product is collected and analyzed offline using an Agilent 7890 gas chromatograph with a flame ionization detector (FID) and an FFAP capillary column (30 m × 0.25 mm × 0.25 μm) with Ar as the carrier gas (flow rate 30 mL / min).

[0029] Based on the content of each component in the reaction tail gas, the carbon dioxide conversion rate, methanol yield, and selectivity in the syngas are calculated using the molar number of carbon atoms, as shown in the following formulas:

[0030] CO2 conversion rate = [n(CO2)in - n(CO2)out] / [n(CO2)in]

[0031] Methanol selectivity = n(MeOH) / [n(CO2)in-n(CO2)out]

[0032] Methanol space-time yield = m(MeOH) / [m(catalyst)×t]

[0033] In the formula, n(CO2)in and n(CO2)out are the moles of CO2 in the feed gas and tail gas, respectively; n(MeOH) and m(MeOH) are the moles and mass of methanol in the product, respectively; m(catalyst) and t are the mass of the catalyst and the reaction time, respectively.

[0034] Example 1:

[0035] Preparation and application of 50CuO-30ZnO-10Al2O3-10CeO2 catalyst:

[0036] Weigh 9.5g Cu(NO3)2·3H2O, 5.48g Zn(NO3)2·6H2O, 3.68g Al(NO3)3·9H2O, and 1.26g Ce(NO3)2·6H2O, and dissolve them in 64.5mL of water to prepare a metal salt solution A with a total metal ion concentration of 1.0mol / L; weigh 10.6g anhydrous Na2CO3 and 4g NaOH, and dissolve them in 100mL of water to prepare a precipitant solution B; weigh 0.26g hexadecyltrimethylammonium bromide, dissolve it completely in 20mL of water, add it to a 250mL three-necked flask, and heat it to 70℃; while stirring, add solutions A and B dropwise to the same beaker, and circulate the solution through the air. The pH of the solution was controlled to be 9.0 by adjusting the dropping rate. Precipitation ended when solution A was added. The resulting suspension was heated to 80℃ and aged for 6 hours. Then it was filtered and washed until neutral. The resulting filter cake was dried at 100℃ for 24 hours and then calcined in air at 350℃ for 6 hours to obtain catalyst 50CuO-30ZnO-10Al2O3-10CeO2. It was crushed, ground and sieved to >100 mesh to obtain catalyst precursor powder. 0.5g of sodium hydroxide was dissolved in 25g of water to prepare an alkaline solution. Then it was heated to 80℃, and 5g of catalyst precursor powder was added and stirred for 5 hours. Then it was filtered and washed until neutral. The resulting filter cake was dried at 105℃ for 12 hours to obtain catalyst powder. Figure 1 This is a SEM image of the catalyst in Example 1. Figure 1 As can be seen, the catalyst prepared in this embodiment is a large number of spherical particles uniformly dispersed on the surface of the thin sheet.

[0037] The catalyst powder is compressed into tablets, crushed, and sieved to obtain catalyst particles of 60-80 mesh. 1g of the sieved catalyst particles is weighed and loaded into a reactor, and the reactor is subjected to an incubation period of 300℃, 0.1MPa, and 2000 h⁻¹. -1Under the conditions of using a 10% H2 / Ar reduction catalyst for 10 h, a synthesis gas with a composition of n(H2):n(CO2):n(CO):n(CH4):n(other hydrocarbons) = 70:20:4.5:3.5:2 was introduced, and the reaction was carried out at a temperature of 220–300 °C, a pressure of 5.0 MPa, and a space velocity of 4000 h⁻¹. -1 Methanol was synthesized under the specified conditions. The reaction results are shown in Table 1. As can be seen from Table 1, both the CO2 conversion rate and the space-time yield of methanol gradually increase with increasing reaction temperature.

[0038] Table 1 Effect of reaction temperature on methanol synthesis performance

[0039] Reaction temperature (°C) <![CDATA[CO₂ conversion rate (%)]]> Methanol selectivity (%) <![CDATA[Methanol space-time yield (g / g cat. ·h)]]> 220 7.8 93.5 0.23 240 12.5 88.3 0.47 260 17.2 85.1 0.65 280 22.7 82.9 0.82 300 26.1 80.5 1.05

[0040] Comparative Example 1:

[0041] A 50CuO-30ZnO-10Al2O3-10CeO2 catalyst was prepared according to the method in Example 1. The catalyst was pulverized, compressed into tablets, and sieved to 60-80 mesh to obtain a catalyst precursor powder. This powder was then used directly for chlorophyll synthesis without alkali treatment under the following reaction conditions: temperature 280℃, pressure 5.0 MPa, and space velocity 4000 h⁻¹. -1 The obtained CO2 conversion rate was 16.3%, the methanol selectivity was 78.5%, and the methanol space-time yield was 0.56 g / g. cat. ·h.

[0042] Compared to the catalyst treated with alkali in Example 1, both the CO2 conversion rate and methanol yield decreased significantly. This demonstrates that alkali treatment for aluminum removal is crucial for improving the catalyst's performance in chlorophyll synthesis. Al removal through alkali treatment not only increases the catalyst's specific surface area and pore volume, improves the dispersion of metallic Cu, and promotes H2 adsorption and dissociation, but also increases the oxygen vacancy concentration, thereby promoting CO2 adsorption and activation to improve its conversion rate and methanol yield.

[0043] Example 2:

[0044] Preparation and application of 60CuO-20ZnO-5Al2O3-5CeO2-10TiO2 catalyst:

[0045] Weigh 9.42g Cu(CH3CO2)2·H2O, 3.66g Zn(NO3)2·6H2O, 1.84g Al(NO3)3·9H2O, 0.57g Ce(CH3CO2)3·4H2O, and 2.13g CHO4Ti, and dissolve them in 141.1mL of water to prepare a metal salt solution A with a total metal ion concentration of 0.5mol / L; weigh 10.6g anhydrous Na2CO3 and 4g NaOH, and dissolve them in 200mL of water to prepare a precipitant solution B; weigh 0.25g octadecyltrimethylammonium chloride, dissolve it completely in 20mL of water, add it to a 500mL three-necked flask, and heat it to 60℃; while stirring, simultaneously add solutions A and B dropwise to... In the beaker, the pH of the solution was controlled to be 9.2 by adjusting the dropping rate. The precipitation ended when solution A was added. The resulting suspension was heated to 90℃ and aged for 5 hours, then filtered and washed until neutral. The resulting filter cake was dried at 120℃ for 10 hours and then calcined in air at 500℃ for 3 hours to obtain catalyst 60CuO-20ZnO-5Al2O3-5CeO2-10TiO2. It was then crushed, ground, and sieved to >100 mesh to obtain catalyst precursor powder. 0.25g of potassium hydroxide was dissolved in 50g of water to prepare an alkaline solution, which was then heated to 90℃. 5g of catalyst precursor powder was added to the solution and stirred for 10 hours. The solution was then filtered and washed until neutral. The resulting filter cake was dried at 110℃ for 8 hours to obtain catalyst powder.

[0046] The catalyst powder is compressed into tablets, crushed, and sieved to obtain catalyst particles of 60-80 mesh. 1g of the sieved catalyst particles is weighed and loaded into a reactor, and the reactor is subjected to an incubation period of 250℃, 0.5MPa, and 1000h⁻¹. -1 Under the conditions of using hydrogen reduction catalyst for 2 hours, synthesis gas with a composition of n(H2):n(CO2):n(CO):n(CH4):n(other hydrocarbons) = 70:20:4.5:3.5:2 was introduced, and the reaction was carried out at a temperature of 250℃, a pressure of 2-8 MPa, and a space velocity of 4000 h⁻¹. -1 Methanol was synthesized under the specified conditions. The reaction results are shown in Table 2. As can be seen from Table 2, both the CO2 conversion rate and the space-time yield of methanol gradually increase with increasing reaction pressure.

[0047] Table 2 Effect of reaction pressure on methanol synthesis performance

[0048] Reaction pressure (MPa) <![CDATA[CO2 Conversion Rate (%)]]> Methanol selectivity (%) <![CDATA[Methanol space-time yield (g / g cat. ·h)]]> 2 12.5 81.8 0.32 4 14.1 83.5 0.55 6 17.9 89.7 0.79 8 21.6 92.1 1.07

[0049] Example 3:

[0050] Preparation and application of 55CuO-25ZnO-10Al2O3-10TiO2 catalyst:

[0051] Weigh 5.82gCuCl2, 2.09gZnCl2, 2.0g(CH3CO2)3Al, 0.87gC 16 H 36 O₄Ti was dissolved in 49.5 mL of water to prepare a metal salt solution A with a total metal ion concentration of 1.5 mol / L; 20.73 g of anhydrous K₂CO₃ and 8.42 g of KOH were weighed and dissolved in 100 mL of water to prepare a precipitant solution B; 0.25 g of sodium dodecylbenzenesulfonate was weighed and fully dissolved in 20 mL of water, then added to a 250 mL three-necked flask and heated to 65 °C; under stirring, solutions A and B were simultaneously added dropwise to the flask, and the pH of the solution was controlled to be 9.1 by adjusting the dropping rate. Precipitation ended when solution A was completely added; the resulting suspension... The liquid was heated to 85℃ and aged for 3 hours, then filtered and washed until neutral. The resulting filter cake was dried at 105℃ for 15 hours and then calcined in air at 400℃ for 10 hours to obtain catalyst 55CuO-25ZnO-10Al2O3-10TiO2. The catalyst was then pulverized, ground, and sieved to >100 mesh to obtain catalyst precursor powder. 1g of sodium hydroxide was weighed and dissolved in 15g of water to prepare an alkaline solution, which was then heated to 60℃. 5g of catalyst precursor powder was added to the solution and stirred for 2 hours. The solution was then filtered and washed until neutral. The resulting filter cake was dried at 100℃ for 24 hours to obtain catalyst powder.

[0052] The catalyst powder is compressed into tablets, crushed, and sieved to obtain catalyst particles of 60-80 mesh. 1g of the sieved catalyst particles is weighed and loaded into a reactor, and the reactor is subjected to an incubation period of 350℃, 1MPa, and 500h⁻¹ space velocity. -1 Under the conditions of using a 50% H2 / N2 reduction catalyst for 6 hours, a synthesis gas with a composition of n(H2):n(CO2):n(CO):n(CH4):n(other hydrocarbons) = 70:20:4.5:3.5:2 was introduced, and the reaction was carried out at a temperature of 260℃, a pressure of 4MPa, and a space velocity of 2000–10000 h⁻¹. -1 Methanol was synthesized under the specified conditions. The reaction results are shown in Table 3. As can be seen from Table 3, with the increase of the reaction space velocity, the CO2 conversion rate gradually decreased, but the space-time yield of methanol gradually increased.

[0053] Table 3 Effect of reaction space velocity on methanol synthesis performance

[0054] <![CDATA[Volumetric hourly space velocity (h -1 )]]> <![CDATA[CO₂ conversion rate (%)]]> Methanol selectivity (%) <![CDATA[Methanol space-time yield (g / g cat. ·h)]]> 2000 20.2 85.6 0.41 4000 18.7 86.1 0.55 6000 16.3 87.2 0.73 8000 13.9 86.8 0.85 10000 11.4 87.0 1.02

[0055] Example 4:

[0056] Preparation and application of 50CuO-20ZnO-15Al2O3-10CeO2-5TiO2 catalyst:

[0057] Weigh 9.5g Cu(NO3)2·3H2O, 2.7g (CH3CO2)2Zn·2H2O, 5.52g Al(NO3)3·9H2O, 1.92g Ce(NO3)2·6H2O, and 0.59g TiCl4, and dissolve them in 75.8mL of water to prepare a metal salt solution A with a total metal ion concentration of 0.8mol / L; weigh 16.6g anhydrous K2CO3 and 6.7g KOH, and dissolve them in 100mL of water to prepare a precipitant solution B; weigh 0.27g hexadecyltrimethylammonium bromide, dissolve it completely in 20mL of water, add it to a 250mL three-necked flask, and heat it to 65℃; while stirring, add solutions A and B dropwise to the same beaker. In the process, the pH of the solution was controlled to be 9.2 by adjusting the dropping rate. The precipitation ended when solution A was added. The resulting suspension was heated to 80℃ and aged for 5 hours. Then it was filtered and washed until neutral. The resulting filter cake was dried at 105℃ for 12 hours and then calcined in air at 400℃ for 5 hours to obtain catalyst 50CuO-20ZnO-15Al2O3-10CeO2-5TiO2. The catalyst was crushed, ground and sieved to >100 mesh to obtain catalyst precursor powder. 0.8g of sodium hydroxide was dissolved in 20g of water to prepare an alkaline solution. The solution was then heated to 75℃, and 5g of catalyst precursor powder was added and stirred for 8 hours. The solution was then filtered and washed until neutral. The resulting filter cake was dried at 100℃ for 20 hours to obtain catalyst powder.

[0058] The catalyst powder is compressed into tablets, crushed, and sieved to obtain catalyst particles of 60-80 mesh. 1g of the sieved catalyst particles is weighed and loaded into a reactor, and the reactor is subjected to an incubation period of 280℃, 0.5MPa, and 1000h⁻¹. -1 Under the conditions of using a 10% H2 / He reduction catalyst for 5 hours, hydrogen-rich syngas produced by a one-step coupled catalytic cracking-steam reforming process from five raw materials (sawdust, wheat straw, sugarcane bagasse, branches, and pig manure) was introduced at 280℃, 5.0 MPa, and 5000 h⁻¹. -1 Methanol was synthesized under the specified conditions. The reaction results are shown in Table 4. As can be seen from Table 4, the catalyst of this invention can effectively convert hydrogen-rich syngas from different biomass feedstocks into green methanol, showing broad prospects for industrial application.

[0059] Table 4. Effects of biomass feedstock on methanol synthesis performance

[0060]

[0061] Example 5:

[0062] Preparation and application of 60CuO-30ZnO-5Al2O3-5CeO2@ATP catalysts with different ATP addition amounts:

[0063] Weigh 9.11g Cu(NO3)2·3H2O, 5.48g Zn(NO3)2·6H2O, 1.84g Al(NO3)3·9H2O, and 0.63g Ce(NO3)2·6H2O, and dissolve them in 57.52mL of water to prepare a metal salt solution A with a total metal ion concentration of 1mol / L; weigh 10.6g anhydrous Na2CO3 and 4g NaOH, and dissolve them in 100mL of water to prepare a precipitant solution B; weigh 0.23g hexadecyltrimethylammonium bromide (CTAB) and 0, 0.25, 0.5, 0.75, and 1.0g attapulgite (ATP), and dissolve them thoroughly in 20mL of water, then add the solution to a 250mL three-necked flask and heat to 70℃; while stirring, add solution A... Solution A and solution B were simultaneously added dropwise to the beaker. The pH of the solution was controlled to be 9.2 by adjusting the dropping rate. Precipitation ended when solution A was completely added. The resulting suspension was heated to 80℃ and aged for 5 hours. Then it was filtered and washed until neutral. The resulting filter cake was dried at 100℃ for 24 hours and then calcined in air at 450℃ for 5 hours to obtain catalyst 60CuO-30ZnO-5Al2O3-5CeO2@ATP. The catalyst was then pulverized, ground, and sieved to >100 mesh to obtain catalyst precursor powder. 0.5g of sodium hydroxide was dissolved in 25g of water to prepare an alkaline solution. The solution was then heated to 80℃, and 5g of catalyst precursor powder was added and stirred for 5 hours. The solution was then filtered and washed until neutral. The resulting filter cake was dried at 105℃ for 12 hours to obtain catalyst powder.

[0064] The catalyst powder is compressed into tablets, crushed, and sieved to obtain catalyst particles of 60-80 mesh. 1g of the sieved catalyst particles is weighed and loaded into a reactor, and the reactor is subjected to an incubation period of 250℃, 0.5MPa, and 1000h⁻¹. -1 Under the conditions of using a 10% H2 / N2 reduction catalyst for 5 h, a synthesis gas with a composition of n(H2):n(CO2):n(CO):n(CH4):n(other hydrocarbons) = 68:17.5:7.5:5:2 was introduced at a temperature of 280℃, a pressure of 6.0 MPa, and a space velocity of 5000 h⁻¹. -1 Methanol was synthesized under the following conditions. The reaction results are shown in Table 5. Table 5 shows that with the increase of attapulgite dosage, the conversion rates of CO2 and CO in the syngas, as well as the selectivity and yield of methanol, all first increased and then decreased, reaching their highest values ​​when the dosage was 10% of the theoretical mass of the catalyst. Further increases in dosage led to a decrease in all performance indicators. This is because, during the co-precipitation process, the addition of attapulgite simultaneously with the addition of the surfactant facilitates the coating of the surfactant on the surface of the attapulgite, improving the adsorption capacity of attapulgite for metal ions and enhancing the dispersion of the mixed metal oxide particles. Figure 2This invention provides a high-performance catalyst for the conversion of hydrogen-rich biomass syngas with high CO2 content into green methanol, thereby improving catalyst performance. However, excessive attapulgite content can reduce the number of hydrogenated metal species in the catalyst, thus decreasing the catalytic performance of syngas conversion to green methanol.

[0065] Table 5. Effect of attapulgite addition on methanol synthesis performance.

[0066]

[0067] The above embodiments illustrate a catalyst for the direct preparation of green methanol from biomass syngas, its preparation method, and its application, provided by the present invention, to help understand the method and core ideas of the present invention. It should be noted that those skilled in the art can make several improvements and modifications to the present invention without departing from the principle of the present invention, and these improvements and modifications also fall within the protection scope of the claims of the present invention.

Claims

1. A catalyst suitable for producing green methanol from hydrogen-rich biomass syngas, characterized in that, The hydrogen-rich biomass syngas is produced from biomass via a one-step coupled catalytic cracking-steam reforming process. The composition of the hydrogen-rich biomass syngas consists of H2, CO2, CO, CH4, and other hydrocarbons, with H2 comprising 65-75% molar content, CO2 15-20% molar content, CO 5-10% molar content, CH4 2-5% molar content, and other hydrocarbons 1-3% molar content. The catalyst precursor has the structural formula xCuO-yZnO-zAl2O3-mMO, where MO is a metal oxide, either CeO2 or a mixture of two of them. In the structural formula of the catalyst precursor, x, y, z, and m represent the mass contents of CuO, ZnO, Al2O3, and the metal oxide MO, respectively, which are 50-60%, 20-30%, 5-15%, and 5-15%. When MO is a mixture of two of CeO2 and TiO2, the mixing ratio is 1:2 to 2:

1. The catalyst preparation method includes the following steps: (1) Dissolve the precursor salts of copper salt, zinc salt, aluminum salt and metal oxide MO in water to prepare solution A, and dissolve the precipitant in water to prepare solution B; the precipitant is selected from a combination of sodium carbonate and sodium hydroxide, or a combination of potassium carbonate and potassium hydroxide; (2) Solution A and solution B are simultaneously added dropwise to a container pre-filled with a certain amount of surfactant at a temperature of 60-70℃ for co-precipitation. The pH of the solution is controlled at 9.0-9.

5. The resulting suspension is aged at 80-90℃ for 3-6 hours, then filtered, washed, dried, and calcined to obtain the catalyst precursor. The calcination temperature and time are 350-500℃ and 3-10 hours, respectively. The surfactant is selected from at least one of hexadecyltrimethylammonium bromide, hexadecyltrimethylammonium chloride, octadecyltrimethylammonium chloride, sodium dodecylbenzenesulfonate, and sodium dodecyl sulfate. (3) The catalyst precursor is crushed, ground and sieved to >100 mesh, and then treated with alkaline solution at 60-90℃ for 2-10 hours. After filtration, washing and drying, the catalyst is obtained. The alkaline solution is an aqueous solution of sodium hydroxide or potassium hydroxide. The liquid-solid mass ratio of the dealuminization process is 3:1 to 10:

1. The amount of alkali used is 5-20% of the mass of the catalyst precursor.

2. The catalyst according to claim 1, characterized in that, In step (1), the copper salt is selected from one of copper nitrate, copper acetate, or copper chloride; the zinc salt is selected from one of zinc nitrate, zinc acetate, or zinc chloride; the aluminum salt is selected from one of aluminum nitrate, aluminum acetate, or aluminum chloride; the precursor salt of the metal oxide MO is selected from at least one of cerium nitrate, cerium acetate, or titanium tetrachloride; the total concentration of copper salt, zinc salt, aluminum salt, and precursor salt of metal oxide MO in solution A is 0.2–1.5 mol / L; and the concentration of the precipitant in solution B is 0.2–1.5 mol / L.

3. The catalyst according to claim 1, characterized in that, The drying temperature and time are 80–120°C and 10–24 h, respectively.

4. The application of the catalyst according to claim 1, characterized in that, The process includes the following steps: Catalyst powder is compressed into tablets, crushed, sieved, and then loaded into a fixed-bed reactor. After reduction and activation, hydrogen-rich biomass syngas is introduced, and the reaction is carried out at a temperature of 220–300℃, a feed gas pressure of 2–8 MPa, and a volumetric hourly space velocity of 2000–10000 h⁻¹. -1 Under certain conditions, a catalytic conversion reaction is carried out to produce green methanol; the composition of the hydrogen-rich biomass syngas is H2, CO2, CO, CH4 and other hydrocarbons, wherein the molar content of H2 is 65-75%, the molar content of CO2 is 15-20%, the molar content of CO is 5-10%, the molar content of CH4 is 2-5%, and the molar content of other hydrocarbons is 1-3%.

5. The application according to claim 4, characterized in that, The biomass is selected from at least one of sugarcane bagasse, straw, bamboo shavings, wood chips, branches, bark, kitchen waste, and livestock and poultry manure; the other hydrocarbons include at least one of ethylene, ethane, propylene, and propane.

6. The application according to claim 4, characterized in that, The catalyst reduction and activation process is carried out at a temperature of 250–350 °C, a pressure of 0.1–1 MPa, and a volume hourly space velocity of 500–2000 h⁻¹. -1 The catalyst is reduced using hydrogen or a mixture of hydrogen and nitrogen for 2 to 12 hours, wherein the hydrogen content in the mixture is 5% to 100%, but not 100%.

7. The application according to claim 4, characterized in that, The reaction temperature is 280-300℃, the feed gas pressure is 6-8MPa, and the volume hourly space velocity is 2000-6000h. -1 .

8. The application according to claim 4, characterized in that, The green methanol is a mixed alcohol with methanol as the main component and methanol selectivity ≥80%.

Citation Information

Patent Citations

  • Method for producing hydrogen through cyclic catalytic reaction of biomass waste

    CN117106485A

  • Catalyst for synthesizing green methanol by coupling biomass gasification with renewable energy hydrogen production as well as preparation method and application of catalyst