D-PtNi / MAPbI3 photocatalyst as well as preparation method and application thereof
d-PtNi is synthesized through a solvothermal co-reduction method and deposited on MAPbI3 to form a d-PtNi/MAPbI3 photocatalyst, which solves the problems of poor reaction rate and stability in photocatalytic hydrogen production technology and achieves efficient and low-cost photocatalysis. Hydrogen production performance and cycle stability.
Patent Information
- Application Number
- CN202410760805.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-13
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2044-06-13
AI Technical Summary
In existing photocatalytic hydrogen production technology, semiconductor photocatalysts have slow reaction rates and poor stability, and Pt resources are scarce and expensive. It is difficult for other cocatalysts to maintain stable and efficient hydrogen production in strong acidic environments.
PtNi alloy nanoparticles were synthesized using a solvothermal co-reduction method, and d-PtNi was formed through dealloying, which was added to MAPbI3 perovskite to form a d-PtNi/MAPbI3 photocatalyst to improve photocatalytic hydrogen production performance and cycle stability.
The d-PtNi/MAPbI3 photocatalyst significantly improves the photocatalytic hydrogen production performance and cycle stability, reduces the preparation cost, the hydrogen production rate can reach 5644 μmol/h, and the solar energy to hydrogen energy conversion efficiency reaches 6.15%, and is tested in a 24-hour cycle remain stable.
Smart Images

Figure CN118767942A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of new energy and photocatalysis, and specifically relates to a d-PtNi / MAPbI3 photocatalyst and a preparation method and application thereof. Background Art
[0002] The information disclosed in this background technology section is only intended to enhance the understanding of the overall background of the invention, and should not necessarily be regarded as an admission or any form of suggestion that the information constitutes the prior art already known to a person skilled in the art.
[0003] Hydrogen energy is a clean secondary energy source with the advantages of high energy density, zero pollution, and zero carbon emissions. It is considered to be one of the most promising energy carriers. Photocatalytic hydrogen production uses solar energy as an energy source, providing a popular alternative to traditional hydrogen production. However, the slow reaction rate and poor stability of semiconductor photocatalysts limit the development of photocatalytic hydrogen production technology. There is still a need to develop efficient and stable photocatalysts to meet the requirements of future practical applications.
[0004] Organic-inorganic hybrid perovskites have suitable and adjustable band gaps, high light absorption coefficients, wide range of light collection and excellent charge carrier migration capabilities, which are beneficial to the conversion of solar energy into chemical energy. However, perovskites are unstable in water and require solutions containing corresponding halogen elements as reaction solutions to maintain stability during photocatalysis, and their hydrogen production efficiency is still limited by intrinsic activity. Constructing heterojunctions and loading co-catalysts can effectively improve the hydrogen production capacity of organic-inorganic hybrid perovskite photocatalysts, among which Pt is the most effective co-catalyst in hydrogen production. However, the shortage of Pt resources and high prices make it difficult to apply it to industrial production, and other co-catalysts are difficult to simultaneously meet the requirements of stability under strong acid and high hydrogen production activity. Summary of the invention
[0005] In order to overcome the deficiencies of the prior art, the purpose of the present invention is to provide a d-PtNi / MAPbI3 photocatalyst and its preparation method and application. PtNi alloy nanoparticles were synthesized by solvent thermal co-reduction method, the PtNi alloy particles were added to HI acid for dealloying, and further deposited on MAPbI3 perovskite to form d-PtNi / MAPbI3 photocatalyst. The d-PtNi / MAPbI3 photocatalyst has excellent separation ability of photogenerated carriers, effectively improves the photocatalytic hydrogen production performance and cycle stability, and the low loading amount of d-PtNi reduces the preparation cost.
[0006] In order to achieve the above object, the present invention is implemented through the following technical solutions:
[0007] In a first aspect, a method for preparing a d-PtNi / MAPbI3 photocatalyst comprises the following steps:
[0008] S1, mixing platinum source, nickel source, NaBH4, PVP and ethylenediamine uniformly and performing a solvothermal reaction to obtain a PtNi alloy, and adding the PtNi alloy to hydroiodic acid for a dealloying reaction to obtain d-PtNi;
[0009] S2. Add d-PtNi and MAPbI3 into a saturated solution of MAPbI3, stir and perform a photodeposition reaction to obtain a d-PtNi / MAPbI3 photocatalyst.
[0010] Preferably, in step S1, the platinum source includes platinum acetylacetonate, the nickel source includes nickel acetylacetonate, and the ratio of the platinum source, the nickel source, NaBH4 and PVP is (3 mmol):(3 mmol):(95-105 mmol):(95-105 g).
[0011] Preferably, in step S1, the solvent thermal reaction is carried out at 150-170° C. for 18-24 hours, and the dealloying reaction time is 1-3 hours.
[0012] Preferably, in step S2, the mass of d-PtNi is 1% to 5% of the mass of MAPbI3.
[0013] Preferably, in step S2, the photodeposition reaction time is 20 to 40 minutes.
[0014] Preferably, the method also includes a method for preparing MAPbI3 and a saturated solution of MAPbI3:
[0015] Lead iodide is dissolved in a mixed solution of hydroiodic acid and hypophosphorous acid. After the lead iodide is completely dissolved, methylamine iodide is added, and after stirring for reaction, solid-liquid separation is performed to obtain MAPbI3 and MAPbI3 saturated solution.
[0016] More preferably, the volume ratio of hydroiodic acid to hypophosphorous acid is (3.5-4.5):1, and the molar ratio of lead iodide to methylammonium iodide is 1:(0.99-1.01).
[0017] More preferably, the stirring reaction time is 1 to 3 hours.
[0018] In a second aspect, a d-PtNi / MAPbI3 photocatalyst is obtained by the preparation method described in the first aspect.
[0019] In a third aspect, the application of the d-PtNi / MAPbI3 photocatalyst as described in the first aspect in photocatalytic cracking of HI to produce hydrogen.
[0020] The beneficial effects achieved by one or more technical solutions of the present invention are as follows:
[0021] As a co-catalyst, d-PtNi effectively improves the separation ability of photogenerated carriers, making the d-PtNi / MAPbI3 photocatalyst have excellent photocatalytic hydrogen production performance and cycle stability. Compared with unde-alloyed PtNi and Pt co-catalyst, d-PtNi can further improve the catalytic performance of the photocatalyst, while achieving cost reduction and performance improvement. The hydrogen production rate of the d-PtNi / MAPbI3 photocatalyst can reach 5644μmol / h; its corresponding solar energy to hydrogen energy conversion efficiency (i.e., photoinduced hydroiodic acid decomposition efficiency) reaches 6.15%. In addition, the hydrogen production performance of the d-PtNi / MAPbI3 photocatalyst did not decrease significantly after a 24-hour cycle test (one cycle every 3 hours, a total of 8 cycles), and the material structure and morphology did not change significantly.
[0022] The synthesis conditions of d-PtNi / MAPbI3 photocatalyst are mild, the preparation method is simple, and the cost is low, and it has broad commercial application prospects. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] The accompanying drawings in the specification, which constitute a part of the present invention, are used to provide a further understanding of the present invention. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute improper limitations on the present invention.
[0024] Figure 1 XRD patterns of (a) d-PtNi, PtNi in Example 1 and Pt in Comparative Example 1 and (b) MAPbI3, 3wt% d-PtNi / MAPbI3 in Example 1 and 3wt% PtNi / MAPbI3 in Comparative Example 2;
[0025] Figure 2 TEM image of d-PtNi in Example 1;
[0026] Figure 3 TEM image of 3wt% d-PtNi / MAPbI3 in Example 1, (b) is a partial enlarged image of (a);
[0027] Figure 4 The performance comparison of photocatalytic cracking HI to produce hydrogen by (a) 3wt% d-PtNi / MAPbI3 in Example 1, 1wt% d-PtNi / MAPbI3 in Example 2 and 5wt% d-PtNi / MAPbI3 in Example 3 and (b) MAPbI3 and 3wt% d-PtNi / MAPbI3 in Example 1, 3wt% Pt / MAPbI3 in Comparative Example 1 and 3wt% PtNi / MAPbI3 in Comparative Example 2;
[0028] Figure 5 The photocatalytic cracking HI hydrogen production cycle stability of 3wt% d-PtNi / MAPbI3 in Example 1;
[0029] Figure 6 (a) photocurrent density and (b) impedance spectrum of MAPbI3 and 3wt% d-PtNi / MAPbI3 in Example 1 and 3wt% PtNi / MAPbI3 in Comparative Example 2. DETAILED DESCRIPTION
[0030] In order to enable those skilled in the art to more clearly understand the technical solution of the present invention, the technical solution of the present invention will be described in detail below in combination with specific embodiments and comparative examples.
[0031] Example 1
[0032] 40mL of hydroiodic acid (48% aqueous solution) and 10mL of hypophosphorous acid (50% aqueous solution) are placed in a 100mL beaker, 14g of lead iodide is added and stirred continuously. After it is completely dissolved, 4.825g of methylamine iodide is slowly added. After stirring for 2h, the black powder and the solution are separated by centrifugation. The obtained MAPbI3 saturated solution is retained, and the black powder is MAPbI3. It is vacuum dried at 60°C for later use.
[0033] 0.12mmol platinum acetylacetonate, 0.12mmol nickel acetylacetonate, 4mmol NaBH4, and 4g PVP were added to a reactor containing 20mL ethylenediamine and stirred until dissolved, and the mixture was subjected to solvent thermal reaction at 160°C for 20h, and centrifuged to obtain PtNi alloy powder. The PtNi alloy powder was placed in 2mL HI acid, de-alloyed for 2h, and then centrifuged to obtain d-PtNi.
[0034] 250 mg MAPbI3 was dispersed in a saturated MAPbI3 solution, 7.5 mg d-PtNi was added and irradiated under simulated sunlight with a 300 W xenon lamp as the light source for 30 minutes. The solid product was collected by centrifugation and vacuum dried at 60°C. The obtained d-PtNi / MAPbI3 photocatalyst was recorded as 3 wt% d-PtNi / MAPbI3.
[0035] Example 2
[0036] 40mL of hydroiodic acid (48% aqueous solution) and 10mL of hypophosphorous acid (50% aqueous solution) are placed in a 100mL beaker, 14g of lead iodide is added and stirred continuously. After it is completely dissolved, 4.825g of methylamine iodide is slowly added. After stirring for 2h, the black powder and the solution are separated by centrifugation. The obtained MAPbI3 saturated solution is retained, and the black powder is MAPbI3. It is vacuum dried at 60°C for later use.
[0037] 0.12mmol platinum acetylacetonate, 0.12mmol nickel acetylacetonate, 4mmol NaBH4, and 4g PVP were added to a reactor containing 20mL ethylenediamine and stirred until dissolved, and the mixture was subjected to solvent thermal reaction at 160°C for 20h, and centrifuged to obtain PtNi alloy powder. The PtNi alloy powder was placed in 2mL HI acid, de-alloyed for 2h, and then centrifuged to obtain d-PtNi.
[0038] 250 mg MAPbI3 was dispersed in a saturated MAPbI3 solution, 2.5 mg d-PtNi was added and irradiated under simulated sunlight with a 300 W xenon lamp as the light source for 30 minutes. The solid product was collected by centrifugation and dried in vacuum at 60°C. The obtained d-PtNi / MAPbI3 photocatalyst was recorded as 1 wt% d-PtNi / MAPbI3.
[0039] Example 3
[0040] 40mL of hydroiodic acid (48% aqueous solution) and 10mL of hypophosphorous acid (50% aqueous solution) are placed in a 100mL beaker, 14g of lead iodide is added and stirred continuously. After it is completely dissolved, 4.825g of methylamine iodide is slowly added. After stirring for 2h, the black powder and the solution are separated by centrifugation. The obtained MAPbI3 saturated solution is retained, and the black powder is MAPbI3. It is vacuum dried at 60°C for later use.
[0041] 0.12mmol platinum acetylacetonate, 0.12mmol nickel acetylacetonate, 4mmol NaBH4, and 4g PVP were added to a reactor containing 20mL ethylenediamine and stirred until dissolved, and the mixture was subjected to solvent thermal reaction at 160°C for 20h, and centrifuged to obtain PtNi alloy powder. The PtNi alloy powder was placed in 2mL HI acid, de-alloyed for 2h, and then centrifuged to obtain d-PtNi.
[0042] 250 mg MAPbI3 was dispersed in a saturated MAPbI3 solution, 12.5 mg d-PtNi was added and irradiated under simulated sunlight with a 300 W xenon lamp as the light source for 30 minutes. The solid product was collected by centrifugation and dried in vacuum at 60°C. The obtained d-PtNi / MAPbI3 photocatalyst was recorded as 5 wt% d-PtNi / MAPbI3.
[0043] Comparative Example 1
[0044] 40mL of hydroiodic acid (48% aqueous solution) and 10mL of hypophosphorous acid (50% aqueous solution) are placed in a 100mL beaker, 14g of lead iodide is added and stirred continuously. After it is completely dissolved, 4.825g of methylamine iodide is slowly added. After stirring for 2h, the black powder and the solution are separated by centrifugation. The obtained MAPbI3 saturated solution is retained, and the black powder is MAPbI3. It is vacuum dried at 60°C for later use.
[0045] 0.12 mmol of platinum acetylacetonate, 4 mmol of NaBH4, and 4 g of PVP were added to a reaction kettle containing 20 mL of ethylenediamine and stirred until dissolved. The mixture was subjected to solvothermal reaction at 160°C for 20 h and centrifuged to obtain Pt powder.
[0046] 250 mg MAPbI3 was dispersed in a saturated MAPbI3 solution, 7.5 mg Pt powder was added and irradiated under simulated sunlight with a 300 W xenon lamp as the light source for 30 minutes. The solid product was collected by centrifugation and vacuum dried at 60°C. The obtained photocatalyst was recorded as 3 wt% Pt / MAPbI3.
[0047] Comparative Example 2
[0048] 40mL of hydroiodic acid (48% aqueous solution) and 10mL of hypophosphorous acid (50% aqueous solution) are placed in a 100mL beaker, 14g of lead iodide is added and stirred continuously. After it is completely dissolved, 4.825g of methylamine iodide is slowly added. After stirring for 2h, the black powder and the solution are separated by centrifugation. The obtained MAPbI3 saturated solution is retained, and the black powder is MAPbI3. It is vacuum dried at 60°C for later use.
[0049] 0.12 mmol of platinum acetylacetonate, 0.12 mmol of nickel acetylacetonate, 4 mmol of NaBH4, and 4 g of PVP were added to a reactor containing 20 mL of ethylenediamine and stirred until dissolved. The mixture was subjected to solvent thermal reaction at 160° C. for 20 h, and centrifuged and dried to obtain PtNi alloy powder.
[0050] 250 mg of MAPbI3 was dispersed in a saturated MAPbI3 solution, and 7.5 mg of PtNi alloy powder was added and irradiated under simulated sunlight with a 300 W xenon lamp as the light source for 30 minutes. The solid product was collected by centrifugation and vacuum dried at 60°C. The obtained photocatalyst was recorded as 3 wt% PtNi / MAPbI3.
[0051] The photocatalysts and co-catalysts obtained in the examples and comparative examples were characterized by XRD, UV-visible diffuse reflectance and transmission electron microscopy. Figure 1 As shown in a, the PtNi alloy has good crystallinity, and the d-PtNi formed by dealloying has no change in the position of the characteristic peak compared to the PtNi alloy, but the degree of crystallinity is reduced. Figure 1As shown in b, MAPbI3 is a tetragonal phase structure with good crystallinity. After loading PtNi alloy and d-PtNi, no corresponding crystallization peak was found, and the crystal structure of MAPbI3 was not changed.
[0052] like Figure 2 As shown in Figure 2, d-PtNi exhibits an agglomerated particle structure. Figure 3 As shown, in 3wt% d-PtNi / MAPbI3, d-PtNi is dispersed on the surface of MAPbI3, d-PtNi exposes the (111) crystal plane, and MAPbI3 exposes the (202) crystal plane.
[0053] Example 4
[0054] 250 mg of 1wt% d-PtNi / MAPbI3, 3wt% d-PtNi / MAPbI3, 5wt% d-PtNi / MAPbI3, MAPbI3, 3wt% PtNi / MAPbI3, and 3wt% Pt / MAPbI3 were respectively dispersed in 50 mL of perovskite saturated HI solution, and the reaction solution was transferred to a photocatalytic reactor (volume: about 100 mL). The reactor was connected to a gas collection system and a gas chromatography gas evaluation system at the top and circulating cooling water (25°C) at the bottom to ensure a constant temperature during the reaction. A 300W xenon lamp was used as the light source on the top to simulate sunlight (AM1.5G).
[0055] like Figure 4 As shown in a, the performance of the photocatalysts at different d-PtNi loadings first increases and then decreases with the loading. 3wt% d-PtNi / MAPbI3 has the highest hydrogen production rate, which can reach 5644μmol / h, and its corresponding solar energy to hydrogen energy conversion efficiency (i.e., photoinduced hydroiodic acid decomposition efficiency) reaches 6.15%. Figure 4 As shown in Figure b, the hydrogen production performance of 3wt% d-PtNi / MAPbI3 is better than that of 3wt% PtNi / MAPbI3 and 3wt% Pt / MAPbI3 with the same promoter loading, which improves the performance of the composite photocatalyst while reducing the amount of Pt used. Figure 5 As shown, there was no performance degradation of 3wt% d-PtNi / MAPbI3 during 8 cycles.
[0056] like Figure 6 As shown, compared with 3wt% PtNi / MAPbI3 and MAPbI3, the photocurrent of 3wt% d-PtNi / MAPbI3 is significantly increased and the impedance is significantly reduced, indicating that 3wt% PtNi / MAPbI3 has a better ability to separate photogenerated carriers, giving it better photocatalytic performance.
[0057] Example 5
[0058] 40mL of hydroiodic acid (48% aqueous solution) and 10mL of hypophosphorous acid (50% aqueous solution) are placed in a 100mL beaker, 14g of lead iodide is added and stirred continuously. After it is completely dissolved, 4.825g of methylamine iodide is slowly added. After stirring for 1h, the black powder and the solution are separated by centrifugation. The obtained MAPbI3 saturated solution is retained, and the black powder is MAPbI3. It is vacuum dried at 60°C for later use.
[0059] 0.12mmol platinum acetylacetonate, 0.12mmol nickel acetylacetonate, 4mmol NaBH4, and 4g PVP were added to a reactor containing 20mL ethylenediamine and stirred until dissolved, and the mixture was subjected to solvent thermal reaction at 150°C for 24h, and centrifuged to obtain PtNi alloy powder. The PtNi alloy powder was placed in 2mL HI acid, de-alloyed for 1h, and then centrifuged to obtain d-PtNi.
[0060] 250 mg MAPbI3 was dispersed in a saturated MAPbI3 solution, 7.5 mg d-PtNi was added and irradiated under simulated sunlight with a 300 W xenon lamp as the light source for 20 minutes. The solid product was collected by centrifugation and vacuum dried at 60 °C to obtain a d-PtNi / MAPbI3 photocatalyst.
[0061] Example 6
[0062] 40mL of hydroiodic acid (48% aqueous solution) and 10mL of hypophosphorous acid (50% aqueous solution) are placed in a 100mL beaker, 14g of lead iodide is added and stirred continuously. After it is completely dissolved, 4.825g of methylamine iodide is slowly added. After stirring for 3 hours, the black powder and the solution are separated by centrifugation. The obtained MAPbI3 saturated solution is retained, and the black powder is MAPbI3. It is vacuum dried at 60°C for later use.
[0063] 0.12mmol platinum acetylacetonate, 0.12mmol nickel acetylacetonate, 4mmol NaBH4, and 4g PVP were added to a reactor containing 20mL ethylenediamine and stirred until dissolved, and the mixture was subjected to solvent thermal reaction at 170°C for 18h, and centrifuged to obtain PtNi alloy powder. The PtNi alloy powder was placed in 2mL HI acid, de-alloyed for 3h, and then centrifuged to obtain d-PtNi.
[0064] 250 mg MAPbI3 was dispersed in a saturated MAPbI3 solution, 7.5 mg d-PtNi was added and irradiated under simulated sunlight with a 300 W xenon lamp as the light source for 40 minutes. The solid product was collected by centrifugation and vacuum dried at 60 °C to obtain a d-PtNi / MAPbI3 photocatalyst.
[0065] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A method for preparing a d-PtNi / MAPbI3 photocatalyst, characterized in that: The following steps are involved: S1, mixing platinum source, nickel source, NaBH4, PVP and ethylenediamine uniformly and performing a solvothermal reaction to obtain a PtNi alloy, and adding the PtNi alloy to hydroiodic acid for a dealloying reaction to obtain d-PtNi; S2. Add d-PtNi and MAPbI3 into a saturated solution of MAPbI3, stir and perform a photodeposition reaction to obtain a d-PtNi / MAPbI3 photocatalyst.
2. The preparation method according to claim 1, characterized in that In step S1, the platinum source includes platinum acetylacetonate, the nickel source includes nickel acetylacetonate, and the ratio of the platinum source, the nickel source, NaBH4 and PVP is (3 mmol): (3 mmol): (95-105 mmol): (95-105 g).
3. The preparation method according to claim 1, characterized in that: In step S1, the solvent thermal reaction is carried out at 150-170° C. for 18-24 hours, and the time for the dealloying reaction is 1-3 hours.
4. The preparation method according to claim 1, characterized in that: In step S2, the mass of d-PtNi is 1% to 5% of the mass of MAPbI3.
5. The preparation method according to claim 1, characterized in that: In step S2, the photodeposition reaction time is 20 to 40 minutes.
6. The preparation method according to claim 1, characterized in that: Also included are methods for preparing MAPbI3 and MAPbI3 saturated solutions: Lead iodide is dissolved in a mixed solution of hydroiodic acid and hypophosphorous acid. After the lead iodide is completely dissolved, methylamine iodide is added, and after stirring for reaction, solid-liquid separation is performed to obtain MAPbI3 and MAPbI3 saturated solution.
7. The preparation method according to claim 6, characterized in that: The volume ratio of hydroiodic acid to hypophosphorous acid is (3.5-4.5):1, and the molar ratio of lead iodide to methylamine iodide is 1:(0.99-1.01).
8. The preparation method according to claim 6, characterized in that: The stirring reaction time is 1 to 3 hours.
9. A d-PtNi / MAPbI3 photocatalyst, characterized in that: The method is obtained by the preparation method according to any one of claims 1 to 8.
10. Use of the d-PtNi / MAPbI3 photocatalyst as claimed in claim 9 in photocatalytic cracking of HI to produce hydrogen.
Citation Information
Patent Citations
Preparation method of methylamine lead iodine-reduced graphene oxide composite photocatalytic material and application in photocatalytic hydrogen production by using the photocatalytic material
CN107876087A
MAPbI3 perovskite-based composite photocatalyst as well as preparation method and application thereof
CN114471717A
High-performance MAPbI3-TiO2 heterojunction type composite photocatalyst and preparation method thereof
CN115970716A
Systems and methods for ptni nanocages
US20190379059A1