Composite two-dimensional indium oxide-based catalyst as well as preparation method and application thereof
By modifying In2O3 to form an In2O3/Mxene catalyst, using h+ as the main active component, the problem of low degradation efficiency of PFASs by traditional catalysts is solved, and efficient PFASs degradation and photocatalytic activity improvement are achieved.
Patent Information
- Application Number
- CN202410749578.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-12
- Publication Date
- 2024-10-15
AI Technical Summary
It is difficult for traditional catalysts to degrade PFASs because their degradation mechanism relies on OH to attack hydrogen atoms on carbon, while PFASs have no hydrogen atoms on carbon, and the oxidation potential of OH is less than the C-C bond energy, making it difficult to break the C-C bond, and the band gap of the In2O3 photocatalyst wide, limiting the development and application of photocatalytic technology.
By using Ti3AlC2-based two-dimensional Mxene material to modify In2O3 to form an In2O3/Mxene catalyst, construct a Schottky Schottky heterojunction, adjust its micromorphology, improve the transfer efficiency of conduction band electrons, and reduce the recombination rate of photogenerated electron holes, using h+ serves as the main catalytically active component.
It significantly improves the degradation efficiency and selectivity of PFASs, improves the photocatalytic activity, solves the problem of low degradation efficiency of PFASs by traditional catalysts, and improves the light utilization ability and stability.
Smart Images

Figure CN118767957A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of organic pollutant treatment, and in particular to a composite two-dimensional indium oxide-based catalyst and a preparation method and application thereof. Background Art
[0002] PFASs are a class of artificially synthesized aliphatic hydrocarbon organic compounds in which all hydrogen atoms attached to the hydrophobic carbon chain are replaced by fluorine and connected to various hydrophilic groups. They are persistent organic pollutants with the characteristics of high toxicity, persistence, bioaccumulation and long-range migration.
[0003] It is difficult for traditional catalysts to degrade PFASs. This is because the degradation mechanism of traditional catalysts for pollutants is to produce ·OH to attack the hydrogen atoms on the carbon of the pollutant to undergo a dehydrogenation reaction, while most PFASs have no hydrogen atoms on their carbon. In addition, the oxidation potential value of ·OH (276.0 kJ / mol) is significantly smaller than the average CC bond energy (347.0 kJ / mol), making it difficult to break the CC bonds of the pollutant.
[0004] In recent years, researchers have obtained a group of nano-photocatalytic materials represented by indium oxide (In2O3), which can degrade FASs by generating photogenerated holes (h + ) instead of converting a large amount of H2O into hydroxyl radicals (·OH), thereby improving the degradation efficiency of PFASs.
[0005] In addition, the inventors have noticed that some researchers have obtained nano-photocatalytic materials with photoelectric properties of In2O3 modified by two-dimensional Mxene materials. For example, in the article "Research on the Performance of Ammonia Sensor Based on Two-Dimensional Mxene / In2O3 Composite Materials", researchers prepared a Ti3C2T x A composite material based on the two-dimensional Mxene material In2O3, which exhibits excellent sensitivity and selectivity to ammonia based on its specific micromorphology.
[0006] Inspired by this, the inventors tried to prepare a composite two-dimensional indium oxide-based catalyst for PFASs to solve the two problems that still exist when using In2O3 as a photocatalyst when PFASs are contaminated:
[0007] (1) In2O3 has a wide band gap and low solar energy utilization, which greatly limits the development and application of photocatalytic technology;
[0008] (2) The recombination process of photogenerated electrons and holes in a single In2O3 semiconductor is usually faster than the process of charge migration to the surface to react catalytically with pollutants. Therefore, the separation efficiency of photogenerated electron-hole pairs needs to be further improved. Summary of the invention
[0009] In order to achieve the above-mentioned purpose, the present invention designs a composite two-dimensional indium oxide-based catalyst, wherein In2O3 is modified by using a Ti3AlC2-based two-dimensional Mxene material, and an In2O3 / MXene material with a specific morphology is obtained by adjusting the preparation method and parameters. The In2O3 / MXene material as a catalyst not only bypasses the problem that ·OH cannot degrade PFASs, but also accelerates the transfer of conduction band electrons of In2O3 to the Mxene surface, thereby reducing the recombination rate of photogenerated electron-hole pairs, thereby showing significant selectivity and sensitivity to PFASs.
[0010] It is worth noting that the present invention does not protect the following prior art or existing discoveries:
[0011] 1) Basic design concept of In2O3 / Mxene series materials;
[0012] 2) Hole (h + ) and the role of hydroxyl radicals (·OH) themselves in photocatalytic degradation.
[0013] The focus of the present invention is:
[0014] An In2O3 / Mxene catalyst having the following precise microstructure, a precise method for preparing the catalyst, and substantial microstructural features of the catalyst and significant progress in solving practical problems.
[0015] 1. Composite two-dimensional indium oxide-based catalyst
[0016] The composite two-dimensional indium oxide-based catalyst designed by the present invention is an In2O3 / Mxene catalyst, and the catalytic structure of the In2O3 / Mxene catalyst includes a Schottky heterojunction consisting of an Mxene component and an In2O3 component uniformly loaded on the surface of the Mxene component, and the mass ratio of the Mxene component to the In2O3 component in the Schottky heterojunction is 1:10;
[0017] The Mxene component is Ti3AlC2 treated with HF, which is in the form of elliptical flakes with a long diameter ranging from 8 to 12 μm, a short diameter ranging from 5 to 7 μm, and a specific surface area of 60 to 80 cm 2 / g,
[0018] The In2O3 component is in the form of a lamellar straight-edged elliptical lamellar layer, with a major diameter ranging from 1 to 1.5 μm, a straight edge spacing ranging from 300 to 500 nm, a lamellar thickness ranging from 50 to 70 nm, and pores with a diameter ranging from 5 to 8 nm are evenly distributed on the surface of the In2O3 component;
[0019] The visible light absorption range of In2O3 / Mxene catalyst is 420-800nm, the bandgap is 2.50eV, and the fluorescence intensity is the highest at a wavelength of 473nm;
[0020] The active components of In2O3 / Mxene catalyst in the catalytic reaction are holes and hydroxyl radicals, denoted as h + and ·OH, in the evaluation system of the degree of action of active components + The weight of is higher than that of OH, and the judgment matrix is as follows:
[0021]
[0022] The weight of each indicator is determined by the hierarchical analysis method, and the value assignment scale is shown in Table 1:
[0023] Table 1 Evaluation scale of the model
[0024]
[0025] It should be noted that the numbers of the various indicators in the present invention do not represent the degree of importance, nor do they have a limiting meaning, but are only for making the description clearer.
[0026] Calculate the eigenvector W of the above matrix, that is:
[0027] h + The weight W h+ =8 / 9, OH weight W ·OH =1 / 9.
[0028] 2. Preparation method of composite two-dimensional indium oxide-based catalyst
[0029] The present invention also provides a method for preparing a composite two-dimensional indium oxide-based catalyst, comprising the steps of:
[0030] S1, preparing Mxene components;
[0031] After Ti3AlC2 is reacted with HF solution, filtered and washed, Mxene components are obtained;
[0032] S2, preparing In2O3 / Mxene catalyst by one-step hydrothermal method;
[0033] S2-1, dispersing a 300 mg / mL In(NO3)3·5H2O solution in a 70% mass concentration ethylene glycol solution and mixing them thoroughly to obtain suspension three;
[0034] S2-2, adding the Mxene component prepared in S1 to the three suspensions in S2-1 and mixing them thoroughly;
[0035] In S2-1 and S2-2, let n be the multiplication factor and n∈R + , the amount of In(NO3)3·5H2O solution added was 2n mL, the amount of ethylene glycol added was [10,40]n mL, and the amount of Mxene component added was [0.005,0.02] ng;
[0036] S2-3, reacting the suspension three at 180-200°C for 20-24h, cooling to room temperature, washing with alcohol and water until the washing liquid is neutral, and then drying at 60°C to obtain powder sample two;
[0037] S2-4, heating the powder sample 2 in S2-3 at a gradient temperature to obtain an In2O3 / Mxene catalyst;
[0038] The gradient temperature is as follows: first, the heating temperature is increased from room temperature to 100°C at a rate of 5-8°C / min, and kept at this temperature for 2-3min;
[0039] Then the temperature was increased from 100°C to 250°C at a rate of 10-12°C / min, and kept warm for 5-8min; secondly, the temperature was increased from 250°C to 400°C at a rate of 10-15°C / min, and kept warm for 1-2min; then, the temperature was increased from 400°C to 500°C at a rate of 15-17°C / min, and kept warm for 1.5-2h; finally, the temperature was cooled to room temperature with the furnace to obtain the In2O3 / Mxene catalyst.
[0040] Furthermore, the steps for preparing the Mxene component in S1 are:
[0041] S1-1, slowly add Ti3AlC2 into 40% HF solution, fully stir at room temperature to obtain suspension 1;
[0042] Let n be the multiplication coefficient and n∈R + , when the addition amount of Ti3AlC2 is 1ng, the addition amount of HF solution is [18,20]nmL;
[0043] S1-2, filtering the suspension in S1-1 to obtain a filter residue, washing the filter residue with deionized water until the pH of the washing solution is ≥6, and then drying the filter residue at 60°C for 2 to 3 hours to obtain a dry sample;
[0044] S1-3, disperse the dried sample in S1-1 in DMSO and stir well to obtain suspension 2; centrifuge suspension 2 to obtain filter residue, and wash with deionized water to obtain powder sample 1;
[0045] Let n be the multiplication coefficient and n∈R + , when the amount of dry sample added was 100 ng, the amount of DMSO added was [18,20] n mL;
[0046] S1-3. The powder sample 1 in S1-3 is dispersed in deionized water at a mass ratio of 1:100, and is subjected to ultrasonic and centrifugal treatment under N2 protection atmosphere to remove the stripped residues to obtain a supernatant of the Mxene component.
[0047] 3. Application of composite two-dimensional indium oxide-based catalysts
[0048] The present invention also provides the application of a composite two-dimensional indium oxide-based catalyst, using an In2O3 / Mxene catalyst to degrade PFASs.
[0049] See also Fig.15 In order to clarify the photocatalytic degradation mechanism of 0.01-In / Mxene heterojunction visible light catalyst, the conduction band and valence band positions of In2O3 were calculated by DRS data and obtained by the following formula:
[0050] E CB =XE e -0.5E g
[0051] E VB =E CB +E g
[0052] X represents the absolute electronegativity of the semiconductor, E e is the energy of a free electron calculated using the hydrogen standard, Eg is the band gap width, and E e The value is 4.5eV, and the bandgap is 2.62eV obtained from DRS data. By calculation, the conduction band and valence band positions of In2O3 are -0.02 and 2.64eV respectively.
[0053] exist Fig.15 In this paper, we combined the experimental and characterization results to infer the photocatalytic degradation mechanism. - The standard reduction potential of (-0.33 eV) is more negative, which means that the electrons in the conduction band have no ability to reduce O2 to O2 - At the same time, after being combined with Mxene, the transfer of conduction band electrons to the Mxene surface is promoted, thereby accelerating the separation rate of photogenerated electron-hole pairs. In addition, compared with the valence band potential of In2O3 and ·OH / H2O (2.27eV), it has sufficient oxidation capacity to oxidize H2O to ·OH. + It can directly react with PFOA to produce oxidation. Combined with the free radical activity experiment, the rate of ·OH and PFOA is lower than h + The reaction rate with PFOA is determined by h + .
[0054] In summary, the construction of multi-dimensional two-dimensional nanosheet In2O3 / nanosheet Mxene heterojunction visible light catalyst (0.01-In / Mxene) enables the material to have higher light utilization ability, faster charge generation and transfer ability, lower photogenerated electron-hole pair recombination rate, and excellent stability and renewable utilization rate. These characteristics greatly improve the photocatalytic activity of heterojunction visible light catalyst 0.01-In / Mxene.
[0055] Compared with the existing catalysts for degrading PFASs, the beneficial effects of the present invention are:
[0056] (1) The composite two-dimensional indium oxide-based catalyst with a Schottky heterojunction, i.e., the In2O3 / MXene catalyst, designed by the present invention adjusts the microscopic morphology of the catalyst so that the conduction band electrons of In2O3 in the catalyst can be accelerated to transfer to the MXene surface, thereby reducing the recombination rate of photogenerated electron-hole pairs.
[0057] (2) The In2O3 / MXene catalyst designed by the present invention has a core catalytic active component h + , rather than ·OH, thus solving the problem of low degradation efficiency of PFASs by ·OH. BRIEF DESCRIPTION OF THE DRAWINGS
[0058] Figure 1 is the XRD spectrum of the catalyst in Example 1;
[0059] Figure 2 This is the SEM spectrum of the flake In2O3 in Example 1;
[0060] Figure 3 is the SEM spectrum of Mxene in Example 1;
[0061] Figure 4 This is the SEM spectrum of In2O3 / Mxene in Example 1;
[0062] Figure 5 This is the EDS-mapping spectrum of In2O3 / Mxene in Example 1;
[0063] Figure 6 is the UV diffuse reflectance spectrum of the catalyst in the experimental example;
[0064] Figure 7 Bandgap spectrum of the catalyst in the experimental example;
[0065] Figure 8 is the fluorescence spectrum of the catalyst in the experimental example;
[0066] Fig. 9This is the photocatalytic activity diagram of the catalyst in the experimental example for degrading PFOA under visible light conditions;
[0067] Fig.10 is the kinetic curve of PFOA degradation by the catalyst under visible light conditions in the experimental example;
[0068] Fig.11 This is the experimental data diagram of the cyclic degradation of PFOA by 0.01-In / Mxene in the experimental example;
[0069] Fig.12 This is the effect spectrum of different quenchers on the PFOA degradation experiment of 0.01-In / Mxene sample;
[0070] Fig.13 The EPR spectra of superoxide radicals captured by DMPO in single In2O3 and 0.01-In / Mxene in PFOA;
[0071] Fig.14 The EPR spectra of hydroxyl radicals captured by DMPO in single In2O3 and 0.01-In / Mxene in PFOA;
[0072] Fig.15 It is a diagram of the degradation mechanism of the catalyst. DETAILED DESCRIPTION
[0073] In order to further illustrate the method adopted by the present invention and the effect achieved, the technical solution of the present invention will be clearly and completely described in combination with experiments below.
[0074] Example 1: This example describes a composite two-dimensional indium oxide-based catalyst.
[0075] The composite two-dimensional indium oxide-based catalyst is an In2O3 / Mxene catalyst. The catalytic structure of the In2O3 / Mxene catalyst includes a Mxene component and a Schottky heterojunction composed of an In2O3 component uniformly loaded on the surface of the Mxene component. The mass ratio of the Mxene component to the In2O3 component in the Schottky heterojunction is 1:10.
[0076] The Mxene component is Ti3AlC2 treated with HF, which is in the form of elliptical flakes with a long diameter ranging from 8 to 12 μm, a short diameter ranging from 5 to 7 μm, and a specific surface area of 60 to 80 cm 2 / g,
[0077] The In2O3 component is in the form of a lamellar straight-edged elliptical lamellar layer, with a major diameter ranging from 1 to 1.5 μm, a straight edge spacing ranging from 300 to 500 nm, a lamellar thickness ranging from 50 to 70 nm, and pores with a diameter ranging from 5 to 8 nm are evenly distributed on the surface of the In2O3 component;
[0078] The visible light absorption range of In2O3 / Mxene catalyst is 420-800nm, the band gap is 2.50eV, and the fluorescence intensity is highest at a wavelength of 473nm.
[0079] Example 2: This example describes the preparation method of the In2O3 / Mxene catalyst in Example 1.
[0080] S1, preparing Mxene components;
[0081] After Ti3AlC2 is reacted with HF solution, filtered and washed, Mxene components are obtained;
[0082] S1-1, slowly add Ti3AlC2 into 40% HF solution, fully stir at room temperature to obtain suspension 1;
[0083] When the addition amount of Ti3AlC2 is 1 g, the addition amount of HF solution is 18 mL;
[0084] S1-2, filtering the suspension in S1-1 to obtain a filter residue, washing the filter residue with deionized water until the pH of the washing solution is ≥6, and then drying the filter residue at 60°C for 2 to 3 hours to obtain a dry sample;
[0085] S1-3, disperse the dried sample in S1-1 in DMSO and stir well to obtain suspension 2; centrifuge suspension 2 to obtain filter residue, and wash with deionized water to obtain powder sample 1;
[0086] When the amount of dried sample added was 100 ng, the amount of DMSO added was 18 mL;
[0087] S1-3, dispersing the powder sample 1 in S1-3 in deionized water at a mass ratio of 1:100, and subjecting it to ultrasonic and centrifugal treatment under N2 protection atmosphere to remove the stripped residues to obtain the supernatant of the Mxene component;
[0088] S2, preparing In2O3 / Mxene catalyst by one-step hydrothermal method;
[0089] S2-1, dispersing In(NO3)3·5H2O solution with a concentration of X mg / mL in ethylene glycol solution with a mass concentration of 70% and mixing them thoroughly to obtain suspension three;
[0090] S2-2, adding the Mxene component prepared in S1 to the three suspensions in S2-1 and mixing them thoroughly;
[0091] In S2-1 and S2-2, the amount of In(NO3)3·5H2O solution added was 2 mL, the amount of ethylene glycol added was 20 mL, and the amount of Mxene component added was 0.01 g;
[0092] S2-3, reacting the suspension 3 at 180°C for 20h, cooling to room temperature, washing with alcohol and water until the washing liquid is neutral, and then drying at 60°C to obtain powder sample 2;
[0093] S2-4, heating the powder sample 2 in S2-3 at a gradient temperature to obtain an In2O3 / Mxene catalyst;
[0094] The gradient temperature is as follows: first, the heating temperature is increased from room temperature to 100°C at a rate of 5°C / min, and kept warm for 2 minutes; then, it is increased from 100°C to 250°C at a rate of 10°C / min, and kept warm for 5 minutes; secondly, it is increased from 250°C to 400°C at a rate of 10°C / min, and kept warm for 1 minute; then, it is increased from 400°C to 500°C at a rate of 15°C / min, and kept warm for 1.5 hours; finally, it is cooled to room temperature with the furnace to obtain the In2O3 / Mxene catalyst.
[0095] Example 3: The description basis of this example is the recording scheme in Example 2, and except for the following contents, the rest of the contents are the same.
[0096] S2, preparing In2O3 / Mxene catalyst by one-step hydrothermal method;
[0097] S2-1, dispersing a 300 mg / mL In(NO3)3·5H2O solution in a 70% mass concentration ethylene glycol solution and mixing them thoroughly to obtain suspension three;
[0098] S2-2, adding the Mxene component prepared in S1 to the three suspensions in S2-1 and mixing them thoroughly;
[0099] In S2-1 and S2-2, the amount of In(NO3)3·5H2O solution added was 2 mL, the amount of ethylene glycol added was 20 mL, and the amount of Mxene component added was 0.005 g.
[0100] Example 4: The description basis of this example is the recording scheme in Example 2, and except for the following contents, the rest of the contents are the same.
[0101] S2, preparing In2O3 / Mxene catalyst by one-step hydrothermal method;
[0102] S2-1, dispersing a 300 mg / mL In(NO3)3·5H2O solution in a 70% mass concentration ethylene glycol solution and mixing them thoroughly to obtain suspension three;
[0103] S2-2, adding the Mxene component prepared in S1 to the three suspensions in S2-1 and mixing them thoroughly;
[0104] In S2-1 and S2-2, the amount of In(NO3)3·5H2O solution added was 2 mL, the amount of ethylene glycol added was 20 mL, and the amount of Mxene component added was 0.02 g.
[0105] Example 5: The description of this example is based on the content described in Example 2, and is intended to illustrate the preparation method of In2O3 / Mxene catalyst under another parameter.
[0106] S1, preparing Mxene components;
[0107] After Ti3AlC2 is reacted with HF solution, filtered and washed, Mxene components are obtained;
[0108] S1-1, slowly add Ti3AlC2 into 40% HF solution, fully stir at room temperature to obtain suspension 1;
[0109] When the addition amount of Ti3AlC2 is 1 g, the addition amount of HF solution is 20 mL;
[0110] S1-2, filtering the suspension in S1-1 to obtain a filter residue, washing the filter residue with deionized water until the pH of the washing solution is ≥ 6, and then drying the filter residue at 60° C. for 3 h to obtain a dry sample;
[0111] S1-3, disperse the dried sample in S1-1 in DMSO and stir well to obtain suspension 2; centrifuge suspension 2 to obtain filter residue, and wash with deionized water to obtain powder sample 1;
[0112] When the amount of dry sample added is 100 g, the amount of DMSO added is 20 mL;
[0113] S1-3, dispersing the powder sample 1 in S1-3 in deionized water at a mass ratio of 1:100, and subjecting it to ultrasonic and centrifugal treatment under N2 protection atmosphere to remove the stripped residues to obtain the supernatant of the Mxene component;
[0114] S2, preparing In2O3 / Mxene catalyst by one-step hydrothermal method;
[0115] S2-1, dispersing a 300 mg / mL In(NO3)3·5H2O solution in a 70% mass concentration ethylene glycol solution and mixing them thoroughly to obtain suspension three;
[0116] S2-2, adding the Mxene component prepared in S1 to the three suspensions in S2-1 and mixing them thoroughly;
[0117] In S2-1 and S2-2, the amount of In(NO3)3·5H2O solution added was 2 mL, the amount of ethylene glycol added was 40 mL, and the amount of Mxene component added was 0.01 g;
[0118] S2-3, reacting the suspension 3 at 200°C for 24h, cooling to room temperature, washing with alcohol and water until the washing liquid is neutral, and then drying at 60°C to obtain powder sample 2;
[0119] S2-4, heating the powder sample 2 in S2-3 at a gradient temperature to obtain an In2O3 / Mxene catalyst;
[0120] The gradient temperature is as follows: first, the heating temperature is increased from room temperature to 100°C at a rate of 8°C / min, and kept warm for 3 minutes; then, it is increased from 100°C to 250°C at a rate of 12°C / min, and kept warm for 8 minutes; secondly, it is increased from 250°C to 400°C at a rate of 15°C / min, and kept warm for 2 minutes; then, it is increased from 400°C to 500°C at a rate of 17°C / min, and kept warm for 2 hours; finally, it is cooled to room temperature with the furnace to obtain the In2O3 / Mxene catalyst.
[0121] Example 6: The description of this example is based on the contents recorded in Example 5, and is intended to illustrate the preparation method of In2O3 / Mxene catalyst under another parameter. Except for the following contents, the rest of the contents are the same.
[0122] S2-1, dispersing a 300 mg / mL In(NO3)3·5H2O solution in a 70% mass concentration ethylene glycol solution and mixing them thoroughly to obtain suspension three;
[0123] S2-2, adding the Mxene component prepared in S1 to the three suspensions in S2-1 and mixing them thoroughly;
[0124] In S2-1 and S2-2, the amount of In(NO3)3·5H2O solution added was 2 mL, the amount of ethylene glycol added was 10 mL, and the amount of Mxene component added was 0.01 g.
[0125] Experimental Example: The description of this experimental example is based on the scheme described in Example 1, and is intended to illustrate the practical application effect of the present invention.
[0126] 1. Experimental reagents: The main materials, reagents and instruments used in this experiment are shown in Tables 2 and 3 below.
[0127] Table 2 Experimental materials and reagents
[0128]
[0129]
[0130] Table 3 Experimental instruments
[0131]
[0132] 2. Characterization methods of sample physicochemical properties
[0133] 2.1 Experimental Design
[0134] The composition, crystal structure and purity of the material were analyzed by Shimadzu XRD-6000 X-ray diffractometer (XRD), with an operating voltage of 40kV, a current of 30mA, and a Cu Kα X-ray generator. The morphology and microscopic element distribution of the material were analyzed by electron scanning microscope (SEM, QUANTA FEG 250). At room temperature, BaSO4 was used as a standard reference, and the light absorption performance of the material was analyzed by solid ultraviolet spectrophotometer (DRS, UV-3600), with a scanning range of 200 to 800nm. The photogenerated carrier separation ability was tested by a 3-22 fluorescence spectrometer (PL) manufactured by Horiba, with an excitation wavelength of 320nm.
[0135] 2.2 Component Characterization
[0136] See also Figure 1 XRD is usually used to analyze the crystal structure of samples and the purity of their phases. The peaks of In2O3 spectrum at 22.50°, 30.59°, 35.46° and 51.02° correspond to (211), (222), (400) and (440) crystal planes, respectively, which are consistent with the peaks of cubic In2O3 standard card JCPDS No.71-2195. In the Mxene spectrum, the peak at 39.2° disappeared, and 28.23°(008) and 37.30°(103) were detected, indicating that Mxene was successfully prepared.
[0137] For In2O3 / Mxene, compared with the characteristic diffraction peak of Bi2MoO6, the peak position of the XRD spectrum after Mxene composite did not change significantly. However, with the continuous increase of Mxene doping, the characteristic peak intensity of the heterojunction photocatalyst In2O3 / Mxene continued to decrease. This shows that after Mxene doping, the structural crystal form of In2O3 is not affected. However, the peak of Mxene was not detected in RGO / Bi2MoO6, which may be due to the low quality and high dispersion of the composite.
[0138] 2.3 Morphological and structural characterization
[0139] Experimental design: SEM spectra and EDS-mapping images of In2O3, Mxene and In2O3 / Mxene samples are shown in Figure 2 to Figure 5 As shown, the morphology of In2O3 is an elliptical nanosheet structure ( Figure 2 ), from the figure, we can also find that there are certain pores on the surface of the flake In2O3 and the size is about 5 to 8nm. Figure 3 and 4 , Mxene presents a two-dimensional nanosheet, In2O3 is tightly loaded on the surface of Mxene, ensuring that In2O3 is well dispersed and fully in contact with Mxene. In order to further analyze the elemental composition and distribution of the sample In2O3 / Mxenei, the sample was subjected to EDS-mapping spectrum analysis (see Figure 5 ), In, O, Ti, and C are evenly distributed on In2O3 / Mxene, which shows that Mxene is well composited with In2O3, which is beneficial to the charge transfer between In2O3 and Mxene.
[0140] 2.4. Photoelectrochemical performance characterization
[0141] The photoelectric properties of photocatalytic materials directly affect their photocatalytic performance. Therefore, in order to investigate the changes in the photoelectric properties of the composite photocatalyst In2O3 / Mxene after doping with Mxene, we analyzed and studied it through UV diffuse reflectance and fluorescence spectroscopy characterization.
[0142] The ability of photocatalysts to utilize light directly affects the performance of photocatalysts. Figure 6It is the UV-visible absorption spectra of single In2O3, Mxene and In2O3 / Mxene in the wavelength range of 200-800nm. Pure Mxene has good optical absorption in both the UV and visible light regions, while the optical absorption intensity of single In2O3 in the visible light region is not high. It is worth noting that the spectrum of the sample after In2O3 and Mxene composite is red-shifted and the light response ability in the visible light region is greatly improved. With the increase of Mxene doping amount, the visible light response ability of the composite sample Mxene / In2O3 first increases and then weakens. The sample 0.01-In / Mxene shows the best visible light response ability. This may be because with the enhancement of Mxene samples, the establishment of heterojunctions enhances the interaction between the two, which increases the light absorption ability. However, too much Mxene weakens its contact with In2O3, which hinders light absorption. In addition, the energy band calculation of the semiconductor is calculated according to the Kubelka-Munk equation to further evaluate the light absorption response ability of the photocatalyst:
[0143] αhν=A(hν-Eg) n
[0144] It has been reported that In2O3 is a direct semiconductor, so n = 0.5. The bandgap calculation results of flake In2O3 and composite sample In2O3 / Mxene are as follows: Figure 7 . The bandgap of In2O3 is 2.62eV. The bandgap of the composite samples has decreased to a certain extent. The bandgap of the composite photocatalysts with different Mxene doping amounts is ranked from large to small as follows: 0.005-In / Mxene>0.02-In / Mxene>0.01-In / Mxene. The smaller the bandgap, the stronger its ability to absorb visible light. The above results show that the composite heterojunction photocatalyst 0.01-In / Mxene has excellent light absorption response ability in the visible light region, which will be beneficial to the rate of generating photogenerated electron-hole pairs under visible light conditions, thereby improving the photocatalytic activity.
[0145] In the photocatalytic process, the separation efficiency of photogenerated electrons and holes will also have a great influence on the photocatalytic activity. Therefore, we analyzed the separation of photogenerated carriers in the samples through the fluorescence spectrum and fluorescence lifetime of the samples (see Figure 8 ). Figure 8 In the results, the fluorescence intensity of single In2O3 is higher than that of the composite sample In2O3 / Mxene. In addition, the fluorescence intensity of the composite photocatalyst In2O3 / Mxene with different Mxene doping amounts is different, among which the fluorescence intensity of the 0.01-In / Mxene sample is the lowest. The lower the fluorescence intensity, the lower the recombination rate of photogenerated carriers of the sample.
[0146] Therefore, the above results show that the composite of Mxene in the heterojunction photocatalyst In2O3 / Mxene enables the sample to have better light utilization to promote the generation and transfer of photogenerated electron-hole pairs, so as to effectively suppress the recombination of photogenerated carriers. In addition, as a good conductor of electrons, Mxene is like a high-speed channel that promotes the transfer of photogenerated electrons from In2O3 to its surface. If the doping amount of Mxene is too little, the excess In2O3 surface electrons cannot be effectively transferred, and if the doping amount of Mxene is too much, it will lead to a reduction in In2O3 per unit mass, thereby affecting the generation of photogenerated electron-hole pairs. Therefore, 0.01-In / Mxene better guarantees the generation and separation of photogenerated carriers compared to other composite samples.
[0147] 3. Photocatalytic activity test experiment
[0148] Experimental design: The photocatalytic reactor includes: light source, quartz cold trap, filter device, multi-test tube stirring device, rotating device, etc. The light source is placed in a dedicated quartz cold trap, and cooling water is passed through to cool down. PFOA is used as a target pollutant to evaluate the activity of the prepared photocatalytic material. During the experiment, 50 mg of photocatalytic material was added to a 50 mL quartz tube with an initial concentration of 10 ppm of PFOA. Before illumination, magnetic stirring was performed for 60 min under dark conditions to ensure that the reactants and catalysts reached adsorption-desorption equilibrium. About 1.5 mL of sample and 10 mL of sample were taken at intervals, filtered with a 0.22 μm filter membrane to remove solid particles, and the filtrate was collected for concentration detection and intermediate product analysis. In order to investigate the stability of the sample, the material after the photocatalytic degradation experiment was centrifuged, washed and dried, and then recycled for a cycle experiment. The experimental results were obtained through more than 5 parallel experiments.
[0149] Pure In2O3 and Mxene were used as control experiments to compare the visible light photocatalytic activities of the samples before and after the composite (see Fig. 9 ). The degradation efficiency of PFOA by single Mxene and In2O3 under visible light irradiation for 3 hours can only reach 17.4% and 47.7%, while the degradation efficiency of heterojunction photocatalyst In2O3 / Mxene doped with different amounts of Mxene is significantly improved compared with them. Among them, the degradation efficiency of 0.01-In / Mxene sample can reach 74.2%. By comparing heterojunction photocatalysts with different Mxene doping amounts, the effect of Mxene content on the photocatalytic performance of the samples was analyzed. It can be clearly seen from Fig. 9It was found that with the continuous increase of Mxene content, the photocatalytic degradation efficiency of the sample first increased and then decreased. The photocatalytic degradation efficiency of the sample 0.01-In / Mxene was the highest. This result shows that the Mxene doping amount has an important influence on the composite sample. Too much or too little Mxene content is not conducive to improving the photocatalytic efficiency. When the Mxene content is too little, the carrier capture sites are reduced and the carrier existence life is shortened, which affects the improvement of the photocatalytic efficiency; and when the Mxene content is too much, it will not only fail to significantly increase the absorption capacity of visible light, but also cause In2O3 to agglomerate on the Mxene surface, which is not conducive to the formation of heterojunction.
[0150] According to the Langmuir-Hinshelwood model, the reaction of the sample's visible light degradation of PFOA conforms to the pseudo-first-order kinetic equation:
[0151] ln(C0 / C)=k app t
[0152] See also Fig.10 Therefore, the photocatalytic degradation reaction time t and ln(C0 / C) show a good linear relationship. Fig.10 The k of the prepared samples was compared app Obviously, the sample 0.01-In / Mxene has the highest k app Value(0.00719min -1 ). app The higher the value, the higher the photocatalytic degradation activity of the sample. app The photocatalytic degradation activity of the prepared samples is arranged from large to small according to the values: 0.01-In / Mxene>0.02-In / Mxene>0.005-In / Mxene>In2O3>Mxene. In summary, the loading amount of Mxene plays an important role in improving the photocatalytic activity. Compared with other samples, 0.01-In / Mxene showed the highest photocatalytic activity.
[0153] The stability and reusability of photocatalysts are important factors in determining whether they have practical application prospects. Therefore, we used the visible light photocatalyst 0.01-In / Mxene to photocatalytically degrade naphthalene, centrifuged, washed, and dried the sample, and repeated the experiment for 5 cycles under the same conditions. We found that the 0.01-In / Mxene sample still maintained good stability and high degradation activity after repeated experiments (see Fig.11 The degradation efficiency after the fifth cycle experiment was slightly lower than that of the first experiment, which may be due to a certain amount of loss in the process of collecting the photocatalyst. This result shows that the heterojunction visible light photocatalyst 0.01-In / Mxene has good stability and reusability.
[0154] 4. Free radical active species determination experiment
[0155] Experimental design: In order to investigate the contribution and influence of different free radicals on the degradation efficiency during the photocatalytic reaction, nitroxide free radicals piperidinol (TEMPOL), isopropyl alcohol (IPA) and ammonium oxalate (AO) were used as superoxide free radicals (·O 2- ), hydroxyl radicals (·OH) and holes (h + ) was added into the degradation reaction solution to carry out the active species quenching experiment.
[0156] The electron paramagnetic resonance (EPR) spectra of the samples dispersed in water and ethanol were measured by Bruker model ESR JES-FA200 spectrophotometer using DMPO, a spin quenching reagent from Sigma, at room temperature under 1000 W xenon lamp illumination.
[0157] In the process of photocatalytic degradation, the main active species are ·OH, ·O2 - and h + , among which one or more active substances may play a role in the photocatalytic oxidation process. In this study, TEMPOL, AO and IPA were selected as ·O2 - ,h + The experiment without quencher was used as a comparative experiment. After adding the quencher, the more the photocatalytic degradation efficiency is reduced, the greater the effect of the active species captured by the quencher on the photocatalytic reaction. Fig.12 It is not difficult to find that after adding OA, the photocatalytic degradation activity of 0.01-In / Mxene is greatly inhibited. After adding IPA, the photocatalytic degradation activity is inhibited to a certain extent; when TEMPOL is added, the photocatalytic efficiency is not greatly affected, which shows that h + Both ·OH and ·OH play a role in the photocatalytic reaction. + Play a major role.
[0158] In order to further analyze the active substances that play a role in the photocatalytic reaction, the free radical EPR experiment captured by DMPO analyzed the free radicals generated by the sample during the photocatalytic process. First, as a blank control, the EPR data was tested in a dark reaction system and a light-added but no catalyst system, and no signal was measured, which ruled out the possibility of free radicals in the dark reaction and pure solvent. Fig.13 and Fig.14 In the figure, we can see that under visible light conditions, 0.01-In / Mxene and single In2O3 were not detected in PFOA. -In addition, ·OH radicals were detected in the PFOA reaction solution, but the signal of single In2O3 was significantly stronger than that of 0.01-In / Mxene. This phenomenon may be due to the fact that ·OH is not the main active species in the photocatalytic reaction of PFOA degradation, and the compound accelerates the h + The generation of h + It is easier to react with PFOA, which confirms that ·OH and h + are the main active species in the photocatalytic reaction process, but h + is the main active species.
[0159] In summary, the following inferences can be drawn: the active component of the In2O3 / Mxene catalyst in the catalytic reaction is h + and ·OH, and in the evaluation system of the degree of action of active components h + The weight of is higher than that of ·OH.
[0160] The hole h in the evaluation system for determining the degree of action of the active component + The weights of and OH, the judgment matrix is as follows:
[0161]
[0162] Calculate the eigenvector W of the above matrix, that is:
[0163] h + The weight W h+ =8 / 9, OH weight W ·OH =1 / 9.
Claims
1. A composite two-dimensional indium oxide-based catalyst, characterized in that: The composite two-dimensional indium oxide-based catalyst is an In2O3 / Mxene catalyst, and the catalytic structure of the In2O3 / Mxene catalyst includes an Mxene component and a Schottky heterojunction composed of an In2O3 component uniformly loaded on the surface of the Mxene component, and the mass ratio of the Mxene component to the In2O3 component in the Schottky heterojunction is 1:10; The Mxene component is Ti3AlC2 treated with HF, in the form of an elliptical sheet, with a long diameter ranging from 8 to 12 μm, a short diameter ranging from 5 to 7 μm, and a specific surface area of 60 to 80 m 2 / g, The In2O3 component is in the form of a lamellar straight-edged elliptical lamellar, with a major diameter ranging from 1 to 1.5 μm, a straight edge spacing ranging from 300 to 500 nm, a lamellar thickness ranging from 50 to 70 nm, and pores with a diameter ranging from 5 to 8 nm are evenly distributed on the surface of the In2O3 component; The In2O3 / Mxene catalyst has a visible light absorption range of 420 to 800 nm, a bandgap of 2.50 eV, and a maximum fluorescence intensity at a wavelength of 473 nm. The active components of the In2O3 / Mxene catalyst in the catalytic reaction are holes and hydroxyl radicals, denoted by h + and ·OH, in the evaluation system of the degree of action of active components + The weight of is higher than that of ·OH.
2. A composite two-dimensional indium oxide-based catalyst according to claim 1, characterized in that: h in the evaluation system for determining the extent of action of the active component + The weights of and OH, the judgment matrix is as follows: Calculate the eigenvector W of the above matrix, that is: h + The weight W h+ =8 / 9, OH weight W ·OH =1 / 9.
3. The method for preparing a composite two-dimensional indium oxide-based catalyst according to claim 1, characterized in that: Includes steps: S1, preparing Mxene components; After Ti3AlC2 is reacted with HF solution, filtered and washed, Mxene components are obtained; S2, preparing In2O3 / Mxene catalyst by one-step hydrothermal method; S2-1, dispersing a 300 mg / mL In(NO3)3·5H2O solution in a 70% mass concentration ethylene glycol solution and mixing them thoroughly to obtain suspension three; S2-2, adding the Mxene component prepared in S1 to the three suspensions in S2-1 and mixing them thoroughly; In S2-1 and S2-2, let n be the multiplication factor and n∈R + , the amount of In(NO3)3·5H2O solution added was 2n mL, the amount of ethylene glycol added was [10,40]n mL, and the amount of Mxene component added was [0.005,0.02] ng; S2-3, reacting the suspension three at 180-200°C for 20-24h, cooling to room temperature, washing with alcohol and water until the washing liquid is neutral, and then drying at 60°C to obtain powder sample two; S2-4, heating the powder sample 2 described in S2-3 at a gradient temperature to obtain an In2O3 / Mxene catalyst; The gradient temperature is: firstly, the heating temperature is increased from room temperature to 100°C at a rate of 5-8°C / min, and then kept at this temperature for 2-3 min; then increase the temperature from 100°C to 250°C at a rate of 10-12°C / min, and keep it warm for 5-8min; secondly increase the temperature from 250°C to 400°C at a rate of 10-15°C / min, and keep it warm for 1-2min; then increase the temperature from 400°C to 500°C at a rate of 15-17°C / min, and keep it warm for 1.5-2h; finally cool it to room temperature with the furnace to obtain In2O3 / Mxene catalyst.
4. The method for preparing a composite two-dimensional indium oxide-based catalyst according to claim 3, characterized in that: The steps for preparing the Mxene component in S1 are: S1-1, slowly add Ti3AlC2 into 40% HF solution, fully stir at room temperature to obtain suspension 1; Let n be the multiplication coefficient and n∈R + , when the addition amount of Ti3AlC2 is 1ng, the addition amount of HF solution is [18,20]nmL; S1-2, filtering the suspension in S1-1 to obtain a filter residue, washing the filter residue with deionized water until the pH of the washing solution is ≥6, and then drying the filter residue at 60°C for 2 to 3 hours to obtain a dry sample; S1-3, dispersing the dried sample in S1-1 in DMSO and stirring well to obtain suspension 2; centrifuging the suspension 2 to obtain a filter residue, and washing it with deionized water to obtain powder sample 1; Let n be the multiplication coefficient and n∈R + , when the amount of dry sample added was 100 ng, the amount of DMSO added was [18,20] n mL; S1-3. The powder sample 1 described in S1-3 is dispersed in deionized water at a mass ratio of 1:100, and is subjected to ultrasonic and centrifugal treatment under N2 protection atmosphere to remove the stripped residues to obtain a supernatant of the Mxene component.
5. The use of a composite two-dimensional indium oxide-based catalyst as claimed in claim 1, characterized in that: The In2O3 / Mxene catalyst is used to degrade PFASs.