Preparation method for morphology control of solvent-induced carbon nitride photocatalytic material

Through solvent-induced CN dots self-assembly technology, carbon nitride photocatalysts with various morphologies are prepared, which solves the problem of photocatalyst morphology control in the existing technology and achieves efficient degradation of new pollutants, especially in tetracycline hydrochloride. It exhibits excellent catalytic performance in degradation.

CN118767966AActive Publication Date: 2024-10-15JIANGXI MODERN POLYTECHNIC COLLEGE
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202410848470.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-27
Publication Date
2024-10-15
Estimated Expiration
2044-06-27

AI Technical Summary

Technical Problem

Existing photocatalyst morphology control technology is difficult to effectively improve its light absorption capacity and selectivity, affecting the separation and transfer process of photogenerated electron-hole pairs, and photocatalysts with different morphologies show different performances in catalytic reactions.

Method used

By inducing the self-assembly of CN dots in different solvents, carbon nitride photocatalysts with different morphologies such as unidimensional sea urchin-like, one-dimensional nanonecklace, one-dimensional nanowire, and two-dimensional nanosheets were prepared, and their morphology was controlled by solvent treatment and calcination steps. , achieving fine control of morphology.

Benefits of technology

Photocatalysts with different morphologies with high catalytic performance were successfully controlled for the degradation of new pollutants, especially in the degradation of tetracycline hydrochloride, which showed good catalytic effects, simple operation and controllable morphology.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118767966A_ABST
    Figure CN118767966A_ABST
Patent Text Reader

Abstract

The invention relates to a preparation method for morphology regulation of a solvent-induced carbon nitride photocatalytic material, which comprises the following steps: S1, preparation of CN dots: fully grinding melamine and alkali into mixed powder, sintering, and cooling to obtain a sintered product; adding the sintered product into high-purity water, carrying out dialysis treatment, evaporating water to dryness, and collecting solid powder, so as to obtain the quantum dots CN dots; s2, performing solvent-induced morphology regulation and control: dispersing the obtained quantum dots CN dots into high-purity water; and respectively treating the quantum dot solution by using different solvents, collecting solids, calcining, and cooling to obtain the carbon nitride quantum dot photocatalysts with different morphologies. Different solvents are ingeniously utilized, different morphologies of quantum dots are successfully induced, and the quantum dot photocatalysts with four different morphologies including a three-dimensional sea urchin shape, a one-dimensional nano necklace, a one-dimensional nanowire and a two-dimensional nanosheet are obtained through respective induction and regulation of the four different solvents.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of photocatalysts, and in particular to a preparation method for regulating the morphology of a solvent-induced carbon nitride photocatalytic material. Background Art

[0002] As people pay more and more attention to new pollutants, the degradation of new pollutants has become an important research direction in the field of environment. Photocatalysis, as a green and advanced oxidation technology, is highly favored in the degradation of new pollutants. The performance of photocatalysts plays a vital role in the photocatalytic degradation process.

[0003] The morphology of photocatalysts has an important influence on catalytic performance. Morphology regulation can affect the surface area and light absorption capacity of photocatalysts, thereby affecting the separation and transfer process of photogenerated electron-hole pairs and the exposure of surface active sites. In addition, photocatalysts with different morphologies may have different crystal plane structures and surface energy levels, which will affect the reaction selectivity of the catalyst. Therefore, by carefully designing and regulating the morphology of photocatalysts, the light absorption capacity, activity and selectivity can be effectively improved, thereby improving the photocatalytic performance. Summary of the invention

[0004] In view of the problems existing in the prior art, the purpose of the present invention is to provide a preparation method for controlling the morphology of quantum dots (CN dots) photocatalysts, which obtains catalysts with different morphologies by inducing CN dots self-assembly through different solvents.

[0005] The purpose of the present invention is achieved by the following technical solutions:

[0006] In a first aspect, the present invention provides a method for preparing a carbon nitride carbon nitride quantum dot photocatalyst by controlling its morphology, comprising the following steps:

[0007] S1. Preparation of CN dots:

[0008] Mixing melamine and alkali in a mortar, grinding them fully into mixed powder, then sintering the mixed powder, and cooling it to obtain a sintered product;

[0009] The sintered product is added to high-purity water, dispersed and dissolved, and the filtrate is collected by filtration. The filtrate is dialyzed. After the dialysis is completed, the water is evaporated and the solid powder is collected to obtain quantum dots CN dots;

[0010] S2. Solvent-induced morphology regulation:

[0011] The obtained quantum dots CN dots are dispersed in high-purity water to obtain a quantum dot solution; different solvents such as glacial acetic acid, methanol, ethanol, and isopropanol are used to treat the quantum dot solution respectively, and after the solvent treatment, the solid is dried to obtain different precursors;

[0012] The different precursors are calcined under a protective gas, and after cooling, carbon nitride photocatalysts with different morphologies are obtained.

[0013] Preferably, in step S1, the alkali comprises potassium hydroxide and sodium hydroxide, and the mass ratio of potassium hydroxide to sodium hydroxide is 1.12:0.4.

[0014] Preferably, in step S1, the mass ratio of melamine to alkali is 3:1.52.

[0015] Preferably, in the step S1, the sintering is carried out in a muffle furnace, the sintering temperature is 300° C., the sintering time is 2 h, and the heating rate is 5° C. / min.

[0016] Preferably, in step S1, the mass volume ratio of melamine to high-purity water is 3 g:100 mL.

[0017] Preferably, in step S1, the dialysis treatment is performed in high-purity water, the dialysis time is 24 hours, and the high-purity water is changed every 6 hours.

[0018] Preferably, in step S1, the dialysis membrane is a 3.5 kD dialysis membrane.

[0019] Preferably, in the step S2, the mass volume ratio of CN dots to high purity water is 100 mg: 20 mL

[0020] Preferably, in the step S2, the solvent treatment refers to mixing the solvent with the quantum dot solution, and performing freeze-drying treatment after the solution forms a gel, or, separating the bottom material after standing for 2 hours and then performing freeze-drying treatment.

[0021] Preferably, in step S2, the volume ratio of glacial acetic acid to quantum dot solution is 3 mL:200 μL.

[0022] Preferably, in step S2, the volume ratio of methanol to quantum dot solution is 2 mL:2 mL.

[0023] Preferably, in step S2, the volume ratio of ethanol to quantum dot solution is 2 mL:2 mL.

[0024] Preferably, in step S2, the volume ratio of isopropanol to quantum dot solution is 2 mL:2 mL.

[0025] Preferably, in step S2, the calcination treatment is carried out in a tubular furnace at 300° C. for 2 h, with a heating rate of 5° C. / min, and the protective gas is argon.

[0026] In a second aspect, the present invention provides a carbon nitride photocatalyst with different morphologies, which is prepared by the above-mentioned preparation method.

[0027] In a third aspect, the present invention provides an application of a carbon nitride photocatalyst with different morphologies in photocatalytic degradation of tetracycline hydrochloride.

[0028] The beneficial effects of the present invention are:

[0029] 1. The method of the present invention can be controlled to prepare carbon nitride photocatalysts with different morphologies. The present invention cleverly uses different solvents to successfully induce different morphologies of quantum dots. Different solvents are induced to obtain photocatalysts with four different morphologies: one-dimensional sea urchin, one-dimensional nanonecklace, one-dimensional nanowire, and two-dimensional nanosheet.

[0030] 2. The method for controlling the morphology of the carbon nitride photocatalyst of the present invention is simple to operate and has controllable morphology; the photocatalyst obtained by control has high catalytic performance. The photocatalyst provided by the present invention can be used to degrade new pollutants and has broad prospects in the field of degradation of new pollutants. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] The present invention is further described using the accompanying drawings, but the embodiments in the accompanying drawings do not constitute any limitation to the present invention. A person skilled in the art can obtain other drawings based on the following drawings without creative work.

[0032] Figure 1 is a scanning electron microscope photograph of the morphology of quantum dots prepared in Example;

[0033] Figure 2 This is a scanning electron microscope image of the morphology of sample B (three-dimensional sea urchin shape) prepared in Example 1;

[0034] Figure 3 is a scanning electron microscope image of the morphology of sample C (one-dimensional nanonecklace) prepared in Example 2;

[0035] Figure 4 is a scanning electron microscope image of the morphology of sample D (one-dimensional nanowire) prepared in Example 3;

[0036] Figure 5 is a scanning electron microscope image of the morphology of sample E (two-dimensional nanosheet) prepared in Example 4;

[0037] Figure 6 This is a performance test chart of quantum dot photocatalysts with different morphologies for photocatalytic degradation of tetracycline hydrochloride under visible light (wavelength greater than 420nm). DETAILED DESCRIPTION

[0038] The technical solution of the present invention is described below through specific examples. It should be understood that the one or more method steps mentioned in the present invention do not exclude the existence of other method steps before and after the combination step or the insertion of other method steps between these explicitly mentioned steps; it should also be understood that these embodiments are only used to illustrate the present invention and are not used to limit the scope of the present invention. Moreover, unless otherwise specified, the numbering of each method step is only a convenient tool for identifying each method step, and is not intended to limit the order of arrangement of each method step or to limit the scope of the present invention. The change or adjustment of the relative relationship thereof shall also be regarded as the scope of the present invention without substantially changing the technical content.

[0039] In order to better understand the above technical scheme, the exemplary embodiments of the present invention are described in more detail below. Although exemplary embodiments of the present invention are shown, it should be understood that the present invention can be implemented in various forms and should not be limited by the embodiments set forth herein. On the contrary, these embodiments are provided in order to enable a more thorough understanding of the present invention and to enable the scope of the present invention to be fully communicated to those skilled in the art.

[0040] The high-purity water used in the present invention refers to water with a conductivity of less than 0.1 μs / cm and a residual salt content of less than 0.3 mg / L at 25° C., and water from which non-dielectric impurities such as trace bacteria, microorganisms, and particles have been removed.

[0041] The present invention will be further described below in conjunction with the following examples.

[0042] Example 1

[0043] A preparation method for solvent-induced carbon nitride photocatalytic material morphology regulation comprises the following steps:

[0044] S1. Preparation of quantum dots (CN dots):

[0045] Weigh 3g of melamine, 1.12g of KOH and 0.4g of NaOH in a mortar and grind them into powder. Then add the evenly ground powder into a 50mL crucible, cover it with a lid, and place it in a muffle furnace for calcination at 300℃ for 2h. The heating rate is set to 5℃ / min. After the crucible cools to room temperature, take it out and disperse the material in the crucible into 100mL of high-purity water. After the material is fully dissolved, filter it to obtain a yellow filtrate. The yellow filtrate is added to a 3.5kD dialysis membrane and sealed, and dialyzed in high-purity water for 24h. The high-purity water is changed every 6h; finally, the dialyzate is poured into a beaker, placed in an oven at 80℃ to evaporate the water, and the powder at the bottom is collected to obtain quantum dots CN dots.

[0046] S2, solvent-induced self-assembly:

[0047] (1) Dispersing 100 mg of CN dots in 20 mL of high-purity water to obtain CN dots dispersion A;

[0048] (2) Take 3 mL of dispersion A in a 5 mL centrifuge tube, add 200 μL of glacial acetic acid, and freeze-dry the solution after it forms a gel to obtain a dehydrated sample B (three-dimensional sea urchin-like morphology);

[0049] (3) The collected sample B was calcined in a tube furnace at 300°C for 2 h with a heating rate of 5°C / min and Ar gas protection; after naturally cooling to room temperature, the corresponding samples were collected.

[0050] Example 2

[0051] A preparation method for solvent-induced carbon nitride photocatalytic material morphology regulation comprises the following steps:

[0052] S1. Preparation of quantum dots (CN dots):

[0053] Weigh 3g of melamine, 1.12g of KOH and 0.4g of NaOH in a mortar and grind them into powder. Then add the evenly ground powder into a 50mL crucible, cover it with a lid, and place it in a muffle furnace for calcination at 300℃ for 2h. The heating rate is set to 5℃ / min. After the crucible cools to room temperature, take it out and disperse the material in the crucible into 100mL of high-purity water. After the material is fully dissolved, filter it to obtain a yellow filtrate. The yellow filtrate is added to a 3.5kD dialysis membrane and sealed, and dialyzed in high-purity water for 24h. The high-purity water is changed every 6h; finally, the dialyzate is poured into a beaker, placed in an oven at 80℃ to evaporate the water, and the powder at the bottom is collected to obtain quantum dots CN dots.

[0054] S2, solvent-induced self-assembly:

[0055] (1) Dispersing 100 mg of CN dots in 20 mL of high-purity water to obtain CN dots dispersion A;

[0056] (2) Take a 5 mL centrifuge tube and add 2 mL of methanol, then gradually add 2 mL of dispersion A into it, stand for 2 h, separate the bottom material, freeze-dry, and obtain sample C (one-dimensional nanonecklace);

[0057] (3) The collected sample C was calcined in a tube furnace at 300°C for 2 h with a heating rate of 5°C / min and Ar gas protection; after naturally cooling to room temperature, the corresponding sample was collected.

[0058] Example 3

[0059] A preparation method for solvent-induced carbon nitride photocatalytic material morphology regulation comprises the following steps:

[0060] S1. Preparation of quantum dots (CN dots):

[0061] Weigh 3g of melamine, 1.12g of KOH and 0.4g of NaOH in a mortar and grind them into powder. Then add the evenly ground powder into a 50mL crucible, cover it with a lid, and place it in a muffle furnace for calcination at 300℃ for 2h. The heating rate is set to 5℃ / min. After the crucible cools to room temperature, take it out and disperse the material in the crucible into 100mL of high-purity water. After the material is fully dissolved, filter it to obtain a yellow filtrate. The yellow filtrate is added to a 3.5kD dialysis membrane and sealed, and dialyzed in high-purity water for 24h. The high-purity water is changed every 6h; finally, the dialyzate is poured into a beaker, placed in an oven at 80℃ to evaporate the water, and the powder at the bottom is collected to obtain quantum dots CN dots.

[0062] S2, solvent-induced self-assembly:

[0063] (1) Dispersing 100 mg of CN dots in 20 mL of high-purity water to obtain CN dots dispersion A;

[0064] (2) Take a 5 mL centrifuge tube and add 2 mL of ethanol, then gradually add 2 mL of dispersion A into it, stand for 2 h, separate the bottom material, freeze-dry, and obtain sample D (one-dimensional nanowires);

[0065] (3) The collected sample D was calcined in a tube furnace at 300°C for 2 h with a heating rate of 5°C / min and Ar gas protection; after naturally cooling to room temperature, the corresponding samples were collected.

[0066] Example 4

[0067] A preparation method for solvent-induced carbon nitride photocatalytic material morphology regulation comprises the following steps:

[0068] S1. Preparation of quantum dots (CN dots):

[0069] Weigh 3g of melamine, 1.12g of KOH and 0.4g of NaOH in a mortar and grind them into powder. Then add the evenly ground powder into a 50mL crucible, cover it with a lid, and place it in a muffle furnace for calcination at 300℃ for 2h. The heating rate is set to 5℃ / min. After the crucible cools to room temperature, take it out and disperse the material in the crucible into 100mL of high-purity water. After the material is fully dissolved, filter it to obtain a yellow filtrate. The yellow filtrate is added to a 3.5kD dialysis membrane and sealed, and dialyzed in high-purity water for 24h. The high-purity water is changed every 6h; finally, the dialyzate is poured into a beaker, placed in an oven at 80℃ to evaporate the water, and the powder at the bottom is collected to obtain quantum dots CN dots.

[0070] S2, solvent-induced self-assembly:

[0071] (1) Dispersing 100 mg of CN dots in 20 mL of high-purity water to obtain CN dots dispersion A;

[0072] (2) Take a 5 mL centrifuge tube and add 2 mL of isopropanol, then gradually add 2 mL of dispersion A into it, stand for 2 h, separate the bottom material, and freeze-dry to obtain sample E (two-dimensional nanosheet);

[0073] (3) The collected sample D was calcined in a tube furnace at 300°C for 2 h with a heating rate of 5°C / min and Ar gas protection; after naturally cooling to room temperature, the corresponding samples were collected.

[0074] Result analysis:

[0075] from Figure 1-5 It can be clearly seen that four quantum dot photocatalysts with different morphologies, namely one-dimensional sea urchin shape, one-dimensional nanonecklace, one-dimensional nanowire and two-dimensional nanosheet, can be obtained by inducing regulation of different solvents. It can be seen that quantum dot photocatalysts with different morphologies can be prepared by regulating the method of the present invention.

[0076] from Figure 6 It can be seen that the quantum dot photocatalysts with different morphologies prepared by the present invention have good performance in catalytic degradation of tetracycline hydrochloride, especially when ethanol is used as the solvent (Example 3), the catalytic effect is the best.

[0077] In the description of this specification, the description with reference to the terms "one embodiment", "some embodiments", "example", "specific example", or "some examples" etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms should not be understood as necessarily being directed to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described may be combined in any one or more embodiments or examples in a suitable manner. In addition, those skilled in the art may combine and combine different embodiments or examples described in this specification.

[0078] Although the embodiments of the present invention have been shown and described above, it is to be understood that the above embodiments are exemplary and are not to be construed as limitations of the present invention. A person skilled in the art may change, modify, replace and vary the above embodiments within the scope of the present invention.

Claims

1. A preparation method for solvent-induced morphology control of carbon nitride photocatalytic materials, It is characterized in that The following steps are involved: S1. Preparation of CN dots: Mixing melamine and alkali in a mortar, grinding them fully into mixed powder, then sintering the mixed powder, and cooling it to obtain a sintered product; The sintered product is added to high-purity water, dispersed and dissolved, and the filtrate is collected by filtration. The filtrate is dialyzed. After the dialysis is completed, the water is evaporated and the solid powder is collected to obtain quantum dots CN dots; S2. Solvent-induced morphology regulation: The obtained quantum dots CN dots are dispersed again in high-purity water to obtain a quantum dot solution; different solvents such as glacial acetic acid, methanol, ethanol, and isopropanol are used to treat the quantum dot solution respectively, and after the solvent treatment, the solid is dried to obtain different precursors; The different precursors are calcined under protective gas respectively, and after cooling, carbon nitride quantum dot photocatalysts with different morphologies are obtained.

2. The method for preparing a solvent-induced carbon nitride photocatalytic material morphology control according to claim 1, It is characterized in that In the step S1, the alkali includes potassium hydroxide and sodium hydroxide, and the mass ratio of potassium hydroxide to sodium hydroxide is 1.12:0.4; the mass ratio of melamine to the alkali is 3:1.

52.

3. The method for preparing a solvent-induced carbon nitride photocatalytic material morphology control according to claim 1, It is characterized in that In the step S1, the sintering is carried out in a muffle furnace, the sintering temperature is 300° C., the sintering time is 2 h, and the heating rate is 5° C. / min.

4. The method for preparing a solvent-induced carbon nitride photocatalytic material morphology control according to claim 1, It is characterized in that In the step S1, the mass volume ratio of melamine to high-purity water is 3 g:100 mL.

5. The method for preparing a solvent-induced carbon nitride photocatalytic material morphology control according to claim 1, It is characterized in that In the step S1, the dialysis treatment is performed in high-purity water, the dialysis time is 24 hours, and the high-purity water is changed every 6 hours.

6. The method for preparing a solvent-induced carbon nitride photocatalytic material morphology control according to claim 1, It is characterized in that In the step S2, the mass volume ratio of CN dots and high-purity water is 100 mg:20 mL.

7. The method for preparing a solvent-induced carbon nitride photocatalytic material morphology control according to claim 1, It is characterized in that In the step S2, the volume ratio of glacial acetic acid to the quantum dot solution is 3 mL:200 μL; the volume ratio of methanol to the quantum dot solution is 2 mL:2 mL; the volume ratio of ethanol to the quantum dot solution is 2 mL:2 mL; and the volume ratio of isopropanol to the quantum dot solution is 2 mL:2 mL.

8. The method for preparing a solvent-induced carbon nitride photocatalytic material morphology control according to claim 1, It is characterized in that In the step S2, the calcination treatment is carried out in a tubular furnace at 300° C. for 2 h, with a heating rate of 5° C. / min, and the protective gas is argon.

9. A carbon nitride photocatalyst with different morphologies, It is characterized in that The preparation method according to claim 1 is used for preparation.

10. Use of the carbon nitride photocatalyst with different morphologies as claimed in claim 9 in photocatalytic degradation of tetracycline hydrochloride.

Citation Information

Patent Citations

  • Method for preparing carbon nitride quantum dots

    CN104140084A

  • Halogenated lead-caesium perovskite fluorescent material and preparation method thereof

    CN109370563A

  • Preparation method and application of blue light dodecahedron perovskite quantum dot material

    CN114891505A

  • Double-promoter modified potassium-doped g-C3N4 photocatalyst and preparation method thereof

    CN117101698A

  • Carbon nitride quantum dot / tungsten trioxide composite photocatalytic material and preparation method therefor

    WO2022077811A1