Grounding material cleaning method and corrosion analysis method based on ammonium citrate mixed solution
Through the combination of ammonium citrate mixed solution and handheld roughness scanner, the problem of cleaning and corrosion analysis of carbon steel grounding materials after adding carbon-based resistance reducing agent is solved, achieving fast, economical and accurate cleaning and corrosion assessment, significantly Improved conductive properties and service life of grounding materials.
Patent Information
- Application Number
- CN202410626434.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-05-20
- Publication Date
- 2024-10-15
AI Technical Summary
The existing technology cannot effectively clean and corrosion analyze carbon steel grounding materials after adding carbon-based resistance reducing agents. The carbon-based resistance reducing agents affect the cleaning agent performance and corrosion analysis results.
Using a cleaning method and corrosion analysis method based on ammonium citrate mixed solution, through steps such as soaking, physical removal of corrosion products and brushing, combined with a handheld roughness scanner to measure surface roughness, provide fast and accurate cleaning and corrosion assessment.
Significantly improves the cleaning effect, improves conductive properties, extends the service life of grounding materials, reduces cleaning costs, and provides flexible cleaning formulas and accurate corrosion analysis results.
Smart Images

Figure CN118768293A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a cleaning method and corrosion analysis of a grounding material, in particular to a cleaning method and a corrosion analysis method of a carbon steel grounding material after a carbon-based resistance reducing agent is added. Background Art
[0002] In recent years, carbon-based grounding materials such as carbon powder resistance reducers (including coke powder), carbon-based grounding modules, and flexible graphite grounding electrodes have been increasingly used in the grounding industry. Grounding materials are widely used in the grounding systems of buildings, factories, and equipment to ensure a good connection between the circuit or equipment and the ground. Since resistance is generated when current passes through the grounding system, which affects the transmission efficiency of the current, carbon-based resistance reducers are needed to reduce the resistance of the grounding system to improve the transmission efficiency of the current. However, in some operation and maintenance excavation processes, it was found that carbon-based resistance reducers have accelerated corrosion of other metal materials (especially steel materials), increasing the risk of failure of the grounding grid. After using carbon-based resistance reducers, the surface of the grounding grid is uneven and the surface roughness increases. In grounding materials, surface roughness is crucial to the development and spread of corrosion. Rough surfaces can provide more surface area, making it easier for corrosive agents to adhere, so the corrosion rate may be faster. On the contrary, flatter surfaces can reduce the risk of corrosion.
[0003] Oxidation, rust and other problems on the surface of the grounding material will affect its grounding effect. Therefore, it is necessary to clean and analyze the corrosion of the grounding material after adding the carbon-based resistance reduction agent.
[0004] Currently, there are various cleaning methods and corrosion analysis methods for carbon steel grounding materials on the market, but these methods are not suitable for carbon steel grounding materials after adding carbon-based resistance reducing agents, because the presence of carbon-based resistance reducing agents will affect the performance and cleaning effect of the cleaning agent, and will also interfere with the corrosion analysis results. Summary of the invention
[0005] In order to solve the technical problems existing in the prior art, the present invention provides a grounding material cleaning method and a corrosion analysis method based on an ammonium citrate mixed solution, which can quickly and effectively clean the carbon steel grounding material after adding a carbon-based drag reduction agent, and at the same time provide a basis for accurately evaluating the corrosion degree and corrosion rate of the grounding material after adding the carbon-based drag reduction agent.
[0006] The present invention is achieved through the following technical solutions:
[0007] A method for cleaning a grounding material based on an ammonium citrate mixed solution, wherein the carbon steel grounding material to which a carbon-based resistance reducing agent is added is soaked in the ammonium citrate mixed solution;
[0008] The solvent of the ammonium citrate mixed solution is water. In terms of mass concentration, the solutes of the ammonium citrate mixed solution include: ammonium citrate: about 6.5% to 7.5%, tartaric acid: about 0.9% to 1.1%, acetic acid: about 0.4% to 0.6%, citric acid: about 0.4% to 0.6%, oxalic acid: about 0.4% to 0.6%, and phosphoric acid: about 0.4% to 0.6%.
[0009] The soaking treatment is carried out at 70°C-90°C.
[0010] Before the immersion treatment, the method also includes: removing the corrosion products on the surface of the carbon steel grounding material by a physical method.
[0011] The corrosion products on the surface of the carbon steel grounding material are removed by a physical method, specifically: the corrosion products on the surface of the carbon steel grounding material are removed by a non-metallic tool, and / or the carbon steel grounding material is scrubbed by a brush.
[0012] After removing the corrosion products on the surface of the carbon steel grounding material by a physical method and before the immersion treatment, the method further includes: cleaning the carbon steel grounding material by using gasoline.
[0013] After the soaking treatment, the method also includes: brushing the carbon steel grounding material with a brush.
[0014] After brushing the carbon steel grounding material with a brush, the method further includes: drying the carbon steel grounding material.
[0015] The drying temperature is 100℃-110℃.
[0016] A grounding material corrosion analysis method based on an ammonium citrate mixed solution is provided to measure the surface roughness of a carbon steel grounding material obtained by the grounding material cleaning method.
[0017] The surface roughness of the carbon steel grounding material obtained by the grounding material cleaning method is measured.
[0018] Compared with the prior art, the present invention has the following beneficial effects:
[0019] The present invention adopts an ammonium citrate mixed solution to clean the grounding material, which has the following advantages: (1) Improved cleaning effect: By adopting an ammonium citrate mixed solution, the cleaning effect is successfully improved. This new solution quickly removes dirt, oil stains, oxides and other substances on the surface of the grounding material, significantly improves the conductive properties of the grounding material, prevents the grounding material from being corroded, protects the surface of the grounding material, and extends the service life. (2) Efficient cleaning: Using an ammonium citrate mixed solution for cleaning is not only faster, but also can effectively save cleaning time and labor costs. (3) Economical and practical: Compared with traditional acid-base solutions, the cost of ammonium citrate mixed solution as a cleaning material is lower, which effectively reduces the cleaning cost and makes the cleaning process more economical and practical. (4) Flexible formula: The formula of the ammonium citrate mixed solution is flexible and diverse, and can be adjusted according to the special conditions and cleaning requirements of the surface of the grounding material, and can meet the cleaning needs of different grounding materials.
[0020] The present invention uses an ammonium citrate mixed solution to quickly and efficiently clean dirt and oxides on the surface of the grounding material without causing damage to the grounding material itself. (5) The ammonium citrate mixed solution will not be affected by the carbon-based drag reducer. Ammonium citrate is an organic acid salt, and relatively few chemical reactions may occur between it and the carbon-based drag reducer. Ammonium citrate mainly removes dirt by coordination and chelation with oxides on the metal surface, and this effect is not directly related to the chemical properties of the carbon-based drag reducer. In addition, ammonium citrate has good solubility in water, which allows it to be fully dispersed in the solution, reducing possible reactions with the carbon-based drag reducer. The present invention also provides a corrosion analysis method using a handheld roughness scanner, which can accurately evaluate the corrosion degree and corrosion rate of the grounding material after the carbon-based drag reducer is added. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0022] Figure 1 is a process flow chart of cleaning the carbon steel grounding material provided by an embodiment of the present invention;
[0023] Figure 2 Schematic diagram of a handheld roughness measuring instrument used in an embodiment of the present invention.
[0024] Figure 3 It is a diagram of the chemical reaction process occurring during the embodiment of the present invention. DETAILED DESCRIPTION
[0025] The following describes the embodiments of the present invention through specific examples, and those skilled in the art can easily understand other advantages and effects of the present invention from the contents disclosed in this specification. The present invention can also be implemented or applied through other different specific embodiments, and the details in this specification can also be modified or changed in various ways based on different viewpoints and applications without departing from the spirit of the present invention.
[0026] It should be noted that the process equipment or devices not specifically specified in the following embodiments are all conventional equipment or devices in the art.
[0027] It should be noted that the terms "include" and "have" and any variations thereof are intended to cover non-exclusive inclusions. For example, a process, method, system, product or device that includes a series of steps or units is not necessarily limited to those steps or units clearly listed, but may include other steps or units that are not clearly listed or inherent to these processes, methods, products or devices. Moreover, unless otherwise specified, the numbering of each method step is only a convenient tool for identifying each method step, and is not intended to limit the order of arrangement of each method step or to define the scope of the present invention. Changes or adjustments in their relative relationships should also be regarded as the scope of the present invention without substantially changing the technical content.
[0028] The carbon steel grounding materials described below in the present invention all refer to carbon steel grounding materials to which a carbon-based resistance reducing agent is added.
[0029] In some specific embodiments of the present invention, the method for cleaning the grounding material based on the ammonium citrate mixed solution comprises the following steps:
[0030] S1: Corrosion product removal
[0031] To ensure thorough cleaning, first use non-metallic tools, such as scrapers or chisels, to carefully and thoroughly remove the corrosion products on the surface of the carbon steel grounding material, and also remove the soil on the surface of the carbon steel grounding material. This step is intended to prepare a clean substrate so that the subsequent steps can be carried out more effectively.
[0032] S2: Metal hard brushing
[0033] The carbon steel grounding material is scrubbed with a hard metal brush. This step is to further remove impurities and solid particles that may remain on the surface of the carbon steel grounding material to ensure that the surface of the specimen is fully cleaned.
[0034] S3: Gasoline cleaning
[0035] Use gasoline to clean the remaining asphalt and grease inside the carbon steel grounding material. This is to remove the oily contaminants remaining on the surface of the carbon steel grounding material and ensure the comprehensiveness and comprehensiveness of the cleaning process.
[0036] S4: Collect into glass container
[0037] Collect the cleaned carbon steel grounding material and cleaning liquid into a glass container. This helps the controllability and environmental friendliness of the entire cleaning process and facilitates the operation of subsequent steps.
[0038] S5: Soaking and cleaning with ammonium citrate mixed solution
[0039] An ammonium citrate mixed solution is prepared using an ammonium citrate cleaning agent as a soaking solution. The ammonium citrate mixed solution has a highly efficient cleaning capability for corrosion products and dirt, while protecting the surface of the carbon steel grounding material from damage.
[0040] S6: Cooling operation and soaking
[0041] The prepared soaking liquid is cooled down, and then the carbon steel grounding material is immersed in the soaking liquid. This step ensures that the cleaning agent can play the best effect at the appropriate temperature and improves the thoroughness of cleaning.
[0042] S7: Metal hard brushing again
[0043] Use a hard metal brush to scrub the carbon steel grounding material again. This step helps to further remove the dirt dissolved during the soaking process and ensure the purity of the surface of the carbon steel grounding material.
[0044] S8: Oven drying
[0045] The cleaned carbon steel grounding material is placed in an oven and dried after heating. This ensures that the carbon steel grounding material is dried quickly after cleaning to prevent new contamination or oxidation.
[0046] S9: Surface roughness measurement
[0047] Finally, the surface roughness is measured. Through this step, the corrosion degree and corrosion rate of the cleaned carbon steel grounding material can be accurately evaluated, and the cleaning effect can be verified while providing a reference for the further use of the grounding material.
[0048] In some specific embodiments of the present invention, the Vickers hardness of the metal hard brush in steps S2 and S7 is between 150-250 HV, and the carbon steel grounding material can be brushed in running water or clean water.
[0049] In some specific embodiments of the present invention, the preparation step of the soaking solution in step S5 includes: fully dissolving the ammonium citrate cleaning agent with water; the volume ratio of the ammonium citrate cleaning agent to water is about 1:10, and the mass concentration range of each substance in the finally prepared soaking solution is: ammonium citrate is about 6.5% to 7.5%, tartaric acid is about 0.9% to 1.1%, acetic acid is about 0.4% to 0.6%, citric acid is about 0.4% to 0.6%, oxalic acid is about 0.4% to 0.6%, and phosphoric acid is about 0.4% to 0.6%. .
[0050] In some specific embodiments of the present invention, step S6 includes the following sub-steps:
[0051] S61: When the carbon steel grounding material is immersed in the immersion liquid, the immersion liquid must cover the carbon steel grounding material.
[0052] S62: Place the container soaking the carbon steel grounding material at 70℃-90℃ for 6-10 hours.
[0053] S63: If the corrosion products have not been removed, the time can be appropriately extended until all corrosion products are removed.
[0054] In some specific embodiments of the present invention, step S7 includes the following sub-steps:
[0055] S71: After taking out the carbon steel grounding material from the immersion solution, scrub it with a hard metal brush in running water, or put it in clean water and scrub it with a hard metal brush, and then wipe it dry with a cloth.
[0056] S72: If any residual corrosion products remain, they can be gently scraped off with a knife.
[0057] S73: If the corrosion products are still not removed, repeat the process.
[0058] In some specific embodiments of the present invention, step S8 includes the following steps:
[0059] S81: Raise the oven temperature to between 100°C and 110°C in advance.
[0060] S82: Place the rinsed carbon steel grounding material in an oven and dry it for more than 2-4 hours to prevent the carbon steel grounding material from being oxidized again.
[0061] Example 1
[0062] A method for cleaning carbon steel grounding material, such as Figure 1 As shown, the following steps are included:
[0063] S1: Use a non-metallic scraper to remove corrosion products on the surface of the carbon steel grounding material and clean the soil on the surface of the carbon steel grounding material.
[0064] S2: Use a metal hard brush to brush the carbon steel grounding material. The Vickers hardness of the metal hard brush is between 150HV and can be brushed in running water or clean water.
[0065] S3: Use gasoline to clean the remaining asphalt and grease inside the carbon steel grounding material.
[0066] S4: Place the cleaned carbon steel grounding material into a glass container.
[0067] S5: preparing a soaking solution using ammonium citrate detergent, the steps comprising: using deionized water to fully dissolve the ammonium citrate detergent, the volume ratio of the ammonium citrate mixed solution to the deionized water being 1:10; the mass concentration of each substance in the prepared soaking solution is: ammonium citrate is about 6.5% to 7.5%, tartaric acid is about 0.9% to 1.1%, acetic acid is about 0.4% to 0.6%, citric acid is about 0.4% to 0.6%, oxalic acid is about 0.4% to 0.6%, and phosphoric acid is about 0.4% to 0.6%.
[0068] S6: After cooling the prepared immersion liquid, immersing the carbon steel grounding material in the immersion liquid, the steps include:
[0069] S61: When the carbon steel grounding material is immersed in the immersion liquid, the immersion liquid must cover the carbon steel grounding material.
[0070] S62: Place the glass container soaked in carbon steel grounding material at 70°C for 6 hours until all corrosion products are removed.
[0071] S7: After removing the carbon steel grounding material, scrub it with a hard metal brush under running water, and then wipe it dry with a cloth.
[0072] S8: After the oven is heated, the rinsed carbon steel grounding material is placed in the oven for drying. The steps include:
[0073] S81: Raise the oven temperature to 100°C in advance.
[0074] S82: Place the rinsed carbon steel grounding material in an oven and dry it for 4 hours to prevent the carbon steel grounding material from being oxidized again.
[0075] S9: Measure the surface roughness and perform corrosion analysis based on the measured results.
[0076] Example 2
[0077] A method for cleaning carbon steel grounding material, such as Figure 1 As shown, the following steps are included:
[0078] S1: Use a non-metallic scraper to remove corrosion products on the surface of the carbon steel grounding material and clean the soil on the surface of the carbon steel grounding material.
[0079] S2: Use a metal hard brush to brush the carbon steel grounding material. The Vickers hardness of the metal hard brush is between 150HV and can be brushed in running water or clean water.
[0080] S3: Use gasoline to clean the remaining asphalt and grease inside the carbon steel grounding material.
[0081] S4: Place the cleaned carbon steel grounding material into a glass container.
[0082] S5: preparing a soaking liquid using an ammonium citrate detergent, the steps include: using deionized water to fully dissolve the ammonium citrate detergent, the volume ratio of the ammonium citrate mixed solution to the deionized water is 1:10; the mass concentration of each substance in the prepared soaking liquid is: the mass concentration range of each substance in the soaking liquid is: ammonium citrate is about 6.5% to 7.5%, tartaric acid is about 0.9% to 1.1%, acetic acid is about 0.4% to 0.6%, citric acid is about 0.4% to 0.6%, oxalic acid is about 0.4% to 0.6%, and phosphoric acid is about 0.4% to 0.6%. According to these ranges, a specific embodiment may be: the mass concentration of ammonium citrate is 6.6%, the mass concentration of tartaric acid is 1%, the mass concentration of acetic acid is 0.5%, the mass concentration of citric acid is 0.5%, the mass concentration of oxalic acid is 0.5%, and the mass concentration of phosphoric acid is 0.5%.
[0083] S6: After cooling the prepared immersion liquid, immersing the carbon steel grounding material in the immersion liquid, the steps include:
[0084] S61: When the carbon steel grounding material is immersed in the immersion liquid, the immersion liquid must cover the carbon steel grounding material.
[0085] S62: Place the glass container soaked in carbon steel grounding material at 80°C for 6 hours until all corrosion products are removed.
[0086] S7: After removing the carbon steel grounding material, scrub it with a hard metal brush under running water, and then wipe it dry with a cloth.
[0087] S8: After the oven is heated, the rinsed carbon steel grounding material is placed in the oven for drying. The steps include:
[0088] S81: Raise the oven temperature to 100°C in advance.
[0089] S82: Place the rinsed carbon steel grounding material in an oven and dry it for 4 hours to prevent the carbon steel grounding material from being oxidized again.
[0090] S9: Measure the roughness of the corrosion surface and perform corrosion analysis based on the measured results.
[0091] Example 3
[0092] A method for cleaning carbon steel grounding material, such as Figure 1 As shown, the following steps are included:
[0093] S1: Use a non-metallic scraper to remove corrosion products on the surface of the carbon steel grounding material and clean the soil on the surface of the carbon steel grounding material.
[0094] S2: Use a metal hard brush to brush the carbon steel grounding material. The Vickers hardness of the metal hard brush is between 150HV and can be brushed in running water or clean water.
[0095] S3: Use gasoline to clean the remaining asphalt and grease inside the carbon steel grounding material.
[0096] S4: Place the cleaned carbon steel grounding material into a glass container.
[0097] S5: preparing a soaking liquid using an ammonium citrate detergent, the steps include: using deionized water to fully dissolve the ammonium citrate detergent, the volume ratio of the ammonium citrate mixed solution to the deionized water is 1:10; the mass concentration of each substance in the prepared soaking liquid is: the mass concentration range of each substance in the soaking liquid is: ammonium citrate is about 6.5% to 7.5%, tartaric acid is about 0.9% to 1.1%, acetic acid is about 0.4% to 0.6%, citric acid is about 0.4% to 0.6%, oxalic acid is about 0.4% to 0.6%, and phosphoric acid is about 0.4% to 0.6%. According to these ranges, a specific embodiment may be: the mass concentration of ammonium citrate is 6.6%, the mass concentration of tartaric acid is 1%, the mass concentration of acetic acid is 0.5%, the mass concentration of citric acid is 0.5%, the mass concentration of oxalic acid is 0.5%, and the mass concentration of phosphoric acid is 0.5%.
[0098] S6: After cooling the prepared immersion liquid, immersing the carbon steel grounding material in the immersion liquid, the steps include:
[0099] S61: When the carbon steel grounding material is immersed in the immersion liquid, the immersion liquid must cover the carbon steel grounding material.
[0100] S62: Place the glass container soaked in carbon steel grounding material at 90°C for 6 hours until all corrosion products are removed.
[0101] S7: After removing the carbon steel grounding material, scrub it with a hard metal brush under running water, and then wipe it dry with a cloth.
[0102] S8: After the oven is heated, the rinsed carbon steel grounding material is placed in the oven for drying. The steps include:
[0103] S81: Raise the oven temperature to 100°C in advance.
[0104] S82: Place the rinsed carbon steel grounding material in an oven and dry it for 4 hours to prevent the carbon steel grounding material from being oxidized again.
[0105] S9: Measure the roughness of the corrosion surface and perform corrosion analysis based on the measured results.
[0106] Example 4
[0107] The corrosion products on the surface of the grounding material are removed by chemical cleaning. When cleaning the corrosion products on the surface of the grounding material, chemical cleaning agents with different formulas should be selected. This time, gasoline is used to clean the remaining asphalt and the grease inside the test piece, and then the degreased test piece is immersed in different mixed cleaning solutions and placed at 80°C for 2-8 hours to remove the corrosion products. Finally, it can be rinsed in deionized water, put into deionized water and brushed with a brush, and then the water stains on the surface of the test piece are wiped with a cloth, and then placed in an oven at about 105°C for drying, and then measured.
[0108] In this experiment, a handheld roughness meter was used to measure the surface roughness of the sample. First, the indication calibration and stylus position calibration were performed, and the parameters of the TR200 roughness meter were set. The sampling length was 2.5 mm, the evaluation length was 5 l, the ISO standard, ±80 μm, RC filtering, and Rz parameters were selected. The unit was μm. The front and back sides of the sample were measured 10 times respectively, and the average value was taken for corrosion sample analysis.
[0109] After the test results were sorted out, solution A was a mixed solution: the mass concentration of ammonium citrate was 6.6%, the mass concentration of tartaric acid was 1%, the mass concentration of acetic acid was 0.5%, the mass concentration of citric acid was 0.5%, the mass concentration of oxalic acid was 0.5%, and the mass concentration of phosphoric acid was 0.5%. Solution B was an ammonium citrate solution with a mass concentration of 9.6%. Solution C was a mixed solution: the mass concentration of tartaric acid was 3.2%, the mass concentration of acetic acid was 1.6%, the mass concentration of citric acid was 1.6%, the mass concentration of oxalic acid was 1.6%, and the mass concentration of phosphoric acid was 1.6%. The total acid concentration of ABC solutions was controlled to be the same. The experimental results are shown in Tables 1 and 2.
[0110] Table 1 Experimental data of corrosion rate measurement of 6 substations including Baoji
[0111]
[0112]
[0113] Table 2 Experimental data of corrosion rate measurement of six substations including Weinan
[0114]
[0115] It can be seen that mixed solution A has the best cleaning effect. When all variables are controlled, the maximum mass loss is obtained, that is, the most oxides are cleaned and the cleaning effect is the best. The second is ammonium citrate solution B, which is a conventional cleaning agent. Mixed solution C has the worst cleaning effect. Ammonium citrate plays a key role in mixed solution A, and the remaining acids play an auxiliary role, making it have a better cleaning effect than single ammonium citrate solution.
[0116] Example 5
[0117] When using a handheld roughness meter to measure the surface roughness of cleaned carbon steel grounding materials, refer to Figure 2 The structure of the handheld roughness measuring instrument shown in the figure places the sensor on the measured surface of the carbon steel grounding material. The driving mechanism inside the handheld roughness measuring instrument drives the sensor to slide along the measured surface at a constant speed. The sensor senses the roughness of the measured surface through the built-in sharp stylus. At this time, the roughness of the measured surface of the carbon steel grounding material causes the stylus to displace. The displacement changes the inductance of the sensor inductor coil, thereby generating an analog signal proportional to the roughness of the measured surface at the output end of the phase-sensitive rectifier. The signal enters the data acquisition system after amplification and level conversion. The DSP chip performs digital filtering and parameter calculation on the collected data. The measurement results are read out on the LCD display, can also be output on a printer, and can also communicate with a PC.
[0118] A handheld roughness meter was used to measure the surface roughness of the carbon steel grounding material. First, the indication calibration and stylus position calibration were performed, and the parameters of the TR200 roughness meter were set. The sampling length was 2.5 mm, the evaluation length was 5 l, the ISO standard, ±80 μm, the RC filter, the Rz (maximum height), the parameter, and the unit was μm. The front and back sides of the sample were measured 10 times respectively, and the average value was taken for corrosion sample analysis.
[0119] If the range is exceeded, the handheld roughness tester usually has adjustable parameters, such as range, sampling length, etc. You can try to adjust these parameters to adapt to the roughness range of the sample. For example, increase the range of the instrument and reduce the sampling length to better measure samples with larger roughness.
[0120] For samples that exceed the measuring range, multiple scans can be performed. It is usually recommended to perform 10-15 scans. The scanning speed and force should be similar to reduce the systematic error. The results of each scan are recorded, and the average and standard deviation are calculated. For different samples, the same measurement method and parameters are used to evaluate the consistency of the data. The results are then combined to obtain more comprehensive data. This can be achieved by dividing the scanning range into multiple parts and then scanning each part separately.
[0121] If a handheld roughness meter does not meet your requirements, you can consider using other roughness measurement instruments such as laser interferometers, atomic force microscopes (AFM), or white light interferometers, which generally have a larger measurement range.
[0122] Corrosion analysis evaluation is essential for assessing the corrosion performance of grounding material carbon steel after adding carbon-based drag reducers. Surface roughness measurement is an important component of corrosion analysis, which provides key information about the surface condition of the material, which is of great significance for the evaluation of corrosion performance. Handheld roughness meters are a commonly used measurement tool, but problems such as over-range, average scan times and value selection need to be carefully addressed. By combining surface roughness data and corrosion test results, the performance of carbon steel components after adding carbon-based drag reducers can be fully evaluated and provide useful information for engineering applications. In corrosion analysis evaluation, data accuracy and repeatability are crucial, so the design of the experiment and data analysis need to be carefully planned and verified to ensure reliable results.
[0123] Although the embodiments of the present invention have been shown and described above, it is understood that the above embodiments are exemplary and cannot be understood as limiting the present invention. Those skilled in the art may change, modify, replace and modify the above embodiments within the scope of the present invention.
[0124] The above specific implementations of the present invention do not constitute a limitation on the protection scope of the present invention. Any other corresponding changes and modifications made based on the technical concept of the present invention should be included in the protection scope of the claims of the present invention.
Claims
1. A method for cleaning grounding materials based on an ammonium citrate mixed solution, characterized in that: The carbon steel grounding material with carbon-based resistance reducing agent added is soaked in an ammonium citrate mixed solution; The solvent of the ammonium citrate mixed solution is water. In terms of mass concentration, the solutes of the ammonium citrate mixed solution include: ammonium citrate: about 6.5% to 7.5%, tartaric acid: about 0.9% to 1.1%, acetic acid: about 0.4% to 0.6%, citric acid: about 0.4% to 0.6%, oxalic acid: about 0.4% to 0.6%, and phosphoric acid: about 0.4% to 0.6%.
2. The method for cleaning grounding materials based on the ammonium citrate mixed solution according to claim 5, characterized in that: The soaking treatment is carried out at 70°C-90°C.
3. The method for cleaning grounding materials based on the ammonium citrate mixed solution according to claim 1, characterized in that: Prior to the soaking treatment, it also includes: A physical method is used to remove the corrosion products on the surface of the carbon steel grounding material.
4. The method for cleaning grounding materials based on the ammonium citrate mixed solution according to claim 3, characterized in that: The corrosion products on the surface of the carbon steel grounding material are removed by a physical method, specifically: the corrosion products on the surface of the carbon steel grounding material are removed by a non-metallic tool, and / or the carbon steel grounding material is scrubbed by a brush.
5. The method for cleaning grounding materials based on the ammonium citrate mixed solution according to claim 3, characterized in that: After removing the corrosion products on the surface of the carbon steel grounding material by physical method and before immersion treatment, it also includes: Use gasoline to clean carbon steel grounding materials.
6. The method for cleaning grounding materials based on the ammonium citrate mixed solution according to claim 1, characterized in that: After the soaking treatment, it also includes: Use a brush to scrub the carbon steel grounding material.
7. The method for cleaning grounding materials based on the ammonium citrate mixed solution according to claim 6, characterized in that: After brushing the carbon steel grounding material, it also includes: Dry the carbon steel grounding material.
8. The method for cleaning grounding materials based on the ammonium citrate mixed solution according to claim 7, characterized in that: The drying temperature is 100℃-110℃.
9. A grounding material corrosion analysis method based on ammonium citrate mixed solution, characterized in that: The surface roughness of the carbon steel grounding material obtained by the grounding material cleaning method according to any one of claims 1 to 8 is measured.
10. The method for analyzing grounding material corrosion based on ammonium citrate mixed solution according to claim 9, characterized in that: Measure the surface roughness of the carbon steel grounding material obtained by the grounding material cleaning method according to any one of claims 1 to 8.