Machining technical method for milling crankshaft of diesel engine at low stress and high speed
Through low-stress high-speed milling technology, including billet tempering and multiple finishing and tempering treatments, the problem of large internal stress in crankshaft machining is solved, the accuracy and impact resistance of the crankshaft are improved, and the processing efficiency and quality stability are improved .
Patent Information
- Application Number
- CN202410942661.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-15
- Publication Date
- 2024-10-15
AI Technical Summary
In the existing crankshaft processing technology, the tempering effect of long-diameter crankshafts is not obvious, and the residual stress in the workpiece is large, resulting in large deformation and unstable accuracy, which affects the subsequent grinding and quenching process and reduces the quality and processing efficiency of the crankshaft.
Low-stress high-speed milling technology is adopted, including billet quenching and tempering, gradual quenching and tempering treatment. Through the staggered setting of fillet and right-angle cutter discs of the internal milling cutter, the cutting speed and feed amount are controlled, the internal stress is reduced, and each processing Fix adjacent positions for multiple finishing and tempering treatments.
It effectively reduces the internal stress during crankshaft machining, improves machining accuracy and surface integrity, reduces the scrap rate, improves the crankshaft's resistance to impact, torsional vibration and wear, and improves the accuracy stability and processing efficiency of mass production. .
Smart Images

Figure CN118768880A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of crankshaft processing, and in particular relates to a low-stress high-speed milling diesel engine crankshaft processing technology method. Background Art
[0002] The crankshaft is the core component of the engine. To achieve stable power output at high speed under extremely high combustion explosion pressure shock and high torque torsional vibration conditions, the crankshaft as a whole is required to have extremely high resistance to torsional vibration, wear resistance, fatigue resistance, and long-term and stable precision. For the crankshaft in a high-power engine, the crankshaft aspect ratio is larger and the crank anisotropy is more prominent, so the strength and precision requirements of the crankshaft are higher, making the crankshaft processing more difficult.
[0003] After analyzing the existing crankshaft production process and finished products, it was found that the crankshafts produced by the existing technology have a relatively large length-to-diameter ratio, and the tempering effect is not obvious, resulting in large residual stress in the workpiece, resulting in a deformation of the workpiece between 4-9mm after rough milling and between 3-8mm after fine milling. There is a certain gap between the accuracy required by the parameters, and the deformation during the processing will also interfere with the subsequent grinding and quenching processes, resulting in a greater deformation of the finished product, reducing the quality of the crankshaft, making the crankshaft's accuracy stability poor during mass production, and the scrap rate high, reducing the crankshaft processing efficiency. Summary of the invention
[0004] In view of this, the present invention aims to propose a low-stress high-speed milling diesel engine crankshaft processing technology method to reduce the internal stress during the crankshaft processing and improve the crankshaft processing accuracy.
[0005] To achieve the above object, the technical solution of the present invention is achieved as follows:
[0006] A low-stress high-speed milling diesel engine crankshaft processing technology method, comprising:
[0007] S1: The blank is quenched and tempered, and the blank is placed in a vertically hoisted pit heating furnace for quenching, so that the hardness of the workpiece is between 302 and 363HB, and the tensile strength is between 980 and 1180MPa;
[0008] S2: Rough machining of crankshaft journals. Fix the main journals separately. After each main journal is fixed, the main journal on the side close to the end and the connecting rod journal on the side close to the start end of the fixed main journal are machined. At the same time, the crank arm surfaces of the machined main journal and connecting rod journal are machined.
[0009] S3: Rough machining heat treatment, using a horizontal heating furnace to temper the crankshaft after rough machining;
[0010] S4: Finishing the crank arm surface of the main journal, fixing the main journals in sequence, and after each fixing of the main journal, finishing the main journal on the side of the fixed main journal close to the rear end of the crankshaft and the crank arm surfaces on both sides thereof;
[0011] S5: Finishing of connecting rod diameter crank arm surface, fixing the main journals in sequence, and after each fixing of the main journals, finishing of the connecting rod diameter on the side of the fixed main journal close to the crankshaft starting end and the crank arm surfaces on both sides thereof;
[0012] S6: outer edge processing, fixing the main shaft journals in sequence, and after each fixing of the main shaft journal, finishing the outer edges of the crank arms of the two main shaft journals adjacent to the fixed main shaft journal;
[0013] S7: Heat treatment of workpiece: tempering of the finished crankshaft in a horizontal heating furnace.
[0014] Furthermore, in step S2, the order of rough machining the crankshaft journal is to process it from the starting end to the end of the crankshaft in sequence;
[0015] In steps S5 and S6, the finishing order of the main shaft crank arm surface and the connecting rod crank arm surface is to process them successively from the starting end to the end end of the crankshaft.
[0016] Furthermore, in step S2, the crankshaft is rough-machined using an internal milling cutter with a cutting speed of 116 m / min, a cutting depth of 0.1 mm, and a feed rate of 0.08 mm / r. The crankshaft workpiece rotates at a speed of 3 min / r through dry cutting.
[0017] Furthermore, in steps S5 and S6, an internal milling cutter is used to finish the crankshaft, with a cutting speed of 116 m / min, a cutting depth of 0.1 mm, a feed rate of 0.05 mm / r, and a dry cutting method. The crankshaft workpiece rotation speed is 2 min / r.
[0018] Furthermore, in steps S2, S4 and S5, the workpiece is processed by an internal milling cutter respectively, and the internal milling cutter is provided with two groups of rounded corner cutter discs and multiple groups of right-angle cutter discs along the axial direction, and the right-angle cutter discs are placed between the two groups of rounded corner cutter discs, the rounded corner cutter disc is fixed with multiple rounded corner blades, the right-angle cutter disc is fixed with multiple right-angle blades, and the right-angle blades or rounded corner blades in adjacent right-angle cutter discs and rounded corner cutter discs are staggered.
[0019] Furthermore, in step S2, two internal milling cutters are used to simultaneously process the main shaft journal near the rear end and the connecting rod diameter near the starting end of the fixed main shaft journal.
[0020] Furthermore, in step S6, two groups of internal milling cutters are used to simultaneously machine the outer edges of the crank arms of the main journals adjacent to each other on both sides of the fixed main journal.
[0021] Furthermore, the tempering treatment in step S3 and step S7 is to place the processed semi-finished workpiece in a horizontal heating furnace, and place the point with the largest crankshaft circular runout at the highest point of the workpiece. The temperature in the heating furnace is 550°, kept warm for 5 hours, and then cooled to room temperature with the furnace.
[0022] Further, in step S1, the quenching temperature is 860±10°C, the holding time is ≥6h, and the total time is 8h~9h. Then, the workpiece is placed in a cooling medium and cooled for 9-13min, and then air-cooled to room temperature.
[0023] Furthermore, the cooling medium is AQ251 quenching liquid with a concentration of 10-15%.
[0024] Compared with the prior art, the low-stress high-speed milling diesel engine crankshaft processing technology method described in the present invention has the following advantages:
[0025] The present invention adopts the method of quenching and modulating the blank before rough machining to improve the hardness and strength of the workpiece and reduce the internal stress of the workpiece formed during the rotation and cutting process; in each machining process, only the adjacent positions of the fixed parts are machined, thereby avoiding the instability of the workpiece caused by the machining process and reducing the machining accuracy; at the same time, after rough machining and fine machining, tempering treatment is performed to improve the flexibility and toughness of the workpiece, thereby further reducing the internal stress of the workpiece caused by the machining process;
[0026] The main journal and connecting rod journal are processed simultaneously on both sides of the main journal where the crankshaft is fixed, so that the forces on both sides of the crankshaft fixed position are similar, reducing the deformation caused by external forces in a single direction during crankshaft processing;
[0027] The milling cutter is formed by combining a rounded cutter disc and a right-angle cutter disc, so that the workpiece can be formed in one step during the processing, which improves the processing efficiency. At the same time, it is beneficial to control the milling force and milling heat generated during the processing, thereby reducing the internal stress of the workpiece during processing. The blades are staggered to facilitate the discharge of waste chips during milling and avoid scratching the workpiece surface.
[0028] The use of low workpiece speed, small feed rate and small depth in the milling process further avoids cutting heat on the workpiece surface, effectively controls the surface quality and machining deformation, and effectively improves the crankshaft machining accuracy and surface integrity. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] The accompanying drawings constituting a part of the present invention are used to provide a further understanding of the present invention. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute an improper limitation of the present invention. In the accompanying drawings:
[0030] Figure 1 The schematic diagram of the crankshaft structure being processed;
[0031] Figure 2 It is a schematic diagram of the processing method process;
[0032] Figure 3 This is a schematic diagram of the internal milling cutter structure and its cross-section. Description of the drawings:
[0034] 1-first main journal; 2-second main journal; 3-third main journal; 4-fourth main journal; 5-fifth main journal; 6-sixth main journal; 7-seventh main journal; 8-eighth main journal; 9-ninth main journal; 11-first connecting rod journal; 12-second connecting rod journal; 13-third connecting rod journal; 14-fourth connecting rod journal; 15-fifth connecting rod journal; 16-sixth connecting rod journal; 17-seventh connecting rod journal; 18-eighth connecting rod journal ; 19- the ninth connecting rod neck; 21- the first crank arm; 22- the second crank arm; 23- the third crank arm; 24- the fourth crank arm; 25- the fifth crank arm; 26- the sixth crank arm; 27- the seventh crank arm; 28- the eighth crank arm; 29- the ninth crank arm; 30- the tenth crank arm; 31- the eleventh crank arm; 32- the twelfth crank arm; 33- the thirteenth crank arm; 34- the fourteenth crank arm; 35- the fifteenth crank arm; 36- the sixteenth crank arm. DETAILED DESCRIPTION
[0035] It should be noted that, in the absence of conflict, the embodiments of the present invention and the features in the embodiments may be combined with each other.
[0036] In the description of the present invention, it should be understood that the terms "center", "longitudinal", "lateral", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside" and the like indicate positions or positional relationships based on the positions or positional relationships shown in the accompanying drawings, and are only for the convenience of describing the present invention and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as limiting the present invention. In addition, the terms "first", "second", and the like are only used for descriptive purposes, and cannot be understood as indicating or implying relative importance or implicitly indicating the number of technical features indicated. Thus, features defined as "first", "second", and the like may explicitly or implicitly include one or more of the features. In the description of the present invention, unless otherwise specified, "multiple" means two or more.
[0037] In the description of the present invention, it should be noted that, unless otherwise clearly specified and limited, the terms "installed", "connected", and "connected" should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection, or it can be indirectly connected through an intermediate medium, or it can be the internal communication of two components. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood by specific circumstances.
[0038] The present invention will be described in detail below with reference to the accompanying drawings and in conjunction with embodiments.
[0039] The low-stress high-speed milling diesel engine crankshaft processing technology method described in the present invention includes S1: tempering the blank, placing the blank in a vertical hoisting pit heating furnace for quenching, so that the hardness of the workpiece is between 302 and 363HB, and the tensile strength is between 980 and 1180MPa. Specifically, the material used for the crankshaft described in this embodiment is 34CrNiMo6 alloy steel, which is vertically hoisted in the pit heating furnace by a hanger and other tooling, and the blank is quenched by the pit heating furnace so that the cross section of each part of the crankshaft is evenly heated. The specific quenching parameters are: temperature The temperature is 860±10℃, the holding time is ≥6h, and the total time is 8h~9h. After the heating is completed, the crankshaft is hoisted into the quenching medium. In this embodiment, the quenching medium is AQ251 quenching liquid with a concentration of 10%-15%. After cooling for 9-13 minutes, the crankshaft is hoisted out of the quenching medium, or the quenching medium is emptied to allow the workpiece to be air-cooled to room temperature in the air, thereby adjusting the hardness of the crankshaft within the required value. Those skilled in the art should know that when other adopted blanks are used for processing, the quenching parameters can be adjusted accordingly according to the material properties.
[0040] S2: Rough machining of crankshaft journals. First, center holes are machined on both ends of the crankshaft. Then, a center point is used to support the center holes on both ends of the blank, or the outer wall of the crankshaft is clamped by a chuck to fix the position of the crankshaft. In the process of machining the crankshaft journals, a main journal at the end is first machined. Then, other main journals and connecting rod diameters are machined based on the main journal. Specifically, a center stand is used to fix the main journals from the starting end to the end of the crankshaft. After each main journal is fixed, the main journal on the side close to the end end and the main journal on the side close to the starting end are machined. The connecting rod neck is processed, and the crank arm surface of the processed main journal and the connecting rod neck is processed at the same time. More specifically, the processed main journal is first fixed by a fixing frame, and then the main journal on the side of the fixed main journal close to the end end and the crank arm surfaces at both ends of the processed main journal are processed by an internal milling cutter. When the third main journal is processed, the main journal and its crank arm surface on the side of the third main journal close to the end end and the connecting rod neck and its crank arm surface on the side close to the starting end can be processed. Taking the crankshaft to be processed in this application as an example, the specific processing sequence can refer to the following table:
[0041]
[0042]
[0043] During each machining process, two internal milling cutters are fixed on the machine tool at the same time, and the two internal milling cutters are used to simultaneously machine the positions to be machined at both ends of the fixed main shaft neck, thereby preventing the fixed main shaft neck from being deformed due to uneven force during machining. During the movement of the internal milling cutter, the cutting speed is 116m / min, the cutting depth is 0.1mm, and the feed rate is 0.08mm / r. Through dry cutting, the rotation speed of the crankshaft workpiece is 3min / r. Through low speed, small feed rate and small depth, cutting heat is avoided on the workpiece surface, and deformation caused by the machining process is avoided.
[0044] It should be noted that, in this embodiment, the starting end is the end where the crankshaft is connected to the gear, and the ending end is the flywheel end of the crankshaft.
[0045] S3: Rough machining heat treatment, use a horizontal heating furnace to temper the crankshaft after rough machining. Specifically, use a tool to make the crankshaft lie horizontally in the horizontal heating furnace, and make the position of the crankshaft's maximum circular runout at the highest point of the horizontal crankshaft. After raising the temperature in the horizontal heating furnace to 550° and keeping it warm for 5 hours, stop heating and make the furnace body and the crankshaft cool down to room temperature synchronously and naturally. During the tempering process, the hardness of the crankshaft is reduced. At the same time, since the maximum circular runout position is at the highest point, the circular runout of the crankshaft is corrected under the action of the crankshaft's own gravity, so as to improve the accuracy of subsequent fine machining.
[0046] S4: Spindle crank arm surface finishing, using a center stand to fix the spindle journal in sequence along the direction from the starting end to the end of the crankshaft, and after each fixation of the spindle journal, the spindle journal and the crank arm surfaces on both sides of the fixed spindle journal close to the end of the crankshaft are finished. The specific parameters in the finishing process can be set to a cutting speed of 116m / min, a cutting depth of 0.1mm, and a feed rate of 0.05mm / r. Dry cutting is used, and the crankshaft workpiece rotation speed is 2min / r. Moreover, due to the further reduction of the feed rate and the workpiece speed, the crankshaft deformation during the milling process is less, and another position in a single direction of the fixed spindle journal can be processed, and the vibration caused by simultaneous processing on both sides is avoided, further improving the processing accuracy. Taking the crankshaft processed in this application as an example, the specific processing sequence is shown in the following table:
[0047]
[0048]
[0049] S5: Finishing of connecting rod diameter crank arm surface, fix the main journal in sequence, and after each fixing of the main journal, finish the connecting rod diameter on the side of the fixed main journal close to the crankshaft starting end and the crank arm surfaces on both sides thereof. Specifically, its tool processing parameters are the same as the finishing parameters in the S4 spindle crank arm surface finishing, and will not be repeated here. By clamping and fixing the main journal and processing the connecting rod journal adjacent to the fixed main journal, the vibration of the crankshaft processing part during the processing is further reduced, and the processing accuracy is improved. Taking the crankshaft processed in this application as an example, the specific processing sequence is shown in the following table:
[0050] Milling sequence Cutting part Center frame support part 1 The first connecting rod neck and the left and right crank arm surfaces Second main journal 2 Second connecting rod neck and left and right crank arm surfaces The third main journal 3 The third connecting rod neck and the left and right crank arm surfaces Fourth main journal 4 Fourth connecting rod neck and left and right crank arm surfaces Fifth main journal 5 Fifth connecting rod neck and left and right crank arm surfaces Sixth main journal 6 Sixth connecting rod neck and left and right crank arm surfaces Seventh main journal 7 Seventh connecting rod neck and left and right crank arm surfaces Eighth main journal 8 The eighth connecting rod neck and the left and right crank arm surfaces Ninth main journal
[0051] S6: outer edge processing, the main journals are fixed in sequence, and after each fixing of the main journal, the outer edges of the crank arms of the two main journals adjacent to the fixed main journal are finely processed. Specifically, the main journal is fixed with a center frame, and the outer edges of the crank arms on both sides of the fixed main journal are processed, which improves the processing efficiency and makes the forces on both sides of the fixed main journal position similar, thereby reducing the deformation effect during the processing. Taking the crankshaft processed in this application as an example, the specific processing sequence is shown in the following table:
[0052] Milling sequence Cutting part Center frame support part 1 The outer edge of the first curved arm and the outer edge of the fourth curved arm Second main journal 2 The outer edge of the second curved arm and the outer edge of the sixth curved arm The third main journal 3 The outer edge of the third curved arm and the outer edge of the seventh curved arm The third main journal 4 Outer edge of the fifth curved arm, outer edge of the eighth curved arm Fourth main journal 5 The outer edge of the twelfth arm and the outer edge of the ninth arm Sixth main journal 6 The outer edge of the 14th arm and the outer edge of the 10th arm Seventh main journal 7 The outer edge of the fifteenth arm and the outer edge of the eleventh arm Seventh main journal 8 The outer edge of the 16th arm and the outer edge of the 13th arm Eighth main journal
[0053] S7: Heat treatment of the workpiece. A horizontal heating furnace is used to temper the crankshaft after fine machining. Specifically, the crankshaft is placed horizontally in the horizontal heating furnace using a tool, and the position with the largest circular runout of the crankshaft is located at the highest point of the horizontal crankshaft. The temperature in the horizontal heating furnace is increased by 550° and kept warm for 5 hours, then the heating is stopped to allow the furnace body and the crankshaft to cool down to room temperature naturally. During the tempering process, the hardness of the crankshaft is reduced. At the same time, since the position of the maximum circular runout is at the highest point, the circular runout of the crankshaft is corrected under the action of the crankshaft's own gravity, so that the circular runout of the crankshaft meets the processing requirements while reducing the internal stress of the crankshaft, laying a good foundation for subsequent grinding and induction quenching processes, making it easier for subsequent processing, improving the stability of the dimensional accuracy of the final crankshaft product, and improving the quality of the crankshaft product and the overall processing efficiency of the crankshaft.
[0054] The low-stress high-speed milling diesel engine crankshaft processing technology method described in the present invention adopts an internal milling cutter to process the main journal, connecting rod journal and crank arm surface of the crankshaft in order to further improve the processing efficiency. The internal milling cutter is provided with two groups of rounded corner cutter discs and multiple groups of right-angle cutter discs along the axial direction, and the right-angle cutter discs are placed between the two groups of rounded corner cutter discs. The rounded corner cutter disc is fixed with multiple rounded corner blades, and the right-angle cutter disc is fixed with multiple right-angle blades. The right-angle blades or rounded corner blades in adjacent right-angle cutter discs and rounded corner cutter discs are staggered, so as to facilitate the discharge of metal waste after milling.
[0055] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.
Claims
1. A low-stress high-speed milling diesel engine crankshaft processing technology method, Features: include S1: The blank is quenched and tempered, and the blank is placed in a vertically hoisted pit heating furnace for quenching, so that the hardness of the workpiece is between 302 and 363HB, and the tensile strength is between 980 and 1180MPa; S2: Rough machining of crankshaft journals. Use a center point to hold the center holes at both ends of the blank and fix the main journals in sequence. After each main journal is fixed, the main journal on the side close to the end end and the connecting rod journal on the side close to the starting end of the fixed main journal are machined, and the crank arm surfaces of the machined main journal and connecting rod journal are machined at the same time. S3: Rough machining heat treatment, using a horizontal heating furnace to temper the crankshaft after rough machining; S4: Finishing the spindle crank arm surface, fixing the main journals respectively, and after each fixing of the main journal, finishing the main journal on the side of the fixed main journal close to the end of the crankshaft and the crank arm surfaces on both sides thereof; S5: Finishing of connecting rod diameter crank arm surface, fixing the main journals in sequence, and after each fixing of the main journals, finishing of the connecting rod diameter on the side of the fixed main journal close to the crankshaft starting end and the crank arm surfaces on both sides thereof; S6: outer edge processing, fixing the main shaft journals in sequence, and after each fixing of the main shaft journal, finishing the outer edges of the crank arms of the two main shaft journals adjacent to the fixed main shaft journal; S7: Heat treatment of workpiece: tempering of the finished crankshaft in a horizontal heating furnace.
2. A low stress high speed milling diesel engine crankshaft processing technology method according to claim 1, Features: In step S2, the order of rough machining the crankshaft journal is to process from the starting end to the end of the crankshaft in sequence; In steps S5 and S6, the finishing order of the main shaft crank arm surface and the connecting rod crank arm surface is to process them successively from the starting end to the end end of the crankshaft.
3. A low stress high speed milling diesel engine crankshaft processing technology method according to claim 1, Features: In step S2, the crankshaft is rough-machined by an internal milling cutter at a cutting speed of 116 m / min, a cutting depth of 0.1 mm, and a feed rate of 0.08 mm / r. The crankshaft workpiece rotates at a speed of 3 min / r by dry cutting.
4. A low stress high speed milling diesel engine crankshaft processing technology method according to claim 1, Features: In steps S5 and S6, an internal milling cutter is used to finish the crankshaft at a cutting speed of 116 m / min, a cutting depth of 0.1 mm, a feed rate of 0.05 mm / r, and a dry cutting method. The crankshaft workpiece rotation speed is 2 min / r.
5. A low stress high speed milling diesel engine crankshaft processing technology method according to claim 1, Features: In steps S2, S4 and S5, the workpiece is processed by an internal milling cutter respectively, and the internal milling cutter is provided with two groups of rounded corner cutter discs and multiple groups of right-angle cutter discs along the axial direction, and the right-angle cutter discs are placed between the two groups of rounded corner cutter discs, the rounded corner cutter disc is fixed with multiple rounded corner blades, the right-angle cutter disc is fixed with multiple right-angle blades, and the right-angle blades or rounded corner blades in adjacent right-angle cutter discs and rounded corner cutter discs are staggered.
6. A low stress high speed milling diesel engine crankshaft processing technology method according to claim 1, Features: In step S2, two internal milling cutters are used to simultaneously machine the main journal near the rear end and the connecting rod diameter near the starting end of the fixed main journal.
7. A low stress high speed milling diesel engine crankshaft processing technology method according to claim 1, Features: In step S6, two groups of internal milling cutters are used to simultaneously machine the outer edges of the crank arms of the adjacent main journals on both sides of the fixed main journal.
8. A low stress high speed milling diesel engine crankshaft processing technology method according to claim 1, Features: The tempering treatment in step S3 and step S7 is to place the processed semi-finished workpiece in a horizontal heating furnace, and place the point with the largest crankshaft circular runout at the highest point of the workpiece. The temperature in the heating furnace is 550°, kept warm for 5 hours, and then cooled to room temperature with the furnace.
9. A low stress high speed milling diesel engine crankshaft processing technology method according to claim 1, Features: In step S1, the quenching temperature is 860±10°C, the holding time is ≥6h, and the total time is 8h~9h. Then the workpiece is placed in the cooling medium and cooled for 9-13min, and then air-cooled to room temperature.
10. A low stress high speed milling diesel engine crankshaft processing technology method according to claim 9, Features: The cooling medium is AQ251 quenching liquid with a concentration of 10-15%.
Citation Information
Patent Citations
Small-displacement internal combustion engine crankshaft preparation method
CN105798558A
Center rack for clamping main journal of crankshaft
CN112296695A
Heat treatment method for high-bearing slender hollow crankshaft
CN117512317A
Crankshaft main coupling journal and balance block end face machining equipment
CN212310947U
Verfahren zur Bearbeitung der Hubzapfen und Mittellager einer Kurbelwelle
GB1230712A