Grinding process method for inhibiting grinding cracks on subsurface of bearing raceway
By increasing the linear speed of the grinding wheel and controlling the maximum undeformed chip thickness, the problem of grinding cracks in the traditional bearing raceway grinding process is solved, the fatigue life and grinding quality of the bearing are significantly improved, and more scientific and precise grinding is achieved. Craftsmanship.
Patent Information
- Application Number
- CN202410901355.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-05
- Publication Date
- 2024-10-15
AI Technical Summary
The traditional bearing raceway grinding process lacks control over the integrity of the raceway surface and subsurface, resulting in grinding crack problems and affecting the fatigue life of the bearing. The process parameters are not designed scientifically, making it difficult to effectively suppress the generation and expansion of grinding cracks.
The linear speed of the grinding wheel is not less than 60m/s, and the maximum undeformed chip thickness is controlled through a mathematical model under low-speed conditions to ensure that it is within a reasonable range. The grinding process parameters are designed to suppress subsurface grinding cracks in the bearing raceway.
It significantly improves the fatigue life and grinding quality of the bearing, reduces the occurrence of grinding cracks, improves the stability and consistency of the grinding process, and narrows the life gap with imported bearings.
Smart Images

Figure CN118769073A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of bearing manufacturing, and in particular relates to a grinding process method for suppressing sub-surface grinding cracks of a bearing raceway. Background Art
[0002] Bearing raceway grinding is one of the most critical processes in bearing manufacturing. The grinding quality of the raceway will directly affect the performance and fatigue life of the bearing. Traditional bearing raceway grinding usually only considers dimensional tolerances, form and position tolerances, and surface roughness, and does not consider surface integrity issues such as raceway sub-surface grinding cracks caused by grinding. The surface integrity defects of the raceway will greatly shorten the fatigue life of the bearing. Since traditional bearing manufacturing lacks key surface integrity indicators to control the surface quality of the bearing raceway, and lacks process methods to regulate key indicators, the fatigue life of domestic bearings is much lower than that of internationally renowned brands. Therefore, in response to the demand for improving bearing fatigue life, it is necessary to provide key indicators that affect bearing fatigue life, namely raceway sub-surface grinding cracks and their characterization parameters, as well as process methods to suppress grinding cracks.
[0003] The existing technology has the following key technical problems in the bearing raceway grinding process, which directly affect the performance and fatigue life of the bearing:
[0004] 1) Lack of surface integrity control:
[0005] The traditional bearing raceway grinding process mainly focuses on dimensional tolerance, geometric tolerance and surface roughness, while ignoring the impact of the grinding process on the raceway surface and sub-surface integrity. Surface defects such as grinding cracks will significantly shorten the fatigue life of the bearing, but these key surface integrity indicators have not been effectively controlled and monitored in traditional processes.
[0006] 2) Impact of surface integrity defects:
[0007] Defects such as grinding cracks on the raceway surface will become the starting point of fatigue cracks during bearing operation, leading to early failure. These surface defects greatly reduce the fatigue life of bearings, making domestic bearings far behind internationally renowned brands in terms of service life. However, traditional manufacturing processes lack effective control methods for these defects.
[0008] 3) Lack of scientific process parameter design:
[0009] In the traditional bearing raceway grinding process, the design of process parameters is often based on experience and simple tolerance control, lacking scientific mathematical models and control methods. In this case, it is difficult to ensure that the key parameters of the grinding process (such as grinding wheel speed, grinding depth, chip thickness, etc.) are within the optimal range, resulting in unstable grinding quality and difficulty in controlling sub-surface cracks.
[0010] 4) Insufficient systematic and scientific process methods:
[0011] The current bearing manufacturing process lacks a systematic and scientific process to control and regulate key indicators of surface integrity, especially the generation and expansion of grinding cracks. The lack of such a process makes it difficult to effectively suppress grinding cracks during the bearing manufacturing process, thereby improving the fatigue life of the bearing.
[0012] The existing technology in the bearing raceway grinding process has problems such as insufficient surface integrity control, the negative impact of surface defects on fatigue life has not been effectively solved, the process parameter design is unscientific, and there is a lack of effective process control methods. These problems seriously restrict the performance and life improvement of domestic bearings. Therefore, it is particularly important to propose targeted solutions and processes for these technical problems. Summary of the invention
[0013] In view of the problems existing in the prior art, the present invention provides a grinding process method for suppressing sub-surface grinding cracks of a bearing raceway.
[0014] The present invention is implemented as follows: (1) a grinding process method for suppressing sub-surface grinding cracks of a bearing raceway, wherein the grinding wheel linear speed generally is not less than 60 m / s; and (2) in the grinding process method for suppressing sub-surface grinding cracks of a bearing raceway, when the grinding wheel linear speed is less than 60 m / s, the design of the grinding process method parameters should meet the control requirements of the maximum undeformed chip thickness.
[0015] Furthermore, (3) the maximum undeformed chip thickness of bearing raceway grinding is expressed as a gmax It is characterized by that a gmax As the key control parameter for suppressing the grinding cracks of the bearing raceway subsurface, the maximum undeformed chip thickness needs to meet a gmax gmax * Here, under the condition that the bearing material is high carbon chromium alloy (DIN100Cr6) and ceramic sintered corundum grinding wheel (Saint-Gobain-Norton), a gmax * The value range is a gmax * ≤1.10μm.
[0016] Further, (4) when the grinding wheel speed is lower than 60 m / s, the design of the grinding process parameters should meet the control requirements of the maximum undeformed chip thickness, that is:
[0017]
[0018] In the formula, v w is the workpiece speed, v s is the grinding wheel speed, a p is the cutting depth, d s is the grinding wheel diameter, d w is the workpiece diameter, λ sl is the distance between consecutive cutting edges.
[0019] Another object of the present invention is to provide a method for evaluating the sub-surface grinding cracks of the bearing raceway, including the length and depth of the sub-surface grinding cracks of the bearing raceway.
[0020] Furthermore, the bearing raceway subsurface grinding crack measurement indicators include the length L of the bearing raceway subsurface grinding crack and the depth D of the bearing raceway subsurface grinding crack.
[0021] In combination with the above technical solutions and the technical problems solved, the advantages and positive effects of the technical solutions to be protected by the present invention are as follows:
[0022] First, the present invention includes a grinding process method for suppressing subsurface grinding cracks of a bearing raceway and a method for evaluating subsurface grinding cracks of a bearing raceway. The bearing raceway grinding process method mainly includes a combination method of grinding process parameters, and control requirements for grinding wheel speed and maximum undeformed chip thickness.
[0023] Second, the present invention can effectively suppress grinding cracks in bearing raceway grinding, overcome the problems of poor grinding quality of rolling bearing raceway surface and difficulty in reasonably optimizing grinding process parameters, and provide reasonable and effective machining process methods and process parameters for improving the service performance and fatigue life of high-end bearing products. By effectively suppressing grinding cracks in the sub-surface of the bearing raceway, the present invention can significantly improve the long-term stability of the actual operation of the bearing and its fatigue life, and narrow the life gap with imported high-end bearings.
[0024] Third, as auxiliary evidence of the inventiveness of the claims of the present invention, it is also reflected in the following important aspects:
[0025] (1) The grinding process of the bearing raceway proposed in the present invention effectively suppresses the grinding cracks on the sub-surface of the bearing raceway, and can usually significantly increase the actual test life of the bearing. In engineering practice, the actual test life range of the bearing manufactured using the technical solution of the present invention is sometimes relatively large. The reason is that there are many parts processing and assembly processes for the bearing, and the production environment of each process, the processing errors of the bearing-related parts, the stability of the automatic loading and unloading mechanism, the wear of the grinding wheel and other process conditions cause inconsistencies and instabilities.
[0026] (2) The technical solution of the present invention overcomes the traditional technical prejudice in bearing manufacturing and breaks through the existing process technology and methods.
[0027] (3) The expected benefits and commercial value of the technical solution of the present invention after transformation are:
[0028] Taking the test bearing model 7002P4 used for fatigue life test of the present invention as an example, since there is a big gap between the fatigue life of domestic bearings, especially high-end bearings and international famous brand bearings, according to the current market price, the price of international famous brand bearings (such as NSK) is generally 3 times or more than that of domestic bearings.
[0029] In summary, the process method proposed in the present invention will significantly improve the fatigue life of domestic bearings and bring huge profits and commercial value to enterprises.
[0030] Fourth, the present invention effectively solves the problem of sub-surface grinding cracks on the bearing raceway in the prior art by introducing the grinding wheel linear speed and the maximum undeformed chip thickness as key control parameters. In the traditional grinding process, due to the lack of precise control of key parameters, cracks are easily caused on the surface and sub-surface of the bearing raceway, affecting its service life and performance. Under the conditions of high-carbon chromium alloy and ceramic sintered corundum grinding wheels, the present invention significantly reduces the occurrence of sub-surface cracks by increasing the grinding wheel linear speed to not less than 60m / s, thereby improving the grinding quality and efficiency.
[0031] When the grinding wheel linear speed is lower than 60m / s, the present invention further optimizes the grinding process by taking the maximum undeformed chip thickness as the key control parameter. Under low-speed grinding conditions, it is difficult for traditional methods to effectively control the generation of subsurface cracks. However, the present invention accurately calculates the maximum undeformed chip thickness through a mathematical model to ensure that it meets a reasonable value range, thereby effectively suppressing subsurface cracks. This control method based on chip thickness makes the grinding process more scientific and precise.
[0032] In the present invention, the specific grinding process parameter design is realized by a mathematical model. The model describes the relationship between the grinding wheel speed, the workpiece speed, the grinding depth, the continuous cutting edge spacing of the grinding wheel, the grinding wheel diameter and the workpiece diameter, and ensures that the maximum undeformed chip thickness is controlled within a reasonable range through calculation. Such parameter design not only optimizes the grinding process, but also significantly improves the stability and consistency of the process, and reduces the quality problems caused by parameter fluctuations.
[0033] Through practical application verification, the present invention significantly reduces the length and depth of the sub-surface grinding cracks of the bearing raceway under the conditions of high-carbon chromium alloy and ceramic sintered corundum grinding wheel. Compared with the traditional process, the grinding process of the present invention shows significant technical progress in improving surface quality and reducing cracks. By using scientific parameter design and strict control methods, the present invention provides an efficient and reliable grinding process for the bearing manufacturing industry, significantly extending the service life of the bearing and improving its operating reliability and safety. BRIEF DESCRIPTION OF THE DRAWINGS
[0034] Figure 1 It is a flow chart of a grinding process method for suppressing sub-surface grinding cracks of a bearing raceway provided by an embodiment of the present invention;
[0035] Figure 2 Schematic diagram of a bearing raceway subsurface grinding crack evaluation method provided by an embodiment of the present invention;
[0036] Figure 3 It is a schematic diagram of a sub-surface grinding crack of a bearing raceway provided in an embodiment of the present invention. DETAILED DESCRIPTION
[0037] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.
[0038] like Figure 1 As shown, the grinding process method for suppressing sub-surface grinding cracks of a bearing raceway provided by an embodiment of the present invention comprises the following steps:
[0039] S101: The grinding wheel linear speed used is not less than 60m / s;
[0040] S102: When the grinding wheel speed is lower than 60m / s, the design of grinding process parameters should meet the control requirements of the maximum undeformed chip thickness.
[0041] The grinding process method for suppressing sub-surface grinding cracks of a bearing raceway provided in an embodiment of the present invention adopts a grinding wheel linear speed of not less than 60 m / s; when the grinding wheel linear speed is less than 60 m / s, the grinding process parameter design should meet the control requirements of the maximum undeformed chip thickness, and the maximum undeformed chip thickness of the bearing raceway grinding is a gmax express;
[0042]
[0043] The maximum undeformed chip thickness needs to meet a gmax gmax * , a gmax * The value range is a gmax * ≤1.10μm.
[0044] It should be noted that the embodiments of the present invention can be implemented by hardware, software, or a combination of software and hardware. The hardware part can be implemented using dedicated logic; the software part can be stored in a memory and executed by an appropriate instruction execution system, such as a microprocessor or dedicated design hardware. It can be understood by a person of ordinary skill in the art that the above-mentioned devices and methods can be implemented using computer executable instructions and / or contained in a processor control code, such as a carrier medium such as a disk, CD or DVD-ROM, a programmable memory such as a read-only memory (firmware), or a data carrier such as an optical or electronic signal carrier. Such code is provided on the carrier medium. The device and its modules of the present invention can be implemented by hardware circuits such as very large-scale integrated circuits or gate arrays, semiconductors such as logic chips, transistors, etc., or programmable hardware devices such as field programmable gate arrays, programmable logic devices, etc., can also be implemented by software executed by various types of processors, and can also be implemented by a combination of the above-mentioned hardware circuits and software, such as firmware.
[0045] The above description is only a specific implementation mode of the present invention, but the protection scope of the present invention is not limited thereto. Any modifications, equivalent substitutions and improvements made by any technician familiar with the technical field within the technical scope disclosed by the present invention and within the spirit and principle of the present invention should be covered by the protection scope of the present invention.
Claims
1. A grinding process method for suppressing sub-surface grinding cracks of a bearing raceway, characterized in that: Under the condition that the bearing material is a high carbon chromium alloy and a ceramic sintered corundum grinding wheel, the grinding process method for suppressing the sub-surface grinding cracks of the bearing raceway generally adopts a grinding wheel linear speed of not less than 60m / s; when the grinding wheel linear speed is less than 60m / s, the maximum undeformed chip thickness a should be gmax As the key control parameter of bearing raceway subsurface grinding cracks.
2. The grinding process method for suppressing sub-surface grinding cracks of a bearing raceway according to claim 1, characterized in that: When the grinding wheel speed is lower than 60m / s, the maximum undeformed chip thickness a that can be ground on the bearing raceway gmax As a key control parameter for suppressing subsurface grinding cracks in bearing raceways, the maximum undeformed chip thickness needs to satisfy a gmax gmax * , a gmax * The value range is a gmax * ≤1.10μm. 3. The grinding process method for suppressing sub-surface grinding cracks of a bearing raceway according to claim 1, characterized in that: When the grinding wheel speed is lower than 60 m / s, the bearing raceway grinding process parameters should meet the maximum undeformed chip thickness a gmax The regulatory requirements are: In the formula, v s is the grinding wheel speed, v w is the workpiece speed, a p is the grinding depth of cut, λ sl is the distance between the continuous cutting edges of the grinding wheel, d s is the grinding wheel diameter, d w is the workpiece diameter.
4. The grinding process method for suppressing sub-surface grinding cracks of a bearing raceway according to claim 1, characterized in that: The sub-surface grinding crack of the bearing raceway can be characterized by the length L of the sub-surface grinding crack of the bearing raceway and the depth D of the sub-surface grinding crack of the bearing raceway.
Citation Information
Patent Citations
Bearing raceway high-speed grinding method considering surface integrity, parameters and application
CN117161834A
Cited By
Low-damage and high-efficiency machining method for array composite pipe component
CN120680355A