Binder for sintering and method for producing ceramic sintered compact

The use of core-shell particles with an elastic core and hydroxyl/carboxyl-containing shell in the sintering binder addresses the issue of cracks and chips in conventional methods, enabling low-temperature, high-density ceramic production.

JP2024145009AInactive Publication Date: 2024-10-15KANEKA CORP

Patent Information

Application Number
JP2023057226
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-31
Publication Date
2024-10-15
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Conventional ceramic sintering methods using polyvinyl alcohol as a molding aid result in cracks and chips during degreasing, and there is a need for a low-temperature sintering process that produces high-density ceramic sintered bodies with minimal organic residue.

Method used

A sintering binder comprising core-shell particles with an elastic core layer and a shell layer containing hydroxyl and carboxyl groups, allowing for low-temperature degreasing and high-density ceramic production.

Benefits of technology

The binder enables low-temperature sintering with high degradability, reducing organic residue and preventing cracks, resulting in high-density ceramic sintered bodies.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024145009000001_ABST
    Figure 2024145009000001_ABST
Patent Text Reader

Abstract

To provide a binder for sintering ceramics which can be sintered at a low temperature, has high degradability, and can obtain a high-density ceramic sintered compact in the production of the ceramic sintered compact.SOLUTION: A binder for sintering ceramics comprises core-shell particles having an elastic core layer and a shell layer covering the elastic core layer. The shell layer comprises a polymer having at least one functional group of a hydroxyl group and a carboxyl group.SELECTED DRAWING: Figure 2
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a sintering binder and a method for producing a ceramic sintered body. [Background technology]

[0002] Fine ceramics are used as electronic materials, structural materials, medical materials, etc., and there is a demand for low-cost, environmentally friendly manufacturing technologies.

[0003] Normally, ceramics require a process in which raw material powder is mixed with a molding aid (organic material) and then molded. Polyvinyl alcohol (PVA) has traditionally been used as such a molding aid. Although molding aids are necessary for molding, if organic matter remains in the final ceramic product, it will deteriorate the product's performance, so they are unnecessary components in ceramic products. Therefore, in ceramics manufacturing, degreasing is performed after molding to remove the molding aid.

[0004] For example, a sintering binder resin composition has been proposed that has excellent sinterability and binder removal properties, and has high elongation and flexibility as well as film strength particularly when formed into a sheet, and is excellent in handleability, workability, and processability when molded. The sintering binder resin composition contains a resin component in which at least one monomer of an alkyl (meth)acrylate and a heterocycle-containing (meth)acrylate is copolymerized with a hydroxyl group-containing (meth)acrylate (see Patent Document 1).

[0005] From the viewpoint of low environmental impact, degreasing using the superheated steam method has been attracting attention in recent years. However, when conventional molding aids, especially polyvinyl alcohol (PVA), are degreased using the superheated steam method, there is a problem that cracks and chips occur in the ceramic sintered body. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] JP 2014-47338 A Summary of the Invention [Problem to be solved by the invention]

[0007] The present invention aims to solve the above-mentioned problems in the prior art and to achieve the following object: That is, the present invention aims to provide a ceramic sintering binder that can be sintered at a low temperature in the production of a ceramic sintered body, has high decomposability, and can produce a high-density ceramic sintered body. [Means for solving the problem]

[0008] The means for solving the above problems are as follows: That is, the sintering binder of the present invention is a binder for sintering ceramics, and is characterized in that it contains core-shell particles having an elastic core layer and a shell layer that covers the elastic core layer, and the shell layer contains a polymer having at least one functional group of a hydroxyl group and a carboxyl group. Effect of the Invention

[0009] According to the present invention, it is possible to solve the above-mentioned problems in the conventional art and achieve the above-mentioned object, and it is possible to provide a binder for sintering ceramics that can be sintered at a low temperature in the production of a sintered ceramic body, and that can give a highly decomposable and high-density sintered ceramic body. [Brief description of the drawings]

[0010] [Figure 1A] FIG. 1A is a diagram showing an example of the appearance of a molded product molded into a tablet shape before degreasing (after molding), a ceramic sintered precursor after degreasing, and a ceramic sintered body tablet after sintering in Example 1. [Figure 1B]FIG. 1B is a diagram showing an example of the appearance of a molded product molded into a tablet shape before degreasing (after molding), a ceramic sintered precursor after degreasing, and a ceramic sintered body tablet after sintering in Example 2. [Figure 1C] FIG. 1C is a diagram showing an example of the appearance of a molded product molded into a tablet shape before degreasing (after molding), a ceramic sintered precursor after degreasing, and a ceramic sintered body tablet after sintering in Example 3. [Figure 1D] FIG. 1D is a diagram showing an example of the appearance of a molded product molded into a tablet shape before degreasing (after molding), a ceramic sintered precursor after degreasing, and a ceramic sintered body tablet after sintering in Example 4. [Figure 1E] FIG. 1E is a diagram showing an example of the appearance of a molded product molded into a tablet shape before degreasing (after molding), a ceramic sintered precursor after degreasing, and a ceramic sintered body tablet after sintering in Example 5. [Figure 1F] FIG. 1F is an enlarged photograph of FIG. 1E showing the appearance of the degreased ceramic sintering precursor and the sintered ceramic sintered body tablet molded into a tablet shape in Example 5. [Figure 1G] FIG. 1G is a diagram showing an example of the appearance of a molded product molded into a tablet shape before degreasing (after molding), a ceramic sintered precursor after degreasing, and a ceramic sintered body tablet after sintering in Comparative Example 1. [Diagram 2] 2 is a graph showing the relationship between mass change and temperature in the degreasing steps of Examples 1, 2, and 4, and Comparative Example 1. The vertical axis shows mass change (mass%), and the horizontal axis shows degreasing temperature (° C.). DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] (sintering binder) The sintering binder of the present invention is a binder for sintering ceramics, and contains core-shell particles having an elastic core layer and a shell layer covering the elastic core layer, and the shell layer contains a polymer having at least one functional group selected from the group consisting of a hydroxyl group and a carboxyl group. The sintering binder of the present invention may further contain other components in addition to the core-shell particles, as necessary.

[0012] Since the sintering binder of the present invention contains the core-shell particles, it can be degreased at a low temperature compared to polyvinyl alcohol (PVA), which has been conventionally used as a sintering binder for ceramics, and therefore has excellent energy efficiency, less organic matter remains in the molded product after degreasing, and the molded product after degreasing has excellent shape retention, and furthermore, it is possible to obtain a high-density ceramic sintered body.

[0013] <Core-shell particles> The core-shell particle has an elastic core layer, a shell layer covering the elastic core layer, and further has other layers as necessary.

[0014] <<Elastic core layer>> The elastic core layer is covered with the shell layer, and therefore exists as the bottom layer (innermost layer) of the core-shell particle.

[0015] In this specification, "elasticity" means a property that distortion occurs when stress is applied, but returns to the original dimensions when the load is removed. The elasticity of the elastic core layer gives the core-shell particles rubber-like properties. Therefore, the elastic core layer of the core-shell particles is preferably made of a rubber-like polymer having rubber properties. This allows the ceramic sintered body obtained by using the ceramic sintering binder to have a high density.

[0016] Examples of the rubber-like polymer constituting the elastic core layer include natural rubber, polysiloxane rubber, diene rubber obtained by polymerizing a conjugated diene monomer as a main monomer (hereinafter sometimes referred to as a "first monomer"), and (meth)acrylic rubber obtained by polymerizing a (meth)acrylate monomer as a first monomer. Also, the polymer may be a polymer obtained by polymerizing these first monomers with vinyl monomers such as aromatic vinyl monomers and vinylcyan monomers (hereinafter sometimes referred to as a "second monomer"). These may be used alone or in combination of two or more. Among these, diene rubber and (meth)acrylic rubber are preferred, and (meth)acrylic rubber is more preferred, from the viewpoint of increasing the density of the ceramic sintered body obtained by using the ceramic sintering binder.

[0017] -Polysiloxane rubber- The polysiloxane rubber is not particularly limited and can be appropriately selected depending on the purpose. For example, polysiloxane-based polymers composed of alkyl or aryl di-substituted silyloxy units such as dimethylsilyloxy units, diethylsilyloxy units, methylphenylsilyloxy units, diphenylsilyloxy units, and dimethylsilyloxy-diphenylsilyloxy units, and polysiloxane-based polymers composed of alkyl or aryl mono-substituted silyloxy units such as organohydrogensilyloxy units in which a part of the alkyl in the side chain is substituted with a hydrogen atom can be mentioned. These may be used alone or in combination of two or more. Among these, polymers composed of dimethylsilyloxy units are more preferable because they are easily available and economical.

[0018] -Conjugated diene monomer- The conjugated diene monomer (first monomer) is not particularly limited and can be appropriately selected depending on the purpose, and examples thereof include butadienes such as 1,3-butadiene, 2-chloro-1,3-butadiene, and 2-methyl-1,3-butadiene, isoprene, etc. These may be used alone or in combination of two or more kinds.

[0019] -(Meth)acrylate monomer- When the elastic core particle contains a (meth)acrylate rubber, a wide range of polymer designs for the elastic body are possible by combining a variety of monomers.

[0020] The (meth)acrylate monomer (first monomer) is not particularly limited and can be appropriately selected depending on the purpose, and examples thereof include alkyl (meth)acrylate, aromatic ring-containing (meth)acrylate, hydroxyalkyl (meth)acrylate, glycidyl (meth)acrylate, alkoxyalkyl (meth)acrylate, allylalkyl (meth)acrylate, polyfunctional (meth)acrylate, etc. These may be used alone or in combination of two or more.

[0021] Examples of the alkyl (meth)acrylate include methyl (meth)acrylate, ethyl (meth)acrylate, butyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, octyl (meth)acrylate, dodecyl (meth)acrylate, stearyl (meth)acrylate, and behenyl (meth)acrylate.

[0022] Examples of the aromatic ring-containing (meth)acrylate include phenoxyethyl (meth)acrylate and benzyl (meth)acrylate.

[0023] Examples of the hydroxyalkyl (meth)acrylate include 2-hydroxyethyl (meth)acrylate and 4-hydroxybutyl (meth)acrylate.

[0024] Examples of the glycidyl (meth)acrylate include glycidyl (meth)acrylate and glycidyl alkyl (meth)acrylate.

[0025] Examples of the alkoxyalkyl (meth)acrylate include 2-methoxymethyl (meth)acrylate, 2-methoxyethyl (meth)acrylate, 2-ethoxymethyl (meth)acrylate, 2-ethoxyethyl (meth)acrylate, 3-methoxypropyl (meth)acrylate, 3-ethoxypropyl (meth)acrylate, 4-methoxybutyl (meth)acrylate, and 4-ethoxybutyl (meth)acrylate.

[0026] Examples of the allyl alkyl (meth)acrylate include allyl (meth)acrylate and allyl alkyl (meth)acrylate.

[0027] Examples of the polyfunctional (meth)acrylate include monoethylene glycol di(meth)acrylate, triethylene glycol di(meth)acrylate, and tetraethylene glycol di(meth)acrylate.

[0028] The glass transition temperature (Tg) of the (meth)acrylic rubber is not particularly limited and may be appropriately selected depending on the purpose, but is preferably less than 0° C., more preferably −10° C. or lower, and even more preferably −40° C. or lower. When the (meth)acrylic rubber has a glass transition temperature (Tg) of 0° C. or lower, the effect of increasing the density of the ceramic sintered body obtained by using the ceramic sintering binder is enhanced.

[0029] The glass transition temperature (Tg) of the (meth)acrylic rubber can be measured by a differential scanning calorimeter (DSC). The glass transition temperature of the (meth)acrylic rubber in the present invention is the lowest peak temperature measured by DSC measurement.

[0030] -Vinyl monomers- The vinyl monomer (second monomer) copolymerizable with the first monomer is not particularly limited and can be appropriately selected depending on the purpose, and examples thereof include vinyl arene, vinyl carboxylic acid, vinyl cyan, vinyl halide, alkene, polyfunctional monomer, etc. These may be used alone or in combination of two or more.

[0031] Examples of the vinyl arenes include styrene, α-methylstyrene, monochlorostyrene, and dichlorostyrene. Examples of the vinyl carboxylic acids include acrylic acid and methacrylic acid. Examples of the vinyl cyanides include acrylonitrile and methacrylonitrile. Examples of the vinyl halides include vinyl chloride, vinyl bromide, and chloroprene. Examples of the alkenes include vinyl acetate, ethylene, propylene, butylene, and isobutylene. Among these, the vinyl monomer is preferably vinyl arenes, and more preferably styrene.

[0032] In order for the elastic core layer to suitably have rubber properties, the rubber-like polymer constituting the elastic core layer is preferably a crosslinked rubber polymer having a crosslinked structure.

[0033] [Cross-linked structure of elastic core layer] The method for introducing a crosslinked structure into the rubber-like polymer is not particularly limited and may be appropriately selected from commonly used methods. For example, a method may be used in which a crosslinkable monomer such as a polyfunctional monomer described below is added to a polymer component obtained by polymerizing the monomer, followed by polymerization.

[0034] The gel content of the elastic core layer is not particularly limited and can be appropriately selected depending on the purpose. However, since the elastic core layer has rubber properties, it is preferably 60% by mass or more, more preferably 80% by mass or more, even more preferably 90% by mass or more, and particularly preferably 95% by mass or more.

[0035] In this specification, the method for calculating the gel content is as follows. First, 2 g of the core-shell particles (powder) is dissolved in 50 mL of methyl ethyl ketone (MEK). The obtained MEK solution is then separated into a component soluble in MEK (MEK soluble matter) and a component insoluble in MEK (MEK insoluble matter). Specifically, the obtained MEK solution is centrifuged at a rotation speed of 30,000 rpm for 1 hour using a centrifuge (e.g., CP60E, manufactured by Hitachi Koki Co., Ltd.), and the solution is separated into a MEK soluble matter and a MEK insoluble matter. Here, a total of three sets of centrifugation are performed. The weights of the obtained MEK soluble matter and MEK insoluble matter are measured, and the gel content is calculated according to the following formula. Gel content (%) = (mass of methyl ethyl ketone insoluble matter) / {(mass of methyl ethyl ketone insoluble matter) + (mass of methyl ethyl ketone soluble matter)} × 100

[0036] -Polyfunctional monomer- The polyfunctional monomer is not particularly limited and can be appropriately selected depending on the purpose, and examples thereof include allyl alkyl (meth)acrylate, polyfunctional (meth)acrylate, aromatic polycarboxylic acid ester, cyanuric acid derivative, aromatic vinyl polyfunctional monomer, etc. These may be used alone or in combination of two or more.

[0037] Examples of the allyl alkyl (meth)acrylate include allyl (meth)acrylate and allyl alkyl (meth)acrylate. Examples of the polyfunctional (meth)acrylate include butanediol di(meth)acrylate, ethylene glycol di(meth)acrylate, triethylene glycol di(meth)acrylate, and tetraethylene glycol di(meth)acrylate. Examples of the aromatic polycarboxylic acid ester include diallyl phthalate. Examples of the cyanuric acid derivative include triallyl cyanurate and triallyl isocyanurate. Examples of the aromatic vinyl polyfunctional monomer include divinylbenzene. Among these, the polyfunctional monomer is preferably an allyl alkyl (meth)acrylate, and more preferably an allyl (meth)acrylate. In this specification, the polyfunctional monomer for introducing a crosslinked structure into the rubber-like polymer does not include butadiene, isoprene, and the like as the conjugated diene monomer (first monomer).

[0038] The shape of the elastic core layer is not particularly limited and may be appropriately selected depending on the purpose, but is preferably spherical.

[0039] When the elastic core layer has a spherical shape, the volume average particle size (Mv) of the elastic core layer is not particularly limited and can be appropriately selected depending on the purpose, but is preferably 0.03 μm to 2 μm, more preferably 0.05 μm to 1 μm, and even more preferably 0.05 μm to 0.5 μm. It is often difficult to stably obtain an elastic core layer having a volume average particle size of less than 0.03 μm. In addition, when the volume average particle size of the elastic core layer is 0.5 μm or less, the density of the ceramic sintered body is easily improved.

[0040] The volume average particle size of the elastic core layer can be measured using a particle size distribution measuring device (for example, Microtrac UPA 150, manufactured by Nikkiso Co., Ltd.).

[0041] The elastic core layer may have a single layer structure or a multi-layer structure. When the elastic core layer has a multi-layer structure, the polymer composition of each layer in the elastic core layer may be the same or different.

[0042] The content of the elastic core layer in the core-shell particles is not particularly limited and can be appropriately selected depending on the purpose, but is preferably 40% by mass or more, more preferably 60% by mass or more, based on the total mass of the core-shell particles. The upper limit of the content of the elastic core layer in the core-shell particles is also not particularly limited, but is preferably 90% by mass or less, more preferably 85% by mass or less, from the viewpoint of improving the dispersion state of the core-shell particles in the sintering binder.

[0043] <<Shell layer>> The shell layer is made of a shell polymer that plays a role in improving the compatibility between the elastic core layer and a solvent that disperses the ceramic raw material powder when the ceramic sintering binder is used for sintering ceramics, thereby enabling the core-shell particles to be suitably dispersed in a medium that disperses the ceramic raw material powder.

[0044] The shell layer is formed by polymerizing, preferably graft-polymerizing, a monomer used for forming the shell layer (hereinafter sometimes referred to as a "monomer for forming the shell layer") to a polymer forming the elastic core layer, and the shell layer and the elastic core layer are substantially chemically bonded to each other to cover the elastic core layer. Therefore, the shell layer is present on the outermost surface of the core-shell particle.

[0045] That is, preferably, the shell polymer is formed by graft polymerizing a monomer that is a component of the shell polymer in the presence of the elastic core layer, and in this manner, the shell polymer is graft polymerized onto the elastic core layer.

[0046] The elastic core layer may be entirely or partially covered with the shell layer. The coverage of the elastic core layer with the shell layer can be confirmed by the following graft ratio.

[0047] The graft ratio of the shell layer in the core-shell particle is not particularly limited and can be appropriately selected depending on the purpose, but is preferably 70% or more, more preferably 80% or more, and even more preferably 90% or more.

[0048] In this specification, the graft ratio of the shell layer in the core-shell particle is calculated as follows. 2 g of the powder of the core-shell particles is immersed in 100 g of methyl ethyl ketone (MEK) at 23° C. for 24 hours, and then the MEK-soluble matter is separated from the MEK-insoluble matter, and the methanol-insoluble matter is further separated from the MEK-soluble matter, and the ratio of the MEK-insoluble matter to the total mass of the MEK-insoluble matter and the methanol-insoluble matter is calculated.

[0049] The shell layer contains a polymer (shell polymer) having at least one functional group selected from the group consisting of a hydroxyl group and a carboxyl group, which makes it easier to maintain the structure of the core-shell particles and improves dispersibility in the sintering binder. The hydroxyl group is not particularly limited, but a polyoxyethylene group having a hydroxyl group at its terminal is preferred.

[0050] The shell layer may further have a functional group other than at least one of a hydroxyl group and a carboxyl group. The functional group of the shell layer is not particularly limited as long as it does not impair the effects of the present invention, and examples of the functional group include a polyethylene oxide (PEO) group (including those without a hydroxyl group at the terminal).

[0051] The shell polymer is not particularly limited as long as it contains a polymer having at least one functional group selected from the group consisting of a hydroxyl group and a carboxyl group, and can be appropriately selected depending on the purpose. However, it is preferable that the shell polymer is compatible with the solvent in which the ceramic raw material powder is dispersed, and it is more preferable that the shell polymer contains a polymer containing at least one monomer selected from the group consisting of a (meth)acrylic monomer, an aromatic vinyl compound, and a vinyl cyanide compound as a constituent monomer.

[0052] Therefore, the monomer for forming the shell layer is preferably at least one selected from the group consisting of (meth)acrylic monomers, aromatic vinyl monomers, and vinyl cyanide monomers. These may be used alone or in combination of two or more.

[0053] -(Meth)acrylic monomer- Examples of the (meth)acrylic monomer include alkyl (meth)acrylates such as allyl (meth)acrylate, (meth)acrylate, methyl (meth)acrylate, ethyl (meth)acrylate, butyl (meth)acrylate, octyl (meth)acrylate, lauryl (meth)acrylate, myristyl (meth)acrylate, stearyl (meth)acrylate, benzyl (meth)acrylate, behenyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, ethylene glycol mono(meth)acrylate, ethylene glycol di(meth)acrylate, 1,3-butylene glycol di(meth)acrylate, and butanediol di(meth)acrylate, and 2-aminoethyl (meth)acrylate. These may be used alone or in combination of two or more.

[0054] Specific examples of the (meth)acrylic monomer include (poly)ethylene glycol (meth)acrylates (e.g., Blenmar (registered trademark) PE-90, PE-200, PE-350, AE-90U, AE-200, AE-400, etc., manufactured by NOF Corporation), (poly)propylene glycol (meth)acrylates (e.g., Blenmar (registered trademark) PP-500, PP-500D, PP-800, PP-1000, PP-2000D, AP-200, AP-400, AP-400D, AP-550, AP-800, AP-1000D, etc., manufactured by NOF Corporation), (poly)ethylene glycol-(poly)propylene glycol mono(meth)acrylates (e.g., Blenmar (registered trademark) PP-500, PP-500D, PP-800, PP-1000, PP-2000D, AP-200, AP-400, AP-400D, AP-550, AP-800, AP-1000D, etc., manufactured by NOF Corporation), and (poly)ethylene glycol-(poly)propylene glycol mono(meth)acrylates (e.g., Blenmar (registered trademark) PP-500, PP-500D, PP-800, PP-1000D, etc., manufactured by NOF Corporation). Blemmer (registered trademark) 50PEP-300, etc.), (poly)ethylene glycol-(poly)butylene glycol mono(meth)acrylate (e.g., Blemmer (registered trademark) 55PET-800, 50PEP-500D, etc., manufactured by NOF Corporation), (poly)propylene glycol-(poly)butylene glycol mono(meth)acrylate (e.g., Blemmer (registered trademark) 10PPB-500B, 10PPB-500BD, etc., manufactured by NOF Corporation), methoxy(poly)ethylene glycol mono(meth)acrylate (e.g., Blemmer (registered trademark) PME-100, PME-200, PME-400, PME-1000, PME-2000, AME-400, etc., manufactured by NOF Corporation;Shin-Nakamura Chemical Co., Ltd.'s NK Ester M-20G, M-40G, M-90G, M-130G, M-230G, M-450G, AM-30G, AM-90G, AM-130G, AM-230G, etc.), methoxy(poly)propylene glycol (meth)acrylate (for example, Shin-Nakamura Chemical Co., Ltd.'s NK Ester M-20G, M-40G, M-90G, M-130G, M-230G, M-450G, etc.), lauroxy(poly)ethylene glycol (meth)acrylate (for example, NOF Corp.'s NK Ester M-20G, M-40G, M-90G, M-130G, M-230G, M-450G, etc.), BLEMMER (registered trademark) PLE-1300 manufactured by NOF Corporation, etc.), stearoxy(poly)ethylene glycol (meth)acrylate (for example, BLEMMER (registered trademark) PSE-1300 manufactured by NOF Corporation, etc.), octyl(poly)ethylene glycol-(poly)propylene glycol mono(meth)acrylate (for example, BLEMMER (registered trademark) 50POEP-800B manufactured by NOF Corporation, etc.), phenoxy(poly)ethylene glycol mono(meth)acrylate (for example, N K-ester PHE-1G, AMP-30GY, etc.), phenoxy (poly)ethylene glycol-(poly)butylene glycol (meth)acrylate (for example, Blenmer (registered trademark) 43PAEP-600B manufactured by NOF Corporation, etc.), nonylphenoxy (poly)propylene glycol (meth)acrylate (for example, Blenmer (registered trademark) ANP-300 manufactured by NOF Corporation, etc.), nonylphenoxy (poly)ethylene glycol-(poly)propylene glycol (meth)acrylate (for example , Blenmer (registered trademark) 75ANEP-600 manufactured by NOF Corporation, etc.), (meth)acrylic acid and (meth)acrylic acid alkyl esters (for example, acrylic acid, methacrylic acid, ethyl acrylate, butyl acrylate, 2-ethylhexyl acrylate, methyl methacrylate, ethyl methacrylate, butyl methacrylate, 2-hydroxyethyl methacrylate, glycidyl methacrylate, etc.), unsaturated nitrile monomers (for example, acrylonitrile, methacrylonitrile, etc.). One molecule may contain one type of these hydrophilic substrates, or two or more types may be contained randomly.

[0055] The glass transition temperature (Tg) of the (meth)acrylic monomer is not particularly limited and can be appropriately selected depending on the purpose, but is preferably 50° C. or higher, more preferably 60° C. or higher, and even more preferably 70° C. or higher. When the (meth)acrylic monomer has a glass transition temperature (Tg) of 50° C. or higher, the strength of the core-shell particles can be improved.

[0056] The glass transition temperature (Tg) of the (meth)acrylic rubber can be measured by a differential scanning calorimeter (DSC) in the same manner as that for the elastic core layer.

[0057] -Aromatic vinyl monomer- Examples of the aromatic vinyl monomer include divinylbenzene, diisopropenylbenzene, divinylnaphthalene, divinylanthracene, etc. These may be used alone or in combination of two or more.

[0058] -Vinyl cyanide monomer- Examples of the vinyl cyanide monomer include acrylonitrile, methacrylonitrile, etc. These may be used alone or in combination of two or more.

[0059] The content of the shell layer in the core-shell particles is not particularly limited and can be appropriately selected depending on the purpose, but is preferably 10% by mass or more, more preferably 15% by mass or more, based on the total mass of the core-shell particles. The upper limit of the content of the shell layer in the core-shell particles is also not particularly limited, but is preferably 40% by mass or less, more preferably 30% by mass or less. When the content of the shell layer in the total mass of the core-shell particles is 10% by mass or more, the core-shell particles are less likely to aggregate and have good handleability, and when it is 40% by mass or less, the content of the elastic core layer in the core-shell particles does not decrease too much, making it easy to improve the density of the ceramic sintered body. In the core-shell particle, the total content of the elastic core layer and the shell layer is 100% by mass.

[0060] The shell layer preferably contains, as constituent monomers, constituent monomers derived from the (meth)acrylic monomer, constituent monomers derived from aromatic vinyl monomers, and constituent monomers derived from vinyl cyanide monomers in a total amount of 10% by mass to 95% by mass, more preferably 30% by mass to 92% by mass, even more preferably 50% by mass to 90% by mass, and particularly preferably 60% by mass to 87% by mass, based on 100% by mass of the shell layer (copolymer).

[0061] The content of the core layer and the monomer composition and content of the shell layer can be calculated from the amounts charged during production. When the amounts charged are unknown, they can be determined by, for example, gas chromatography mass spectrometry (GC / MS), proton nuclear magnetic resonance spectrometry ( 1 1 H-NMR, differential scanning calorimetry (DSC), and other methods may be used alone or in combination of two or more thereof.

[0062] <<Method of manufacturing core-shell particles>> The method for producing the core-shell particles is not particularly limited and can be appropriately selected depending on the purpose, but one embodiment of the method for producing the core-shell particles is described below. One embodiment of the method for producing the core-shell particles includes an elastic core layer forming step, a shell layer forming step, and further includes other steps as necessary.

[0063] -Core layer formation process- When the polymer forming the elastic core layer constituting the core-shell particle is formed by polymerizing at least one monomer (first monomer) selected from a diene monomer (conjugated diene monomer) and a (meth)acrylate monomer, the elastic core layer can be formed by, for example, emulsion polymerization, suspension polymerization, microsuspension polymerization, etc. As a specific example, the method described in International Publication No. 2005 / 028546 can be used.

[0064] When the polymer forming the elastic core layer contains a polysiloxane-based polymer, the elastic core layer can be formed by, for example, emulsion polymerization, suspension polymerization, microsuspension polymerization, etc. As a specific example, the method described in International Publication No. 2006 / 070664 can be used.

[0065] -Method of forming the shell layer- The shell layer can be formed by polymerizing the monomer for forming the shell layer by known radical polymerization in the presence of the elastic core layer (particle). When the elastic core layer (particle) is obtained as an emulsion, it is preferable to polymerize the monomer for forming the shell layer by emulsion polymerization. As a specific example, it can be produced according to the method described in International Publication No. 2005 / 028546.

[0066] <Other ingredients> The sintering binder may contain components other than the core-shell particles as long as the effects of the present invention are not impaired. The other components are not particularly limited as long as they do not impair the effects of the present invention, and can be appropriately selected depending on the purpose, and examples thereof include various additives such as solvents, dispersants, plasticizers, emulsifiers, antifoaming agents, pH adjusters, lubricants, fluidizing agents, preservatives, antifungal agents, colorants (dyes, pigments, etc.), preservatives, stabilizers, etc. These may be used alone or in combination of two or more.

[0067] The content of the other components in the sintering binder is not particularly limited as long as it does not impair the effects of the present invention, and can be appropriately selected depending on the purpose.

[0068] <<Solvent>> The solvent is not particularly limited and can be appropriately selected depending on the purpose. However, a solvent capable of dispersing the ceramic raw material powder and the sintering binder is preferable, and examples thereof include water and organic solvents.

[0069] Examples of the organic solvent include alcohols, ketones, ethers, modified ethers, ketones, esters, hydrocarbons, halogenated hydrocarbons, etc. These may be used alone or in combination of two or more.

[0070] Examples of the alcohols include methanol, ethanol, 1-propanol, 2-propanol, 1-butanol, 2-butanol, tert-butyl alcohol, 2-methoxyethanol, 2-ethoxyethanol, 2-(2-ethoxyethoxy)ethanol, diethylene glycol monobutyl ether, and glycerin. Examples of the ketones include acetone and methyl ethyl ketone. Examples of the ethers include tetrahydrofuran, diethyl ether, diisopropyl ether, 1,4-dioxane, and dimethoxyethane. Examples of the modified ethers include ether-modified ethers such as ether-modified alkylene glycols, and ester-modified ethers such as ester-modified alkylene glycols. A specific example is propylene glycol monomethyl ether acetate (PGMEA). Examples of the esters include ethyl acetate and butyl acetate. Examples of the hydrocarbons include hexane and toluene. Examples of the halogenated hydrocarbons include chloroform and carbon tetrachloride.

[0071] Among these, the solvent is preferably water or a water-soluble organic solvent from the viewpoints of safety to the living body and ease of removal, and more preferably water, ethanol, 2-propanol, tert-butyl alcohol, 2-ethoxyethanol, 2-(2-ethoxyethoxy)ethanol, propylene glycol monomethyl ether acetate, acetone, tetrahydrofuran, hexane, toluene, etc., and even more preferably water.

[0072] <<Dispersant>> There are no particular restrictions on the dispersant, and it can be appropriately selected according to the purpose. For example, ammonium polycarboxylate (such as ammonium citrate tribasic, etc.), ammonium polyacrylate, acrylic copolymer resin, acrylic ester copolymer, polyacrylic acid, bentonite, carboxymethyl cellulose, anionic surfactant (such as polyoxyethylene alkyl ether phosphate ester such as polyoxyethylene lauryl ether phosphate ester, etc.), nonionic surfactant, olein glyceride, amine surfactant, oligosaccharide alcohol, etc. can be mentioned. These can be used alone or in combination of two or more.

[0073] <<Plasticizer>> There are no particular restrictions on the plasticizer, and it can be appropriately selected according to the purpose. For example, polyethylene glycol, glycerin, propylene glycol, dibutyl phthalate, etc. can be mentioned. These can be used alone or in combination of two or more.

[0074] <<Emulsifier>> There are no particular restrictions on the emulsifier, and it can be appropriately selected according to the purpose. For example, alkyl ether, phenyl ether, sorbitan derivative, ammonium salt, etc. can be mentioned. These can be used alone or in combination of two or more.

[0075] <<Defoamer>> There are no particular restrictions on the defoamer, and it can be appropriately selected according to the purpose. For example, alcohol, polyether, polyethylene glycol, silicone, wax, etc. can be mentioned. These can be used alone or in combination of two or more.

[0076] <<pH Adjusting Agent>> The pH adjuster is not particularly limited and can be appropriately selected depending on the purpose, and examples thereof include ammonia, ammonium salts (including ammonium hydroxide such as tetramethylammonium hydroxide), alkali metal salts, alkaline earth metal salts, etc. These may be used alone or in combination of two or more.

[0077] <<Lubricants>> The lubricant is not particularly limited and can be appropriately selected depending on the purpose, and examples thereof include polyoxyethylene chelate ether, wax, etc. These may be used alone or in combination of two or more kinds.

[0078] [Application] The sintering binder of the present invention can be suitably used in the production of ceramics because it can be sintered at a low temperature in the production of a sintered ceramic body, and can provide a sintered ceramic body that is highly decomposable and has a high density.

[0079] (Method of manufacturing sintered ceramics) The method for producing a ceramic sintered body of the present invention includes a mixing step, a molding step, a degreasing step, and a firing step, and may further include other steps as necessary.

[0080] <Mixing process> The mixing step is a step of obtaining a mixture by mixing at least the ceramic raw material powder and the sintering binder of the present invention. In addition to the ceramic raw material powder and the sintering binder, other components such as a solvent and a dispersant may be mixed in the mixing step. The mixing step obtains a mixture of the ceramic raw material powder and the sintering binder, and further, if necessary, other components, and preferably obtains a slurry-like mixture in which the ceramic raw material powder and the sintering binder, and further, if necessary, other components are dispersed in the solvent.

[0081] The ceramic raw material powder is preferably uniformly dispersed in the solvent in the slurry mixture. When the method for producing a ceramic sintered body includes a drying step described later, the slurry mixture in which the ceramic raw material powder is uniformly dispersed in the solvent is used in the drying step, whereby, for example, clogging of a spray nozzle can be suppressed when spray drying is performed.

[0082] In addition, from the viewpoint of productivity, it is preferable that the slurry mixture does not foam. If foaming occurs in the slurry mixture, the slurry mixture may be left to stand or may be appropriately added with a known defoamer until the foam disappears, and then the mixture may be used in the next step.

[0083] The method for mixing the materials in the mixing step is not particularly limited and can be appropriately selected depending on the purpose, and examples thereof include mechanical dispersion methods using a roll mill, colloid mill, high-pressure injection type disperser, ultrasonic disperser, vibration mill, planetary mill, bead mill, etc. In addition, the slurry composition may be one that has been subjected to a dispersion treatment using heat or pressure, such as reflux treatment or hydrothermal treatment. These methods may be used alone or in combination of two or more.

[0084] <<Ceramic raw material powder>> The material of the ceramic raw material powder is not particularly limited and can be appropriately selected depending on the purpose, and examples thereof include alumina, zirconia, aluminum nitride, silicon carbide, silicon nitride, forsterite, steatite, cordierite, sialon, barium titanate, lead zirconate titanate, ferrite, mullite, etc. These may be used alone or in combination of two or more.

[0085] The content of the ceramic raw material powder in the mixture is not particularly limited and can be appropriately selected depending on the purpose, but is preferably 70 mass% or less, more preferably 60 mass% or less, and even more preferably 50 mass% or less, based on the total mass of the mixture, in order to suppress aggregation of particles during drying. Also, the lower limit of the content of the ceramic raw material powder in the mixture is not particularly limited, but is preferably 10 mass% or more, more preferably 20 mass% or more, and even more preferably 30 mass% or more.

[0086] <<Sintering binder>> The content of the sintering binder in the mixture is not particularly limited and can be appropriately selected depending on the purpose, but from the viewpoint of suppressing aggregation of particles during drying, the content of the core-shell particles is preferably 20% by mass or less, more preferably 15% by mass or less, and even more preferably 10% by mass or less, based on the total mass of the mixture. In addition, the lower limit of the content of the sintering binder in the mixture is not particularly limited, but the content of the core-shell particles is preferably 0.01% by mass or more, more preferably 0.05% by mass or more, and even more preferably 0.1% by mass or more.

[0087] The mass ratio of the content of the sintering binder to the content of the ceramic raw material powder is not particularly limited and can be appropriately selected depending on the purpose, but the content of the core-shell particles in the sintering binder is preferably 0.1 parts by mass to 20 parts by mass, more preferably 0.3 parts by mass to 15 parts by mass, and even more preferably 0.5 parts by mass to 10 parts by mass, relative to 100 parts by mass of the ceramic raw material powder. When the content of the core-shell particles in the sintering binder is 0.1 parts by mass to 20 parts by mass, relative to 100 parts by mass of the ceramic raw material powder, the ceramic sintered body can be easily densified.

[0088] <<Solvent>> The solvent in the mixture is not particularly limited and can be appropriately selected depending on the purpose. For example, the solvent may be the same as those described in the <<Solvent>> section of <<Other Components>> in the (sintering binder) above.

[0089] The content of the solvent in the mixture is not particularly limited and can be appropriately selected depending on the purpose. However, in order to suppress aggregation of particles during drying and obtain a denser ceramic sintered body, the total content of the solvent relative to the total mass of the mixture is preferably 70 mass% or less, more preferably 60 mass% or less, and even more preferably 50 mass% or less. The "total content of the solvent" here means the total mass of the content of the solvent contained in the sintering binder and the mass of the solvent added in the mixing step.

[0090] <<Other ingredients>> The other components in the mixture are not particularly limited and can be appropriately selected depending on the purpose. For example, the other components may be the same as the various additives described in the <Other Components> section of the (Sintering Binder) above.

[0091] The content of the other components in the mixture is not particularly limited as long as it does not impair the effects of the present invention, and can be appropriately selected depending on the purpose.

[0092] <Molding process> The molding step is a step of obtaining a molded product by molding the mixture.

[0093] The molding method for molding the powder composition is not particularly limited, and can be appropriately selected from known methods depending on the shape of the desired molded product, such as pressure molding, extrusion molding, tape molding, casting molding, injection molding, doctor blade method, etc. These may be used alone or in combination of two or more. Among these, the pressure treatment method is preferred as the molding method for molding the mixture. By molding the mixture by the pressure treatment method, the density of the molded product can be improved, and the density of the ceramic sintered body can also be improved.

[0094] -Pressure molding method- When the pressure molding method is carried out, the mixture is preferably in the form of a powder composition obtained by a drying step described below from the viewpoint of handling.

[0095] The pressure molding method is not particularly limited, and examples thereof include a method of applying pressure in one direction such as uniaxial pressing, a cold isostatic press (CIP) method, and a warm isostatic press (WIP) method. These may be used alone or in combination of two or more. Among these, cold isostatic pressing is preferred.

[0096] The pressure during the CIP treatment is preferably high because the desired molded product is easily obtained. The pressure during the CIP treatment is not particularly limited and can be appropriately selected depending on the purpose, but is preferably 100 MPa or more, more preferably 150 MPa or more, and even more preferably 200 MPa or more. Furthermore, when the pressure during the CIP treatment is 100 MPa or more, a high-density ceramic sintered body is obtained. Furthermore, the upper limit of the pressure during the CIP treatment is not particularly limited, but from the viewpoint of production efficiency, it is more preferably 300 MPa or less.

[0097] The temperature during the CIP treatment is not particularly limited and may be appropriately selected depending on the purpose, but is preferably 5° C. or higher, more preferably 10° C. or higher, and even more preferably 15° C. or higher. There is also no particular upper limit to the temperature during the CIP treatment, but from the viewpoint of production efficiency, it is preferably 300° C. or lower, more preferably 100° C. or lower, and even more preferably 50° C. or lower.

[0098] The density of the molded product obtained in the molding step is not particularly limited and can be appropriately selected depending on the manufacturing method of the molded product, etc. The higher the density of the molded product, the higher the density of the obtained ceramic sintered body.

[0099] The shape of the molded product obtained in the molding step is not particularly limited, and may be any desired shape depending on the application. The molded product may have a single-layer structure or a multi-layer structure. By making the molded product have a multi-layer structure, the ceramic sintered body finally obtained can have a multi-layer structure.

[0100] <Degreasing process> The degreasing step is a step of degreasing the molded product to obtain a ceramic sintering precursor. Since the molded product contains the sintering binder, a ceramic sintering precursor without chipping or cracking can be obtained.

[0101] The method for degreasing the molded product is not particularly limited and can be appropriately selected depending on the purpose, and examples thereof include superheated steam degreasing, pressure degreasing, etc. These may be used alone or in combination of two or more.

[0102] The superheated steam degreasing method is a method in which the molded product is heated while being brought into contact with superheated steam. In this specification, "superheated steam" means steam having a temperature higher than 100°C.

[0103] The heating temperature in the presence of the superheated steam is not particularly limited and can be appropriately selected depending on the purpose, but is preferably 120°C or higher, more preferably 150°C or higher, and even more preferably 200°C or higher. The upper limit of the heating temperature in the presence of the superheated steam is also not particularly limited and can be appropriately selected depending on the purpose, but is preferably 900°C or lower, more preferably 800°C or lower, and even more preferably 700°C or lower. When the heating temperature in the presence of the superheated steam is 120°C or higher, the generation of organic residues in the ceramic sintering binder can be effectively suppressed. When the heating temperature in the presence of the superheated steam is 900°C or lower, the sintering can be prevented from proceeding excessively, making processing difficult. The heating temperature in the presence of the superheated steam may be changed or may be constant within the preferred temperature range, or the temperature may change at some times and be constant at other times.

[0104] When the heating temperature in the presence of the superheated steam is raised within the preferred temperature range, the heating rate is not particularly limited and can be appropriately selected depending on the purpose, but is preferably 1 ° C. / min or more, more preferably 5 ° C. / min or more, and even more preferably 10 ° C. / min or more. The upper limit of the heating rate is also not particularly limited and can be appropriately selected depending on the purpose, but is preferably 150 ° C. / min or less, more preferably 50 ° C. / min or less, and even more preferably 20 ° C. / min or less. When the heating rate is 5 ° C. / min or more, the productivity of the ceramic sintering precursor is improved. In addition, when the heating rate is 150 ° C. / min or less, the volume difference between the inside and the outside of the molded product or the ceramic sintering precursor can be suppressed, and when the molded product contains an organic substance, the rapid decomposition of the organic substance can be suppressed, and the occurrence of cracks or destruction in the ceramic sintering precursor can be suppressed.

[0105] The heating time in the presence of the superheated steam is not particularly limited and can be appropriately selected depending on the purpose, but is preferably 0.5 hours or more, more preferably 1 hour or more, and even more preferably 2 hours or more, from the viewpoint of being able to stably obtain the desired ceramic sintering precursor with good productivity. The upper limit of the heating time in the presence of the superheated steam is also not particularly limited and can be appropriately selected depending on the purpose, but is preferably 10 hours or less, more preferably 8 hours or less, and even more preferably 6 hours or less, from the viewpoint of production efficiency.

[0106] The degreasing step can be carried out using a sintering furnace connected to a superheated steam generator. The type of superheated steam generator is not particularly limited and can be appropriately selected from known types, for example, a commercially available steam heater can be used. In addition, it is preferable that the generator can be controlled to the above-mentioned degreasing temperature range. The type of the sintering furnace is also not particularly limited, and for example, an electric furnace or a degreasing furnace used in general industry can be used.

[0107] The ceramic sintered precursor can be cut (milled) into a desired shape according to the intended use before being converted into a ceramic sintered body in the firing process described below. For example, when the ceramic sintered body is used as a dental material such as a dental prosthesis, the ceramic sintered precursor can be cut (milled) into a shape corresponding to the intended use to obtain a ceramic sintered body to be used for such an application. There is no particular limitation on the method of cutting (milling), and it can be performed, for example, using a known milling device.

[0108] <Firing process> The firing step is a step of firing the ceramic sintering precursor to obtain a ceramic sintered body. Since the ceramic sintering precursor contains the sintering binder, a ceramic sintered body without chips or cracks can be obtained by firing the ceramic sintering precursor. The ceramic sintered body obtained by such a method is also included in the scope of the present invention.

[0109] The sintering temperature in the firing step is not particularly limited and can be appropriately selected depending on the purpose, but is preferably 900°C or higher, more preferably 1,000°C or higher, and even more preferably 1,200°C or higher. If the sintering temperature is 900°C or higher, the sintering can be sufficiently advanced, and a dense ceramic sintered body can be easily obtained. In addition, since it is preferable to sufficiently sinter the organic matter contained in the sintering binder in the firing step, the upper limit is not particularly limited, but from the viewpoint of production efficiency, it is preferable to be 1,500°C or lower. The sintering temperature may be changed or constant within the preferred temperature range, or the temperature may be changed at some times and constant at other times.

[0110] When the sintering temperature is raised within the preferred temperature range, the heating rate or cooling rate is not particularly limited and can be appropriately selected depending on the purpose, but is preferably 1 ° C. / min or more, more preferably 5 ° C. / min or more, and even more preferably 10 ° C. / min or more. When the heating rate or cooling rate is 1 ° C. / min or more, the productivity of the ceramic sintered body is improved. In addition, the upper limit of the heating rate or cooling rate is also not particularly limited and can be appropriately selected depending on the purpose, but is preferably 50 ° C. / min or less, more preferably 20 ° C. / min or less, and even more preferably 15 ° C. / min or less. When the heating rate is 50 ° C. / min or less, the volume difference between the inside and the outside of the ceramic sintered precursor or the ceramic sintered body can be suppressed, and the rapid decomposition of the organic matter in the ceramic sintered precursor can be suppressed, and the occurrence of cracks or destruction in the ceramic sintered body can be suppressed.

[0111] The sintering time in the firing step is not particularly limited and can be appropriately selected depending on the purpose.

[0112] The firing step can be performed using a known sintering furnace. The type of the sintering furnace is not particularly limited, and for example, an electric furnace or a degreasing furnace used in general industry can be used. The degreasing step and the firing step can be performed in the same sintering furnace or in different sintering furnaces.

[0113] <Other processes> The other steps are not particularly limited as long as they do not impair the effects of the present invention, and may be appropriately selected depending on the purpose. Examples of the other steps include a drying step, a surface protection treatment step, and a coating step.

[0114] <<Drying process>> The drying step is a step of drying the mixture to obtain a powder composition.

[0115] The drying method for drying the mixture is not particularly limited and can be appropriately selected from known methods, such as spray drying, supercritical drying, freeze drying, hot air drying, filtration drying, and reduced pressure drying. These may be used alone or in combination of two or more. Among these, spray drying, supercritical drying, and freeze drying are preferred, and spray drying is more preferred, since they can suppress the aggregation of particles during drying and can provide a denser ceramic sintered body.

[0116] The supercritical fluid used in the case of performing supercritical drying as the drying method is not particularly limited, and examples thereof include water, carbon monoxide, carbon dioxide, dinitrogen monoxide, nitrogen, methane, ethane, propane, 2,3-dimethylbutane, ethylene, dimethyl ether, etc. These may be used alone or in combination of two or more.

[0117] The drying conditions in each of the above drying methods are not particularly limited, and known drying conditions can be appropriately adopted. When an organic solvent is used as a dispersion medium, it is preferable to perform drying in the presence of a non-flammable gas, and more preferably to perform drying in the presence of nitrogen, in order to reduce the risk of explosion during drying.

[0118] The moisture content of the powder composition obtained in the drying step is not particularly limited, but is preferably 1.5% by mass or less, more preferably 1% by mass or less, and even more preferably 0.5% by mass or less. The water content of the powder composition can be measured, for example, by the Karl Fischer method.

[0119] <<Surface protection treatment process>> The surface protection treatment step is a step of forming a protective layer on the surface of the ceramic sintering precursor. By carrying out this surface protection treatment step, the surface of the ceramic sintering precursor can be given durability, etc., that allows the ceramic sintering precursor to be used as is, for example.

[0120] Specific examples of the protective layer include a water-resistant layer, a weather-resistant layer, a light-resistant layer, a heat-insulating layer, and a gloss layer.

[0121] The surface protection treatment can be carried out by a known surface protection treatment device, for example, a spray device, a coating device, or the like.

[0122] <<Painting process>> The coating step is a step of coating the ceramic sintering precursor. By carrying out the coating step, the ceramic sintering precursor can be colored in a desired color.

[0123] The coating can be carried out by using a known coating device, for example, a coating device using a spray, a roller, a brush, or the like. EXAMPLES

[0124] The present invention will be specifically described below with reference to Production Examples, Examples, and Comparative Examples, but the present invention is not limited to these Production Examples and Examples. In the Production Examples, Examples, and Comparative Examples, "%" means "% by mass" and "parts" means "parts by mass" unless otherwise specified.

[0125] (Production Example 1: Production of latex L-1 containing core-shell particles) <Formation of Elastic Core Layer> 2,730g of deionized water and 5.0g of EMAL 2FG (sodium lauryl sulfate, solid content concentration 30%, Kao Corporation) were charged into an 8L polymerization vessel, which was then heated to 50℃ and nitrogen was flowed in. Next, a mixture of 150g of butyl acrylate, 0.375g of allyl methacrylate, and 0.3g of t-butyl hydroperoxide (solid content concentration 69%) was charged into the 8L polymerization vessel, followed by a solution of 0.00864g of ferrous sulfate heptahydrate (FeSO4·7H2O) and 0.03456g of disodium ethylenediaminetetraacetate (EDTA) dissolved in 8.6g of deionized water, and then 48.0g of sodium formaldehyde sulfoxylate (solid content concentration 5%) was charged and stirred for 30 minutes. Next, 4.7g of EMALE 2FG was added to the 8L polymerization vessel, followed by a mixture of 1,650g of butyl acrylate, 4.125g of allyl methacrylate, 27.0g of Phosphanol RD-510Y (polyoxyethylene lauryl ether phosphoric acid, manufactured by Toho Chemical Industry Co., Ltd.), and 3.0g of t-butyl hydroperoxide (solid concentration 69%), which was added to the 8L polymerization vessel over 165 minutes. Upon completion of the addition of the mixture, 3.0g of t-butyl hydroperoxide (solid concentration 69%) was added to the 8L polymerization vessel and stirred for 30 minutes. As a result, a latex containing acrylic rubber particles with a solid concentration of 40.0% was obtained.

[0126] <Shell layer formation> 4,500 g of the obtained latex containing acrylic rubber particles (solid concentration 40.0%) was charged into the 8 L polymerization vessel, and 60.0 g of sodium formaldehyde sulfoxylate (solid concentration 5%) was added. Then, a mixture of 1,050 g of methyl methacrylate, 60 g of styrene, 90 g of polyethylene glycol monomethacrylate (average number of moles added of oxyethylene groups: 4.5, product name: Blenmar (registered trademark) PE-200, manufactured by NOF Corporation), and 3.3 g of t-butyl hydroperoxide (solid concentration 69%) was added to the 8 L polymerization vessel over 120 minutes to start polymerization. During the polymerization reaction, sodium formaldehyde sulfoxylate and t-butyl hydroperoxide were appropriately added. The polymerization reaction was terminated 80 minutes after the start of polymerization. Then, 10.5 g of Emulgen LS-110 (polyoxyethylene polyoxypropylene alkyl ether, manufactured by Kao Corporation) was added to the latex containing the polymer to obtain latex L-1 having a conversion rate of 100%, a solid content concentration of 49.0%, and a volume average particle diameter of 230 nm, which contains polymer particles (core-shell particles) having a core-shell structure with an elastic core layer of acrylic rubber particles and a shell layer having hydroxyl groups (polyoxyethylene groups).

[0127] (Production Example 2: Production of latex L-2 containing core-shell particles) <Formation of Elastic Core Layer> 90g of deionized water and 10g of disodium hydrogen phosphate (solid content concentration 10%) were charged into a 100L pressure-resistant autoclave, followed by a solution of 0.237g of ferrous sulfate heptahydrate (FeSO4·7H2O) and 0.395g of disodium ethylenediaminetetraacetate (EDTA) dissolved in 125.8g of deionized water, and deoxidized for 15 minutes at -0.01MPa. Next, 66.7g of Neopelex G-15 (sodium dodecylbenzenesulfonate, solid content concentration 15.0%, Kao Corporation), 9,000g of 1,3-butadiene, 11,000g of styrene, and 150g of t-dodecyl mercaptan were charged into the 100L pressure-resistant autoclave, and the internal temperature was raised to 50℃. Subsequently, 140.0 g of sodium formaldehyde sulfoxylate (solid concentration 5%) and 7.7 g of paramenthane hydroperoxide (solid concentration 52%) were added to initiate polymerization. 15 hours after the start of polymerization, the mixture was degassed under reduced pressure to remove the butadiene remaining without being used in the polymerization, thereby terminating the polymerization. As a result, a latex containing styrene-butadiene rubber particles with a solid concentration of 45.0% was obtained. During the polymerization reaction, sodium formaldehyde sulfoxylate, paramenthane hydroperoxide, ferrous sulfate heptahydrate (FeSO4·7H2O), and disodium ethylenediaminetetraacetate (EDTA) were added to the 100 L pressure autoclave in arbitrary amounts at arbitrary times.

[0128] <<Shell layer formation>> 2,000 g of the obtained latex containing styrene-butadiene rubber particles (solid concentration 45.0%) was charged into an 8L polymerization vessel, and 60.0 g of sodium formaldehyde sulfoxylate (solid concentration 5%) was added. Then, a mixture of 237.6 g of styrene, 26.4 g of methyl methacrylate, 36 g of polyoxymethylene methacrylate, and 3.3 g of t-butyl hydroperoxide (solid concentration 69%) was added to the 8L polymerization vessel over 120 minutes to start polymerization. During the polymerization reaction, sodium formaldehyde sulfoxylate and t-butyl hydroperoxide were appropriately added. The polymerization reaction was terminated 80 minutes after the start of polymerization. As a result, latex L-2 was obtained, which contains polymer particles (core-shell particles) having a core-shell structure with an elastic core layer of styrene-butadiene rubber particles and a shell layer having hydroxyl groups (polyoxyethylene groups), with a conversion rate of 100%, a solid content concentration of 46.0%, and a volume average particle diameter of 200 nm.

[0129] (Production Example 3: Production of latex L-3 containing core-shell particles) <Formation of Elastic Core Layer> 2,730g of deionized water and 5.0g of EMAL 2FG (sodium lauryl sulfate, solid content 30%, Kao Corporation) were charged into an 8L polymerization vessel, which was then heated to 50℃ and nitrogen was flowed in. Next, a mixture of 150g of butyl acrylate, 0.375g of allyl methacrylate, and 0.3g of t-butyl hydroperoxide (solid content concentration 69%) was charged into the 8L polymerization vessel, followed by a solution of 0.00864g of ferrous sulfate heptahydrate (FeSO4·7H2O) and 0.03456g of disodium ethylenediaminetetraacetate (EDTA) dissolved in 8.6g of deionized water, and then 48.0g of sodium formaldehyde sulfoxylate (solid content concentration 5%) was charged and stirred for 30 minutes. Next, 4.7g of EMALE 2FG was added to the 8L polymerization vessel, followed by a mixture of 2,850g of butyl acrylate, 4.125g of allyl methacrylate, 27.0g of Phosphanol RD-510Y (polyoxyethylene lauryl ether phosphoric acid, manufactured by Toho Chemical Industry Co., Ltd.), and 3.0g of t-butyl hydroperoxide (solid concentration 69%), which was added to the 8L polymerization vessel over 165 minutes. At the end of the addition of the mixture, 3.0g of t-butyl hydroperoxide (solid concentration 69%) was added to the 8L polymerization vessel and stirred for 30 minutes. This resulted in a latex containing acrylic rubber particles with a solid content of 40.0%.

[0130] <Shell layer formation> 4,500 g of the obtained latex containing acrylic rubber particles (solid concentration 40.0%) was charged into the 8 L polymerization vessel, and 60.0 g of sodium formaldehyde sulfoxylate (solid concentration 5%) was added. Then, a mixture of 1,050 g of methyl methacrylate, 60 g of styrene, 90 g of methyl methacrylate, and 3.3 g of t-butyl hydroperoxide (solid concentration 69%) was added to the 8 L polymerization vessel over 120 minutes to start polymerization. During the polymerization reaction, sodium formaldehyde sulfoxylate and t-butyl hydroperoxide were appropriately added. The polymerization reaction was terminated 80 minutes after the start of polymerization. Then, 10.5 g of Emulgen LS-110 (polyoxyethylene polyoxypropylene alkyl ether, manufactured by Kao Corporation) was added to the latex containing the polymer to obtain latex L-3 having a conversion rate of 100%, a solid content concentration of 49.0%, and a volume average particle diameter of 230 nm, the latex containing polymer particles (core-shell particles) having a core-shell structure with an elastic core layer of acrylic rubber particles and a shell layer having a carboxyl group.

[0131] (Production Example 4: Production of latex L-4 containing core-shell particles) <Formation of Elastic Core Layer> 2,730g of deionized water and 5.0g of EMAL 2FG (sodium lauryl sulfate, solid content 30%, Kao Corporation) were charged into an 8L polymerization vessel, which was then heated to 50℃ and nitrogen was flowed in. Next, a mixture of 150g of butyl acrylate, 0.375g of allyl methacrylate, and 0.3g of t-butyl hydroperoxide (solid content concentration 69%) was charged into the 8L polymerization vessel, followed by a solution of 0.00864g of ferrous sulfate heptahydrate (FeSO4·7H2O) and 0.03456g of disodium ethylenediaminetetraacetate (EDTA) dissolved in 8.6g of deionized water, and then 48.0g of sodium formaldehyde sulfoxylate (solid content concentration 5%) was charged and stirred for 30 minutes. Next, 4.7g of EMALE 2FG was added to the 8L polymerization vessel, followed by a mixture of 2,850g of butyl acrylate, 4.125g of allyl methacrylate, 27.0g of Phosphanol RD-510Y (polyoxyethylene lauryl ether phosphoric acid, manufactured by Toho Chemical Industry Co., Ltd.), and 3.0g of t-butyl hydroperoxide (solid concentration 69%), which was added to the 8L polymerization vessel over 165 minutes. At the end of the addition of the mixture, 3.0g of t-butyl hydroperoxide (solid concentration 69%) was added to the 8L polymerization vessel and stirred for 30 minutes. This resulted in a latex containing acrylic rubber particles with a solid content of 40.0%.

[0132] <Shell layer formation> 4,500 g of the obtained latex containing acrylic rubber particles (solid concentration 40.0%) was charged into the 8 L polymerization vessel, and 60.0 g of sodium formaldehyde sulfoxylate (solid concentration 5%) was added. Then, a mixture of 832.5 g of styrene, 277.5 g of acrylonitrile, 90 g of polyethylene glycol monomethacrylate (average number of moles of oxyethylene groups added: 4.5, product name: Blenmar (registered trademark) PE-200, manufactured by NOF Corporation), and 3.3 g of t-butyl hydroperoxide (solid concentration 69%) was added to the 8 L polymerization vessel over 120 minutes to start polymerization. During the polymerization reaction, sodium formaldehyde sulfoxylate and t-butyl hydroperoxide were appropriately added. The polymerization reaction was terminated 80 minutes after the start of polymerization. Then, 10.5 g of Emulgen LS-110 (polyoxyethylene polyoxypropylene alkyl ether, manufactured by Kao Corporation) was added to the latex containing the polymer to obtain latex L-4 having a conversion rate of 100%, a solid content concentration of 49.0%, and a volume average particle diameter of 230 nm, which contains polymer particles (core-shell particles) having a core-shell structure with an elastic core layer of acrylic rubber particles and a shell layer having hydroxyl groups (polyoxyethylene groups).

[0133] (Production Example 5: Production of latex L-5 containing core-shell particles) <Formation of Elastic Core Layer> 2,730g of deionized water and 5.0g of EMAL 2FG (sodium lauryl sulfate, solid content 30%, Kao Corporation) were charged into an 8L polymerization vessel, which was then heated to 50℃ and nitrogen was flowed in. Next, a mixture of 150g of butyl acrylate, 0.375g of allyl methacrylate, and 0.3g of t-butyl hydroperoxide (solid content concentration 69%) was charged into the 8L polymerization vessel, followed by a solution of 0.00864g of ferrous sulfate heptahydrate (FeSO4·7H2O) and 0.03456g of disodium ethylenediaminetetraacetate (EDTA) dissolved in 8.6g of deionized water, and then 48.0g of sodium formaldehyde sulfoxylate (solid content concentration 5%) was charged and stirred for 30 minutes. Next, 4.7g of EMALE 2FG was added to the 8L polymerization vessel, followed by a mixture of 1,850g of butyl acrylate, 1,000g of styrene, 4.125g of allyl methacrylate, 27.0g of Phosphanol RD-510Y (polyoxyethylene lauryl ether phosphoric acid, manufactured by Toho Chemical Industry Co., Ltd.), and 3.0g of t-butyl hydroperoxide (solid concentration 69%), which was added to the 8L polymerization vessel over 165 minutes. At the end of the addition of the mixture, 3.0g of t-butyl hydroperoxide (solid concentration 69%) was added to the 8L polymerization vessel and stirred for 30 minutes. This resulted in a latex containing acrylic rubber particles with a solid content of 40.0%.

[0134] <Shell layer formation> 4,500 g of the obtained latex containing acrylic rubber particles (solid concentration 40.0%) was charged into the 8 L polymerization vessel, and 60.0 g of sodium formaldehyde sulfoxylate (solid concentration 5%) was added. Then, a mixture of 1,050 g of methyl methacrylate, 60 g of styrene, 90 g of polyethylene glycol monomethacrylate (average addition mole number of oxyethylene substrate: 4.5, product name: Blenmar (registered trademark) PE-200, manufactured by NOF Corporation), and 3.3 g of t-butyl hydroperoxide (solid concentration 69%) was added to the 8 L polymerization vessel over 120 minutes to start polymerization. During the polymerization reaction, sodium formaldehyde sulfoxylate and t-butyl hydroperoxide were appropriately added. The polymerization reaction was terminated 80 minutes after the start of polymerization. Then, 10.5 g of Emulgen LS-110 (polyoxyethylene polyoxypropylene alkyl ether, manufactured by Kao Corporation) was added to the latex containing the polymer to obtain latex L-5 having a conversion rate of 100%, a solid content concentration of 49.0%, and a volume average particle diameter of 230 nm, which contains polymer particles (core-shell particles) having a core-shell structure with an elastic core layer of acrylic rubber particles and a shell layer having hydroxyl groups (polyoxyethylene groups).

[0135] <<Measurement of glass transition temperature (Tg)>> The glass transition temperatures (Tg) of the elastic core layers obtained in the manufacturing processes of Manufacturing Examples 1 to 5 and the polyvinyl alcohol (product name: Cerna WF-804, manufactured by Chukyo Yushi Co., Ltd.) used in Comparative Example 1 described later were measured using a differential scanning calorimeter (DSC). Specifically, a differential scanning calorimeter (manufactured by Seiko Instruments Inc.) was used to measure the temperature range of -100°C to 200°C in a nitrogen atmosphere (flow rate 50 mL / min) at a temperature rise rate of 10°C / min, and the lowest endothermic peak temperature was taken as the glass transition temperature of the elastic core layer or polyvinyl alcohol. The results are shown in Table 1 below.

[0136] [Table 1]

[0137] Example 1 <Mixing process> 150g of alumina, 150g of distilled water, and 600g of zirconia balls with a diameter of 10mm were mixed in a pot mill for 24 hours to obtain an aqueous dispersion slurry of alumina. Next, 1.5g of a polycarboxylate ammonium dispersant (solid concentration: 10%, product name: Celna D-305, manufactured by Chukyo Yushi Co., Ltd.) (solid content added amount relative to the powder material: 0.4%) and 1.53g (solid content amount: 0.75g) of latex L-1 (solid concentration: 49.0%) obtained in Production Example 1 were added thereto, and after mixing in a pot mill for 1 hour, the zirconia balls were removed to obtain a slurry composition. When the appearance of the obtained slurry composition was visually observed, the alumina was uniformly dispersed and in a good condition.

[0138] <Drying process> The slurry composition obtained in the mixing step was made into a powder composition using a small spray dryer (ADL311S-A, manufactured by Yamato Scientific Co., Ltd.).

[0139] <Molding process> The powdered composition obtained in the drying step was placed in a mold and uniaxially molded at 10 MPa for 60 seconds. Next, a core metal was placed in the center of the mold and cold isostatic pressing (CIP) was performed at 23°C and 250 MPa for 60 seconds. This resulted in a circular tablet-shaped green compact with a diameter of 22.5 mm and a height of 11 mm.

[0140] <Degreasing process> The green compact obtained in the molding step was subjected to superheated steam degreasing under the following degreasing conditions using a superheated steam treatment device (manufactured by Takasago Industrial Co., Ltd.), to obtain a ceramic sintering precursor. [Degreasing conditions] The initial temperature was room temperature (23±1°C) and the final temperature was 150°C. The temperature was raised at a rate of 10°C / min under a nitrogen atmosphere while injecting nitrogen (N2) at a rate of 10 L / min. The following temperature increase and decrease were performed under superheated steam while injecting superheated steam at a rate of 5 kg / hour. After holding at 150°C for 0.5 hours under superheated steam, the temperature was increased from 150°C to 700°C at a rate of 10°C / min, held at 700°C for 1 hour, and then decreased from 700°C to 200°C at a rate of 10°C / min. Next, the furnace was cooled from 200° C. to room temperature in an air atmosphere.

[0141] <Firing process> After the degreasing step, the ceramic sintering precursor was sintered in an air atmosphere high-temperature furnace (SH-2025, manufactured by Motoyama Corporation) under the sintering conditions shown below, to obtain the ceramic sintered body of Example 1. [Sintering conditions] Sintering was performed in an air atmosphere. The starting temperature was room temperature (23±1°C) and the ending temperature was 1,400°C. After increasing the temperature at 10°C / min, the material was kept at 1,400°C for 1 hour, and then cooled from 1,400°C to room temperature at 10°C / min.

[0142] Example 2 In the mixing step of Example 1, the sintering binder used was changed from 1.53 g (solid content: 0.75 g) of Latex L-1 (solid content concentration: 49.0%) obtained in Production Example 1 to 1.63 g (solid content: 0.75 g) of Latex L-2 (solid content concentration: 46.0%) obtained in Production Example 2. The mixing step, drying step, molding step, degreasing step, and firing step were performed in the same manner as in Example 1, to obtain a ceramic sintered body of Example 2. When the appearance of the slurry-like composition obtained in the mixing step was visually observed, alumina was uniformly dispersed and in a good condition.

[0143] Example 3 In the mixing step of Example 1, the sintering binder used was changed from Latex L-1 obtained in Production Example 1 to Latex L-3 obtained in Production Example 3, but the mixing step, drying step, molding step, degreasing step, and firing step were performed in the same manner as in Example 1 to obtain a ceramic sintered body of Example 4. When the appearance of the slurry composition obtained in the mixing step was visually observed, alumina was uniformly dispersed and in a good condition, but foaming was intense and the efficiency of powderization in the subsequent drying step was poor.

[0144] Example 4 In the mixing step of Example 1, the sintering binder used was changed from Latex L-1 obtained in Production Example 1 to Latex L-4 obtained in Production Example 4, and the mixing step, drying step, molding step, degreasing step, and firing step were performed in the same manner as in Example 1 to obtain a ceramic sintered body of Example 4. When the appearance of the slurry-like composition obtained in the mixing step was visually observed, alumina was uniformly dispersed and in a good condition.

[0145] Example 5 In the mixing step of Example 1, the sintering binder used was changed from Latex L-1 obtained in Production Example 1 to Latex L-5 obtained in Production Example 5, and the mixing step, drying step, molding step, degreasing step, and firing step were performed in the same manner as in Example 1 to obtain a ceramic sintered body of Example 5. When the appearance of the slurry composition obtained in the mixing step was visually observed, alumina was uniformly dispersed and in a good condition.

[0146] Comparative Example 1 In the mixing step of Example 1, the sintering binder used was changed from 1.53 g (solid content: 0.75 g) of Latex L-1 (solid content concentration: 49.0%) obtained in Production Example 1 to 7.5 g (solid content: 0.75 g) of polyvinyl alcohol (active ingredient concentration: 10 mass%, product name: Celna WF-804, manufactured by Chukyo Yushi Co., Ltd.), but the mixing step, drying step, molding step, degreasing step, and firing step were performed in the same manner as in Example 1 to obtain a ceramic sintered body of Example 2. When the appearance of the slurry-like composition obtained in the mixing step was visually observed, alumina was uniformly dispersed and in a good condition.

[0147] <<Size and mass of molded product after molding process>> The diameter and thickness of the molded products obtained in the molding process of Examples 1 to 5 and Comparative Example 1 were measured with a digital caliper (manufactured by Mitutoyo Corporation), and the mass of these molded products was measured with an electronic balance (manufactured by METTLER TOLEDO). The results are shown in Table 2 below.

[0148] [Table 2]

[0149] There was no significant difference in diameter and thickness between the molded products of Examples 1 to 5 and Comparative Example 1. The mass was slightly larger in Comparative Example 1, but this was thought to be due to the difference in the specific gravity between the acrylic monomer used in the sintering binder and polyvinyl alcohol.

[0150] <<Changes in mass and appearance of ceramic sintering precursor after degreasing process>> The mass of the ceramic sintered precursor obtained in the degreasing step in Examples 1 to 5 and Comparative Example 1 was measured with an electronic balance (manufactured by METTLER TOLEDO). The results are shown in Table 3 below. From the measured values, the rate of change in mass before and after the degreasing step was calculated based on the following formula. In addition, an example of the appearance of the molded product before degreasing and the ceramic sintered precursor after degreasing photographed with a digital camera is shown in FIG. 1A (Example 1), FIG. 1B (Example 2), FIG. 1C (Example 3), FIG. 1D (Example 4), FIG. 1E and FIG. 1F (Example 5), and FIG. 1G (Comparative Example 1). In Example 5, since the Tg of the elastic core layer was high, cracks and / or chips occurred in the molded product before degreasing obtained in the molding step, and therefore cracks and / or chips also occurred in the ceramic sintered precursor after degreasing. Note that FIG. 1E and FIG. 1F show a sample in which cracks occurred in the molded product before degreasing and the ceramic sintered precursor after degreasing as an example of Example 5. Change rate (%) = (mass after degreasing - mass before degreasing) / mass before degreasing x 100

[0151] [Table 3]

[0152] The content of the organic matter added in the mixing step in Examples 1 to 5 and Comparative Example 1 was about 1 mass % (solid content). Therefore, the closer the conversion rate is to 1 mass %, the more the organic matter has been degreased in the degreasing step. From the results in Table 3, there was no significant difference in the conversion rate between the molded products in Examples 1 to 5 and Comparative Example 1. On the other hand, when organic matter is carbonized in the degreasing step, the ceramic sintering precursor becomes black in appearance. As shown in Figs. 1A to 1G, after degreasing in Example 2 and Comparative Example 1, the ceramic sintering precursor became slightly black. Furthermore, if the shape cannot be maintained after the molding step or the degreasing step, and cracks or chips occur in the ceramic sintering precursor, this will lead to cracks or chips in the final ceramic sintered body. As can be seen from Figures 1A to 1D and 1G, none of the ceramic sintering precursors of Examples 1 to 4 and Comparative Example 1 had cracks or chips. As can be seen from Figures 1E and 1F, in Example 5, cracks and / or chips occurred in the molded product before degreasing obtained in the molding step, and therefore cracks and / or chips also occurred in the ceramic sintering precursor after degreasing.

[0153] <<Size, mass, density, and appearance of ceramic sintered body after firing process>> -Measurement of the size of sintered ceramics after firing process- The diameter and thickness of the ceramic sintered bodies obtained in the firing process of Examples 1 to 5 and Comparative Example 1 were measured with a digital caliper (manufactured by Mitutoyo Corporation), and the mass of these ceramic sintered bodies was measured with an electronic balance (manufactured by METTLER TOLEDO). The results are shown in Table 4 below. 2 shows the relationship between the temperature change and the mass change in the firing process for Example 1, Example 2, Example 4, and Comparative Example 1. Note that, for Example 3 and Example 5, the relationship between the temperature change and the mass change in the firing process was not examined.

[0154] - Measurement of density of sintered ceramics after firing process - The density of the ceramic sintered bodies obtained in the firing step of Examples 1 to 5 and Comparative Example 1 was measured with an automatic specific gravity meter (manufactured by Toyo Machinery Co., Ltd.) The results are shown in Table 4 below.

[0155] -Observation of the appearance of ceramic sintered bodies after firing process- Examples of the appearances of the ceramic sintered bodies obtained in the firing processes of Examples 1 to 5 and Comparative Example 1 photographed with a digital camera are shown in FIG. 1A (Example 1), FIG. 1B (Example 2), FIG. 1C (Example 3), FIG. 1D (Example 4), FIGS. 1E and F (Example 5), and FIG. 1G (Comparative Example 1). 1A to 1D and 1G show that no cracks or chips were generated in the ceramic sintered bodies of Examples 1 to 4 and Comparative Example 1. As shown in Figs. 1E and 1F, in Example 5, cracks and / or chips were generated in the molded product before degreasing and the ceramic sintered precursor after degreasing obtained in the molding step, and therefore cracks and / or chips were further promoted in the ceramic sintered body obtained in the firing step. Figs. 1E and 1F show a sample in which chips were generated in the ceramic sintered body as an example of Example 5.

[0156] [Table 4]

[0157] The results in Table 4 show that the ceramic sintered bodies of Examples 1 to 5 had improved density compared to the ceramic sintered body of Comparative Example 1. In addition, from the results of FIG. 2, it was found that Examples 1, 2, and 4 could be sintered at a lower temperature than Comparative Example 1, and organic matter derived from the sintering binder was less likely to remain.

[0158] Examples of aspects of the present invention include the following. <1> A binder for sintering ceramics, comprising: The present invention comprises a core-shell particle having an elastic core layer and a shell layer covering the elastic core layer, The sintering binder is characterized in that the shell layer contains a polymer having at least one functional group selected from the group consisting of a hydroxyl group and a carboxyl group. <2> The elastic core layer contains a (meth)acrylic rubber. <1> 1. The sintering binder according to claim 1. <3> The (meth)acrylic rubber has a glass transition temperature of less than 0° C. <1> or <2> 1. The sintering binder according to claim 1. <4> The shell layer contains a polymer containing at least one monomer selected from the group consisting of a (meth)acrylic monomer, an aromatic vinyl compound, and a vinyl cyanide compound as a constituent monomer. <1> from <3> The sintering binder according to any one of claims 1 to 5, <5> At least a ceramic raw material powder and the <1> from <4> A mixing step of obtaining a mixture by mixing the sintering binder described in any one of the above items. a molding step of molding the mixture to obtain a molded product; a degreasing step of degreasing the molded product to obtain a ceramic sintering precursor; A firing step of firing the ceramic sintering precursor to obtain a ceramic sintered body; The present invention relates to a method for producing a sintered ceramic body, the method comprising the steps of:

Claims

1. A binder for sintering ceramics, comprising: The present invention comprises a core-shell particle having an elastic core layer and a shell layer covering the elastic core layer, A sintering binder, wherein the shell layer contains a polymer having at least one functional group selected from the group consisting of a hydroxyl group and a carboxyl group.

2. The sintering binder according to claim 1 , wherein the elastic core layer contains a (meth)acrylic rubber.

3. The sintering binder according to claim 2 , wherein the (meth)acrylic rubber has a glass transition temperature of less than 0° C.

4. 3. The sintering binder according to claim 1 or 2, wherein the shell layer contains a polymer containing at least one selected from the group consisting of (meth)acrylic monomers, aromatic vinyl compounds, and vinyl cyanide compounds as a constituent monomer.

5. A mixing step of obtaining a mixture by mixing at least a ceramic raw material powder and the sintering binder according to claim 1 or 2; a molding step of molding the mixture to obtain a molded product; a degreasing step of degreasing the molded product to obtain a ceramic sintering precursor; A firing step of firing the ceramic sintering precursor to obtain a ceramic sintered body; A method for producing a ceramic sintered body, comprising:

Citation Information

Patent Citations

  • Binder resin composition for sintering

    JP2014047338A

Cited By

  • Method for producing ceramic calcined body

    WO2025206348A1