Surface corrosion method of pure silicon carbide ceramic
By using Murakami's reagent to corrode silicon carbide ceramics at 200-250°C, the problems of complex equipment and major safety hazards in the existing technology are solved, safe and fast surface corrosion is achieved, and corrosion temperature and time is significantly reduced, and the sample is ensured. Microstructure integrity and experimental safety.
Patent Information
- Application Number
- CN202411154610.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-22
- Publication Date
- 2024-11-29
AI Technical Summary
The existing surface corrosion methods of silicon carbide ceramics have complex equipment, dangerous chemical use, large safety hazards, complex operation, and high-temperature molten strong alkali or strong acid corrosion methods pose a threat to the personal safety of experimental personnel, and common methods are difficult to characterize quickly and safely. Sample surface tissue.
The surface corrosion was carried out using Murakami's reagent (a mixture of KOH, K3[Fe(CN)6] and H2O), the corrosion temperature was controlled at 200-250℃, the corrosion time was controlled at 1-10 minutes, and the diamond sand disk and polished velvet cloth were used. Samples are sanded and polished and subsequently corroded on the heating platform.
The surface corrosion of silicon carbide ceramics with safe, fast and low risk coefficient is achieved, which significantly reduces the corrosion temperature and time. The grain shape is complete and the grain boundaries are clear under the observation of microstructure, which simplifies the operation steps and improves the experimental safety.
Smart Images

Figure CN119043852A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a surface corrosion method for pure silicon carbide ceramics, belonging to the technical field of silicon carbide ceramic material preparation. Background Art
[0002] Silicon carbide (SiC) ceramics have broad application prospects in the fields of bulletproof armor, semiconductors, and extreme environment structural parts due to their low density, high hardness, high thermal conductivity, high oxidation resistance, and high chemical inertness. Silicon carbide is mainly α-crystalline and β-crystalline, and the β-crystalline will transform into the α-crystalline when the temperature is higher than 1800°C. At present, the method for obtaining dense ceramic bodies of silicon carbide is mainly to add sintering aids and high-temperature sintering. For example, CN104926309 mixes alumina with a mass ratio of 0.6-10% of SiC, phenolic resin with a mass ratio of 2.4-31.7% of SiC, or carbon black with a mass ratio of 0.7-9.6% of SiC with submicron silicon carbide powder, and hot-presses and sinters at 2050-2300°C to obtain dense silicon carbide ceramics. However, adding sintering aids will introduce impurity phases, affecting the high-temperature performance of silicon carbide ceramics. High-temperature sintering methods such as pressureless sintering and hot pressing sintering require high sintering temperatures and long process times, which can also cause abnormal grain growth. Spark plasma sintering (SPS) is a low-temperature rapid sintering method. Under the same conditions, the sintering temperature is 100-150°C lower than that of pressureless sintering. It can achieve dense bulk ceramic sintering and the sample has good mechanical properties.
[0003] Organization observation is a conventional test method used by technicians to characterize ceramics according to relevant standards and regulations. Through microstructure, data such as the internal grain morphology, size, distribution, and internal organizational defects of silicon carbide ceramics can be obtained, which is convenient for further organizational analysis and mechanical property testing of sintered samples.
[0004] In order to quantify the relationship between the structure and performance of silicon carbide ceramics, the surface of the sample needs to be corroded to observe the microstructure. The current surface corrosion treatment methods mainly include plasma etching and chemical etching. Plasma etching refers to the use of a mixed gas of CF4 and O2 to excite a highly chemically active plasma. Under the action of an electric field, ions bombard the surface of the sample at high speed, thereby etching the sample. However, the equipment required for this etching method is complex, and this high-energy impact is prone to introduce high residual stress, which will cause irreversible damage to the sample itself. Chemical etching can be divided into high-temperature molten strong alkali etching and strong acid etching. High-temperature molten strong alkali etching refers to placing the ceramic sample in molten NaOH or KOH for 1 minute. The heating temperature of this method is relatively high, greater than 400°C, which is prone to safety hazards and complex operation; strong acid corrosion refers to the use of a high-concentration hydrofluoric acid or a mixed reagent of hydrofluoric acid and nitric acid, which is corroded at room temperature or high temperature for more than 10 minutes. This method has high safety hazards and high requirements for equipment and instruments. The strong alkali and strong acid reagents used in the above corrosion methods are dangerous chemical samples in the laboratory and are highly toxic, which can easily cause damage to the personal safety of the experimenters, and general research institutions and units do not have the qualifications to purchase them. Therefore, in order to quickly characterize the surface structure of the sample, a convenient, safe and fast surface corrosion method is necessary.
[0005] Based on the above problems, the purpose of the present invention is to provide a safer and more convenient surface corrosion method for pure silicon carbide ceramics, which is simple to operate and has a low risk factor. The chemical reagent used in the method is Murakami's reagent, which consists of KOH, K3[Fe(CN)6] (potassium hexacyanoferrate) and H2O, with a mass ratio of 1:1:10. Murakami's reagent is a commonly used chemical reagent and can be purchased directly. The equipment required for the method is simple, which is a heating platform or an electric furnace. The key to the present invention is the corrosion temperature and corrosion time. The corrosion temperature is between 200-250°C. When the temperature is low, the corrosion effect is not obvious and the complete silicon carbide grain boundary cannot be presented. The corrosion temperature is high, the reagent evaporates quickly, and when the temperature of potassium hexacyanoferrate is higher than 300°C, the components will decompose to a certain extent, and the corrosion effect will be reduced. The corrosion time is also important. If the time is short, the grain boundary is not clear, the corrosion test is long, and some grains are severely corroded, resulting in poor surface morphology quality. Summary of the invention
[0006] The invention provides a surface corrosion method for pure silicon carbide ceramics. On the premise of effectively corroding the silicon carbide ceramics, the method simplifies the operation steps, reduces the risk factor and the corrosion temperature, and shortens the corrosion time.
[0007] A surface corrosion method for pure silicon carbide ceramics in the present invention mainly includes the following process steps:
[0008] 1) Sintering of pure silicon carbide ceramics: first, α-crystalline SiC spherical powder with a particle size of 1μm-40μm is directly loaded into a graphite mold, and then the graphite mold is placed in a spark plasma sintering device for high-temperature sintering. The temperature is raised to 1700-1750℃ at a heating rate of 100℃ / min, the sintering pressure is 80-100MPa, and the heat preservation and pressure holding time is 1-10min. After sintering, it is naturally cooled in the furnace to obtain a pure silicon carbide ceramic sample. The sample is processed into a long strip with a size of 3mm×4mm×8mm using a diamond wire cutting machine.
[0009] 2) Surface treatment of silicon carbide ceramics: The prepared silicon carbide ceramic strip samples were polished with diamond sand discs ranging from coarse to fine. The specifications of the diamond sand discs were 1000 mesh and 2000 mesh respectively. The polishing method was to press the sample evenly with fingers until the wear marks of the sample were consistent after polishing. Then, the sand disc of the next specification was replaced, the sample was rotated 45°, and polishing was continued until the wear marks of the previous pass disappeared and new wear marks with consistent directions were formed.
[0010] Then polish with a polishing flannel coated with diamond abrasive paste. The specifications of the abrasive paste are 3.5μm, 2.5μm, and 0.5μm. The polishing method is to place the sample on a polishing machine with a polishing flannel cloth, first apply a 3.5μm abrasive paste, press the sample with your fingers, and rotate the sample perpendicular to the scratch on the sample surface. Polish for 1h, then apply the next specification of abrasive paste, rotate the sample 45°, and repeat the above operation until the sample surface is mirror-bright and scratch-free after polishing with a 0.5μm polishing paste.
[0011] 3) Silicon carbide ceramic surface corrosion: Murakami's reagent is added to a reaction container, and the reaction container containing the reagent is placed on a heating platform or a temperature-controllable device and heated to 200-250°C, and kept warm; the polished silicon carbide sample is placed in the reaction container and corrosion is started; the corrosion is completed after 1-10 minutes, and the corroded silicon carbide sample is placed in a beaker filled with clean water and ultrasonically cleaned for 0.1-5 minutes, and then placed in a beaker filled with anhydrous ethanol and ultrasonically cleaned for 0.1-5 minutes, and finally dried.
[0012] Alternatively, Murakami's reagent and the polished silicon carbide sample can be directly placed in a reaction container at the same time, and the reaction container is placed on a heating platform or a temperature-controllable device and heated to 200-250° C. and kept warm; the corrosion is completed after 1-10 minutes, and the corroded silicon carbide sample is placed in a beaker filled with clean water for ultrasonic cleaning for 0.1-5 minutes, and then placed in a beaker filled with anhydrous ethanol for ultrasonic cleaning for 0.1-5 minutes, and finally dried.
[0013] The corroded silicon carbide ceramic sample is placed under an optical microscope to observe the corresponding microstructure. It can be found that the silicon carbide ceramic corroded by this method has complete grain shape and clear grain boundaries.
[0014] All the above steps are carried out under normal pressure and air atmosphere.
[0015] The beneficial effects of the present invention include:
[0016] The reagents used in the present invention are common chemical reagents, which can be purchased directly and are convenient to obtain.
[0017] The present invention reduces the corrosion temperature to 200-250° C., has low temperature, high safety and simple operation.
[0018] The present invention reduces the corrosion time to 1-10 minutes, has a fast corrosion speed, and significantly reduces the risk factor and operation difficulty of the corrosion test. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] Figure 1 The microstructure of the silicon carbide ceramic sample in the embodiment after being corroded in a reagent at 250°C for 5 minutes
[0020] Figure 2 This is the microstructure picture of the silicon carbide ceramic sample in the comparative example after being corroded in a reagent at 100℃ for 1h.
[0021] Figure 3 This is the microstructure picture of the silicon carbide ceramic sample in the comparative example after being corroded in a reagent at 25℃ for 1h. DETAILED DESCRIPTION
[0022] The present invention is further described below in conjunction with the accompanying drawings and specific examples. It should be understood that the following examples are only used to further illustrate the present invention and cannot be understood as limiting the scope of protection of the present invention. Some non-essential improvements and adjustments made by those skilled in the art based on the above content of the present invention belong to the scope of protection of the present invention. The specific process parameters and the like in the following examples are also only examples within a suitable range, that is, those skilled in the art can make a selection within a suitable range through the description herein, and are not limited to the specific values exemplified below.
[0023] Example 1
[0024] Step 1) Sintering of pure silicon carbide ceramics: first, directly load α-crystalline SiC spherical powder with a powder particle size of 40 μm into a graphite mold, and then place the graphite mold in a spark plasma sintering device for high-temperature sintering, heating the temperature to 1750°C at a heating rate of 100°C / min, the sintering pressure is 80 MPa, and the heat preservation and pressure holding time is 5 minutes. After sintering, it is naturally cooled in the furnace to obtain a pure silicon carbide ceramic sample, and the sample is processed into a long strip with a size of 3 mm×4 mm×8 mm using a diamond wire cutting machine.
[0025] Step 2) Surface treatment of silicon carbide ceramics: The prepared silicon carbide ceramic strip samples are polished with diamond sand discs from coarse to fine. The specifications of the diamond sand discs are 1000 mesh and 2000 mesh respectively. The polishing method is to press the sample evenly with your fingers until the wear marks of the sample are consistent after polishing. Then, replace the sand disc with the next specification, rotate the sample 45°, and continue polishing until the wear marks of the previous pass disappear and new wear marks with consistent directions are formed.
[0026] Then polish with a polishing flannel coated with diamond abrasive paste. The specifications of the abrasive paste are 3.5μm, 2.5μm, and 0.5μm. The polishing method is to place the sample on a metallographic polishing machine with a polishing flannel cloth, first apply a 3.5μm abrasive paste, press the sample with your fingers, and rotate it perpendicular to the scratches on the sample surface. Polish for 1h, then apply the next specification of abrasive paste, rotate the sample 45°, and repeat the above operation until the sample surface is mirror-bright and scratch-free after polishing with a 0.5μm polishing paste.
[0027] Step 3) Silicon carbide ceramic surface corrosion: use a rubber-tipped dropper to draw 10 ml of Murakami's reagent into a glass beaker, place the glass beaker on a multi-functional heating platform, heat to 250°C at a heating rate of 100°C / min, keep warm, use tweezers to completely immerse the polished silicon carbide sample in the corrosion reagent, and gently stir with a glass rod. Corrode for 5 minutes. After the corrosion is completed, use tweezers to take out the sample and place it in a beaker filled with a large amount of deionized water for ultrasonic cleaning for 2 minutes, then place it in a beaker filled with a large amount of anhydrous ethanol for ultrasonic cleaning for 2 minutes, and finally blow dry the sample with a hair dryer.
[0028] Step 4) The corroded silicon carbide ceramic sample is placed under an optical microscope to observe the corresponding microstructure. It can be found that the silicon carbide ceramic corroded by this method has a complete grain shape and clear grain boundaries.
[0029] The silicon carbide ceramic obtained by etching in this embodiment was observed under an optical microscope, and its microstructure is as follows: Figure 1 shown.
[0030] Comparative Example 1-1
[0031] Step 1) is the same as in Example 1.
[0032] Step 2) is the same as in Example 1.
[0033] Step 3) Silicon carbide ceramic surface corrosion: use a rubber-tipped dropper to draw 10 ml of Murakami's reagent into a glass beaker, place the glass beaker on a multi-functional heating platform, heat to 100 ° C at a heating rate of 100 ° C / min, keep warm, use tweezers to completely immerse the polished silicon carbide sample in the corrosion reagent, and gently stir with a glass rod. Corrode for 1 hour. After the corrosion is completed, use tweezers to take out the sample and place it in a beaker filled with a large amount of deionized water for ultrasonic cleaning for 2 minutes, then place it in a beaker filled with a large amount of anhydrous ethanol for ultrasonic cleaning for 2 minutes, and finally blow dry the sample with a hair dryer.
[0034] Step 4) The corroded silicon carbide ceramic sample is placed under an optical microscope to observe the corresponding microstructure, and it can be found that no corrosion occurs on the surface of the sample.
[0035] The silicon carbide ceramic obtained by corrosion in this comparative example was observed under an optical microscope, and its microstructure is as follows: Figure 2 shown.
[0036] Comparative Example 1-2
[0037] Step 1) is the same as in Example 1.
[0038] Step 2) is the same as in Example 1.
[0039] Step 3) Surface corrosion of silicon carbide ceramics: Use a rubber-tipped dropper to draw 10 ml of Murakami's reagent into a glass beaker, place the glass beaker on a multi-functional heating platform, set the temperature to 25°C, use tweezers to completely immerse the polished silicon carbide sample in the corrosion reagent, and gently stir with a glass rod. Corrode for 1 hour. After the corrosion is completed, use tweezers to take out the sample and place it in a beaker filled with a large amount of deionized water for ultrasonic cleaning for 2 minutes, then place it in a beaker filled with a large amount of anhydrous ethanol for ultrasonic cleaning for 2 minutes, and finally use a hair dryer to blow dry the sample.
[0040] Step 4) The corroded silicon carbide ceramic sample is placed under an optical microscope to observe the corresponding microstructure. It can be found that the corrosion effect on the sample surface is not good, the grains of the corroded sample are incomplete, and the grain boundaries are not clear.
[0041] The silicon carbide ceramic obtained by corrosion in this comparative example was observed under an optical microscope, and its microstructure is as follows: Figure 3 shown.
Claims
1. A surface corrosion method for pure silicon carbide ceramics, characterized in that: The following steps are involved: 1) Sintering of pure silicon carbide ceramics: first, put silicon carbide powder into a graphite mold, then place the graphite mold in a spark plasma sintering device for high-temperature sintering, and naturally cool with the furnace after sintering to obtain a pure silicon carbide ceramic sample; 2) Surface treatment of silicon carbide ceramics: Grind and polish the silicon carbide ceramic sample with a diamond sand disc, and then polish it with a polishing cloth coated with diamond abrasive paste until the sample surface is mirror-like; 3) Silicon carbide ceramic surface corrosion: Add Murakami's reagent into a reaction container, place the reaction container containing the reagent into a heating platform or a temperature-controllable device, heat it to a set temperature, and keep it warm; place the polished silicon carbide sample into the reaction container and start corrosion; the corroded silicon carbide sample is first washed with deionized water, then washed with anhydrous alcohol and dried.
2. A surface corrosion method for pure silicon carbide ceramics, characterized in that: The following steps are involved: 1) Sintering of pure silicon carbide ceramics: first, put silicon carbide powder into a graphite mold, then place the graphite mold in a spark plasma sintering device for high-temperature sintering, and naturally cool with the furnace after sintering to obtain a pure silicon carbide ceramic sample; 2) Surface treatment of silicon carbide ceramics: Grind and polish the silicon carbide ceramic sample with a diamond sand disc, and then polish it with a polishing cloth coated with diamond abrasive paste until the sample surface is mirror-like; 3) Silicon carbide ceramic surface corrosion: Add Murakami's reagent and silicon carbide sample into a reaction container, place the reaction container in a heating platform or a temperature-controllable device, heat to a set temperature, and keep warm; the corroded silicon carbide sample is first washed with deionized water, then washed with anhydrous alcohol and then dried.
3. A surface corrosion method for pure silicon carbide ceramics according to any one of claims 1-2, characterized in that: The silicon carbide powder is α-crystalline SiC spherical powder with a particle size of 1-40 μm; the specific process of spark plasma sintering is as follows: the sintering temperature is 1700-1750° C., the sintering pressure is 80-100 MPa, and the heat preservation and pressure holding time is 1-10 min.
4. A surface corrosion method for pure silicon carbide ceramics according to any one of claims 1-2, characterized in that: The diamond grinding discs are 1000 mesh and 2000 mesh respectively.
5. A surface corrosion method for pure silicon carbide ceramics according to any one of claims 1-2, characterized in that: The specifications of diamond grinding paste are 3.5μm, 2.5μm and 0.5μm respectively.
6. A surface corrosion method for pure silicon carbide ceramics according to any one of claims 1-2, characterized in that: The corrosion heating temperature is 200-250°C, the corrosion time is 1-10min, the deionized water cleaning time is 0.1-5min, and the anhydrous alcohol cleaning time is 0.1-5min.
7. A surface corrosion method for pure silicon carbide ceramics according to any one of claims 1-2, characterized in that: The pure silicon carbide ceramics corroded by this method have obvious grain shapes and clearly visible grain boundaries.
Citation Information
Cited By
Uniform separation device for ceramic sintering and ceramic sintering method