Integrally-formed heat insulation felt and preparation method thereof

Through the preparation method of integrated molding insulation felt, the mixing of stirring and beating and thickening liquid is used to form a network structure, which solves the problems of glue waste and process complexity, and achieves efficient thermal insulation and mechanical performance improvement.

CN118769449APending Publication Date: 2024-10-15GONG YI VAN RES INNOVATION COMPOSITE MATERIAL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410844685.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-27
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

The existing airgel felt preparation process has the problems of glue waste, multiple process steps, and high cost. It is difficult to ensure the thermal insulation performance and mechanical properties while reducing glue waste.

Method used

Using the preparation method of integrated molded thermal insulation felt, by mixing the beating and thickening liquid, adding adhesive and thermal insulation powder, a pre-finished liquid is formed for deposition and drying, thereby reducing glue dripping and remaining waste, forming Mesh structure to improve thermal insulation and mechanical properties.

Benefits of technology

It effectively reduces the waste of glue, simplifies the process steps, reduces production costs, improves the thermal insulation performance and mechanical properties, and forms a dense and uniform thermal insulation felt.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004915380500000091
    Figure BDA0004915380500000091
  • Figure BDA0004915380500000101
    Figure BDA0004915380500000101
Patent Text Reader

Abstract

The invention belongs to the technical field of heat insulation materials, and relates to an integrally-formed heat insulation felt and a preparation method thereof, and the preparation method comprises the following steps: preparing pretreatment slurry: taking water and fibers, stirring and pulping, uniformly mixing, adding an adhesive, and uniformly mixing again to prepare the pretreatment slurry; preparing a thickening liquid: mixing a thickening agent with water to prepare the thickening liquid; preparing a pre-finished product liquid: uniformly mixing a thickening liquid, the pretreatment slurry and heat insulation powder to prepare the pre-finished product liquid; the heat insulation powder comprises aerogel powder; the mass ratio of the fibers to the adhesive to the water to the heat insulation powder in the pre-finished product liquid is 1: (0.5-5): (100-200): (0.1-1.1); preparing a finished product: depositing the pre-finished product liquid to obtain a deposition layer, and drying to obtain the finished product. The invention belongs to the technical field of heat insulation materials, and relates to an integrally formed heat insulation felt and a preparation method thereof, so that a prepared heat insulation mat has good heat insulation performance and mechanical performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of thermal insulation materials, and relates to an integrated thermal insulation felt and a preparation method thereof. The prepared thermal insulation mat has good thermal insulation performance and mechanical properties. Background Art

[0002] Aerogel, as a natural thermal insulation material, is currently one of the main raw materials for the preparation of thermal insulation pads. However, due to its low mechanical properties, it usually needs to be attached to fibers to be prepared into aerogel felt. Aerogel felt is also reinforced with fibers to prepare aerogel felt with thermal insulation properties. The resulting aerogel felt is widely used in energy storage, household, petrochemical and construction, pipeline insulation and other fields.

[0003] The preparation of existing aerogel felt usually requires first obtaining fiber felt, then preparing glue, mixing the glue and the fiber felt for impregnation, obtaining the aerogel felt composite of the fiber felt and the glue through a real-time gel process, and then taking it out for drying and aging. However, during this process, there will be glue left over, and the glue will also drip from the fiber felt during the impregnation process. The glue will also gel during the residual and dripping process, making it impossible to recycle it and combine it with the fiber felt for a second time. Therefore, a large amount of glue will be wasted, and there are many steps and high process costs. Therefore, it is necessary to develop a new method to prepare thermal insulation pads to reduce the waste of glue while ensuring the performance of aerogel thermal insulation pads. Summary of the invention

[0004] In view of the above technical problems, the present invention provides an integrated thermal insulation felt and a preparation method thereof, which can reduce the waste of aerogel and improve the thermal insulation performance of the prepared aerogel felt.

[0005] To achieve the above object, the present invention adopts the following technical solutions:

[0006] In a first aspect, the present invention provides a method for preparing an integrated thermal insulation felt, characterized in that it comprises the following steps:

[0007] Preparing pretreated pulp: taking water and fibers, stirring and beating, and after mixing evenly, adding a binder, and mixing evenly again to prepare pretreated pulp;

[0008] Preparing a thickening liquid: mixing a thickener and water to prepare a thickening liquid;

[0009] Preparing a pre-finished product liquid: uniformly mixing the thickening liquid, the pre-treated slurry and the thermal insulation powder to prepare a pre-finished product liquid; the thermal insulation powder comprises aerogel powder; the mass ratio of fiber, adhesive, water and thermal insulation powder in the pre-finished product liquid is 1: (0.5-5): (100-200): (0.1-1.1);

[0010] Preparation of finished product: sediment the pre-finished product liquid to obtain a supernatant and a sediment layer, and dry the sediment layer to obtain the finished product.

[0011] Beneficial effects: This solution firstly stirs and slurries water and fibers, then adds an adhesive, under the action of the adhesive, the fibers can be bonded and entangled, and then a thickening liquid is prepared. After the pretreated slurry and the thickening liquid are mixed, the thermal insulation powder (including aerogel powder) is added to obtain a pre-finished liquid. Compared with aerogel glue, the use of aerogel powder reduces the dripping of glue and the waste of residual glue caused by the real-time gelation process. At the same time, compared with the production method of thermal insulation pads of glue-impregnated fiber felt, the steps are simple, saving production processes and costs.

[0012] The adhesive allows the interlaced fibers to form a network structure. On the one hand, the network structure reduces the deposition rate of the fibers in subsequent steps and reduces the difference in deposition rate between the fibers and the thermal insulation powder. On the other hand, it allows the thermal insulation powder to be filled into the pores of the network structure formed by the fibers. As a result, the integrated felt structure formed by subsequent drying is denser and the thermal insulation performance is more uniform and better. The combination of the network structure fibers and the filling of the thermal insulation powder also makes the prepared integrated felt have better mechanical properties and is not easy to break. Since the density of the fiber is higher than that of the aerogel powder, the deposition rate of the fiber is faster than that of the aerogel powder. However, under the action of the thickening liquid, the viscosity of the pre-finished product liquid is increased. In the pre-finished product liquid with a certain viscosity, since the surface area and aspect ratio of the fiber are much larger than those of the aerogel powder particles, the deposition resistance encountered is greater than that of the aerogel powder. Therefore, when settling, the fiber is more obstructed than the aerogel powder, and the decrease in the deposition rate is greater than that of the aerogel powder. Therefore, the thickener can adjust the deposition rate difference between the fiber and the thermal insulation powder, so that the fiber and the thermal insulation powder in the prepared deposition layer can be evenly combined and distributed, so that the obtained integrated felt has good thermal insulation and mechanical properties.

[0013] Furthermore, the binder used in preparing the pretreated pulp is at least one of polyacrylate and polyurethane.

[0014] Furthermore, the fiber used in preparing the pretreated pulp is at least one of preoxidized silk fiber, glass fiber, quartz fiber, mullite fiber, aluminum silicate fiber, alumina fiber, and basalt fiber.

[0015] Furthermore, the thickener used in preparing the thickened liquid is at least one of sodium polyacrylate, polyvinyl pyrrolidone, polyacrylamide, carboxymethyl cellulose, and hydroxypropyl methyl cellulose.

[0016] Furthermore, in the preparation of the finished product, the pre-finished product liquid is deposited to obtain a deposited layer, and then the deposited layer is subjected to a hydrophobic treatment and dried.

[0017] The hydrophobic treatment includes a gas phase hydrophobic method, a liquid phase hydrophobic method or spraying a prepared hydrophobic agent on the surface of the deposited layer;

[0018] Furthermore, the pre-finished product liquid also includes a functional filler; the functional filler is at least one of silicon carbide and titanium dioxide.

[0019] The addition of titanium dioxide can increase the ability of the thermal insulation powder to resist light radiation, reduce the temperature rise caused by light radiation, and further improve the thermal insulation performance of the prepared thermal insulation felt.

[0020] Furthermore, in the preparation of the pre-finished product liquid, the mass ratio of the fiber to the functional filler is 100:(5-40).

[0021] Furthermore, the thermal insulation powder in the preparation of the pre-product liquid also includes fumed silica powder; the mass ratio of the fumed silica powder to the aerogel powder is 10:(1-5); the particle size of the fumed silica used is 0.05 μm to 0.5 μm; the particle size of the aerogel powder used is 2 to 100 nm;

[0022] Furthermore, the fiber is pretreated before use, and the pretreatment includes immersing the fiber in a pretreatment solution for 5-10 minutes and then taking it out and drying it; the pretreatment solution is composed of hydrochloric acid, water and chitosan in a mass ratio of (4-6): (95-110): (8-13).

[0023] Technical effect: By pretreating the fibers, the fiber surface is first etched by the hydrochloric acid in the pretreatment liquid to increase the roughness of the fiber surface. During subsequent deposition, the friction between the fibers when entangled with each other is increased, and the network structure formed is more firm and stable. At the same time, since chitosan is a hydrophilic product, the chitosan is covered on the fiber surface through fiber impregnation, and the hydrophilicity of the fiber surface is improved. Since the aerogel powder in the thermal insulation powder is a hydrophilic powder, during the deposition process, the aerogel powder and the fiber are attracted by the hydrophilic groups, so that the powder can be more firmly and stably filled in the network structure formed by the fiber, thereby improving the mechanical properties of the prepared aerogel pad and the thermal insulation performance.

[0024] In a second aspect, the present invention provides an integrated thermal insulation felt, comprising fibers, a thickener, an adhesive and thermal insulation powder; the mass ratio of the fibers, thickener, adhesive and thermal insulation powder used is (75-95): (0.005-0.05): (1-10): (4-30).

[0025] Compared with the prior art, the beneficial effect of the present invention lies in: by combining the thermal insulation powder containing aerogel powder with fibers, the fibers are crossed through deposition to form a network structure, the thermal insulation powder is deposited in the network structure, the network structure is filled, and then the mold is opened and dried to prepare a thermal insulation pad, which effectively reduces the waste of aerogel glue and also makes the prepared thermal insulation pad have good mechanical properties and thermal insulation properties. DETAILED DESCRIPTION

[0026] The following examples are used to illustrate the present invention, but are not intended to limit the scope of the present invention. Unless otherwise specified, the technical means used in the examples are conventional means known to those skilled in the art. The test methods in the following examples are conventional methods unless otherwise specified.

[0027] In one embodiment, the drying in the prepared product is supercritical drying, atmospheric drying or freeze drying. The drying temperature of ethanol supercritical drying is 245-260°C, the drying pressure is 8-11MPa, the heating rate is 5-20°C / min, the supercritical state holding time is 0.5h-3h, and the degassing time is 3h-9h; the drying temperature of CO2 supercritical drying is 40-55°C, the drying pressure is 8-20MPa, the heating rate is 1-5°C / min, the replacement time is 3h-12h, and the degassing time is 3h-12h; the atmospheric drying treatment is 6h-24h after the normal alkane solvent is replaced, and 6h-24h is dried at 50-80°C; the freeze drying treatment is a pre-freezing time of 3-12h, a pre-freezing temperature of -30°C to -5°C, a cold trap temperature of -60 to -40°C, a vacuum degree of 10-500Pa, and a drying time of 12h to 36h.

[0028] In one embodiment, the integrated thermal insulation felt is packaged after it is dried. The packaging uses a packaging film material, and the packaging film material used is an organic film material with an adhesive attached to the surface, and the organic film material is one of PET, PI, PE, PEEK, PTFE, PVC, PP, and PC films. The packaging can improve the protective effect of the integrated thermal insulation felt. At the same time, the adhesive on the surface of the packaging film is melted by hot pressing, and then bonded to wrap and package the integrated thermal insulation felt, so that the organic film protects the integrated thermal insulation felt and reduces the cracking and powdering of the integrated thermal insulation felt during use.

[0029] Example 1

[0030] A method for preparing an integrated thermal insulation felt mainly comprises the following steps:

[0031] S1: water and fiber are put into a mixing barrel, and the mixture is stirred and slurried by a stirring paddle at a stirring rate of 1300 r / min for 10 min, then the stirring rate is increased to 2500 r / min for 17 min, then the stirring rate is reduced to 1000 r / min for 3 min, and after stirring evenly, a binder is added, and the mixture is stirred evenly again to prepare a pretreated slurry; the binder used is polyacrylate; the fiber used is ceramic fiber;

[0032] S2: Take another mixing barrel, put the thickener and water into the mixing barrel and mix them evenly to prepare a thickened liquid; the mass ratio of the thickener to the fiber is 0.1:1; the mass ratio of the thickener to the water is 1:10; the thickener used is sodium polyacrylate;

[0033] S3: after the thickening liquid in step S2 is evenly mixed with the pretreated slurry prepared in step S1, thermal insulation powder is added, and after being evenly mixed, a pre-finished product liquid is prepared; the thermal insulation powder is aerogel powder; the mass ratio of the fiber, adhesive, water, and thermal insulation powder used is 1:3:150:0.6; the particle size of the aerogel powder used is 50nm;

[0034] S4: deposit the pre-finished product liquid, remove the upper clear liquid, obtain the deposited layer, and then open the mold, take samples, and dry.

[0035] An integrated thermal insulation felt is prepared by the above-mentioned method for preparing the integrated thermal insulation felt; the mass ratio of the fiber, the thickener, the adhesive and the thermal insulation powder in the integrated thermal insulation felt is 85:0.03:5:20.

[0036] Example 2

[0037] The difference between this embodiment and embodiment 1 is that the adhesive used in step S1 is composed of polyacrylate and polyurethane in a mass ratio of 1:1, and the rest is the same as in embodiment 1.

[0038] Example 3

[0039] The difference between this embodiment and embodiment 2 is that the fiber used in step S1 is mullite fiber, and the rest is the same as that in embodiment 2.

[0040] Example 4

[0041] The difference between this embodiment and embodiment 2 is that the fiber used in step S1 is a mixture of mullite fiber and ceramic fiber in a mass ratio of 2:1, and the rest is the same as in embodiment 2.

[0042] Example 5

[0043] The difference between this embodiment and embodiment 4 is that the thickener used in step S1 is composed of sodium polyacrylate, polyvinyl pyrrolidone and polyacrylamide in a mass ratio of 1:2:1, and the rest is the same as in embodiment 4.

[0044] Example 6

[0045] The difference between this embodiment and Embodiment 5 is that in step S4, the pre-finished product liquid is deposited, the upper clear liquid is removed to obtain a deposited layer, and then after the mold is opened, a hydrophobic liquid is sprayed on the deposited layer after the mold is opened, and then a sample is taken and dried; the hydrophobic liquid used is prepared by mixing a hydrophobic agent and water in a mass ratio of 1:10, and the hydrophobic agent used is methyltrimethoxysilane; the rest is the same as in Embodiment 5.

[0046] Example 7

[0047] The difference between this embodiment and embodiment 6 is that in step S3, after the thickening liquid in step S2 is mixed with the pretreated slurry prepared in step S1, a functional filler is added after adding the aerogel powder, and then mixed evenly; the functional filler used is silicon carbide, and the rest is the same as in embodiment 6.

[0048] Example 8

[0049] The difference between this embodiment and Embodiment 6 is that in step S3, after the thickening liquid in step S2 is mixed with the pretreated pulp prepared in step S1, a functional filler is added after adding the aerogel powder, and then mixed evenly; the functional filler used is composed of silicon carbide and titanium dioxide in a mass ratio of 2:1; the mass ratio of the fiber to the functional filler is 100:25; and the rest is the same as in Embodiment 6.

[0050] Example 9

[0051] The difference between this embodiment and Embodiment 8 is that the thermal insulation powder also includes fumed silica powder, and the mass ratio of the fumed silica powder to the aerogel powder is 10:3, and the rest is the same as in Embodiment 8; the particle size of the fumed silica powder is 0.3 μm.

[0052] Example 10

[0053] The difference between this embodiment and Embodiment 9 is that the fiber used in step S1 is pretreated before use, and the pretreatment includes placing the fiber in a pretreatment liquid and immersing it for 7 minutes, taking it out and drying it; the pretreatment liquid used is composed of hydrochloric acid, water and chitosan in a mass ratio of 5:100:10, and the rest is the same as in Embodiment 9.

[0054] Comparative Example 1

[0055] The difference between this comparative example and Example 1 is that a method for preparing an integrated thermal insulation felt comprises the following steps:

[0056] S1: Take a mixing barrel, put the thickener and water into the mixing barrel and mix them evenly to prepare a thickening liquid; the mass ratio of the thickener to the fiber is 0.1:1; the mass ratio of the thickener to the water is 1:10; the thickener used is sodium polyacrylate;

[0057] S2: Put water, fiber and thermal insulation powder into a mixing barrel, stir and slurry with a stirring paddle at a stirring rate of 2500r / min for 30min. After mixing evenly, add a binder and stir evenly again to prepare a pretreated slurry; the binder used is polyacrylate; the fiber used is ceramic fiber; the thermal insulation powder is aerogel powder; the mass ratio of the fiber, binder, water and thermal insulation powder used is 1:3:150:0.6;

[0058] S3: the thickening liquid in step S1 is mixed evenly with the pretreated pulp prepared in step S2 to prepare a pre-finished product liquid;

[0059] S4: depositing the pre-finished product liquid in step S3, removing the upper clear liquid, obtaining a deposited layer, and then opening the mold, sampling, and drying.

[0060] Comparative Example 2

[0061] The difference between this comparative example and Example 1 is that the integrated molded thermal insulation felt does not contain a thickener, and the rest is the same as that in Example 1.

[0062] Detection Methods

[0063] Thermal insulation performance of the finished product: Take a heating table, cut the integrated thermal insulation felt prepared in Examples 1 to 10 and Comparative Examples 1 to 2 into samples with a size of 80*80mm and a thickness of 5mm, place them on the heating table, set the heating temperature of the heating table to 675°C, set the heating time to 20min, then measure the temperature of the cold and hot surfaces of the finished aerogel felt, and calculate the temperature difference. The results are shown in Table 1.

[0064] Table 1 Thermal insulation properties of thermal insulation pads obtained in Examples 1 to 10 and Comparative Examples 1 to 2

[0065] Example Temperature difference between hot and cold surfaces (℃) Example 1 380 Example 2 386 Example 3 374 Example 4 393 Example 5 399 Example 6 403 Example 7 410 Example 8 415 Example 9 418 Example 10 431 Comparative Example 1 346 Comparative Example 2 323

[0066] Mechanical properties test:

[0067] The thermal insulation felt was prepared by the preparation method of the integrated thermal insulation felt in Examples 1-10 and Comparative Examples 1-2, and the thickness of the thermal insulation felt was prepared to be 3.8 mm. The thermal insulation felt was prepared into a test sample with a width of 40 mm, and a tensile performance test was performed. The original gauge length was 200 mm, and the tensile strength (MPa) of each test sample was recorded in Table 2;

[0068] Table 2

[0069]

[0070]

[0071] The embodiments described above are only preferred embodiments of the present invention and are only used to explain the present invention, not to limit the scope of implementation of the present invention. For those skilled in the art, other implementation methods can certainly be easily made by replacement or modification based on the technical contents disclosed in this specification. Therefore, all changes and improvements made on the principles of the present invention should be included in the scope of the patent application of the present invention.

Claims

1. A method for preparing an integrated thermal insulation felt, It is characterized by: The steps include: Preparing pretreated pulp: taking water and fibers, stirring and beating, and after mixing evenly, adding a binder, and mixing evenly again to prepare pretreated pulp; Preparing a thickening liquid: mixing a thickener and water to prepare a thickening liquid; Preparing a pre-finished product liquid: uniformly mixing the thickening liquid, the pre-treated slurry and the thermal insulation powder to prepare a pre-finished product liquid; the thermal insulation powder comprises aerogel powder; the mass ratio of fiber, adhesive, water and thermal insulation powder in the pre-finished product liquid is 1: (0.5-5): (100-200): (0.1-1.1); Preparation of finished product: sediment the pre-finished product liquid to obtain a supernatant and a sediment layer, and dry the sediment layer to obtain the finished product.

2. The method for preparing the integrated thermal insulation felt according to claim 1, It is characterized in that The binder used in preparing the pre-treated pulp is at least one of polyacrylate and polyurethane.

3. The method for preparing the integrated thermal insulation felt according to claim 1, It is characterized in that The fiber used in preparing the pre-treated pulp is at least one of pre-oxidized silk fiber, glass fiber, quartz fiber, mullite fiber, aluminum silicate fiber, alumina fiber and basalt fiber.

4. The method for preparing the integrated thermal insulation felt according to claim 1, It is characterized in that The thickener in the preparation of the thickening liquid is at least one of sodium polyacrylate, polyvinyl pyrrolidone, polyacrylamide, carboxymethyl cellulose and hydroxypropyl methyl cellulose.

5. The method for preparing the integrated thermal insulation felt according to claim 1, It is characterized in that The preparation of the finished product further comprises subjecting the deposited layer to a hydrophobic treatment, wherein the hydrophobic treatment is performed before or after drying.

6. The method for preparing the integrated thermal insulation felt according to claim 1, It is characterized in that The pre-finished product liquid also includes a functional filler; the functional filler is at least one of silicon carbide and titanium dioxide.

7. The method for preparing the integrated thermal insulation felt according to claim 6, It is characterized in that In the preparation of the pre-finished product liquid, the mass ratio of the fiber to the functional filler is 100:(5-40).

8. The method for preparing the integrated thermal insulation felt according to claim 1, Features ; The thermal insulation powder used in preparing the pre-product liquid also includes fumed silicon dioxide powder.

9. The method for preparing the integrated thermal insulation felt according to claim 1, It is characterized in that The fiber is pretreated before use, and the pretreatment includes placing the fiber in a pretreatment solution and immersing it for 5-10 minutes, and then taking it out and drying it; the pretreatment solution is composed of hydrochloric acid, water and chitosan in a mass ratio of (4-6): (95-110): (8-13).

10. An integrated thermal insulation felt, It is characterized by: The invention comprises fiber, thickener, adhesive and thermal insulation powder; the mass ratio of the fiber, thickener, adhesive and thermal insulation powder is (75-95): (0.005-0.05): (1-10): (4-30).