Method for constructing micro-nano pattern on surface of polybutylene-1 film based on scanning probe induction
Through the method of constructing micro-nano patterns on the surface of polybutene-1 films induced by scanning probes, the problem of prolonged production cycle and increased cost caused by the spontaneous crystalline transformation of polybutene-1 was solved, and the surface of polybutene-1 films was realized. Micro- and nanoscale control of patterns and wide application of polymer materials.
Patent Information
- Application Number
- CN202410709121.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-03
- Publication Date
- 2024-10-15
AI Technical Summary
Polybutene-1 spontaneously and irreversibly undergoes crystalline transformation, resulting in longer production cycles and increased economic costs.
A method of constructing micro-nano patterns on the surface of polybutene-1 films induced by scanning probes was used. The films were prepared by spin coating and melted and crystallized under a nitrogen protective atmosphere. A silicon nitride probe with a tapered tip was used to scan. Scan in the peak force tapping mode on the probe microscope, adjust the scanning parameters to control the crystalline transformation area, and build a polybutene-1 crystal pattern with controllable size and position.
The micro- and nanoscale control of the surface pattern size and position of the polybutene-1 film has been achieved, broadening the application of polymer ultra-thin films in battery separators, sensors, packaging films and other fields, reducing the production cycle and economic costs.
Smart Images

Figure CN118769576A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of micro / nano processing, and in particular to a method for constructing micro / nano patterns on the surface of a polybutene-1 film based on scanning probe induction. Background Art
[0002] Polybutene-1 has outstanding creep resistance, heat resistance, good toughness, wear resistance and excellent processability. It is widely used in films, pipes and plates and is called "plastic gold". With the commercialization of isotactic polybutene-1, it has significant application prospects in functional materials such as battery separators. As a polycrystalline polymer, polybutene-1 usually forms metastable crystal form II during melt cooling and crystallization. When placed at room temperature, it will spontaneously and irreversibly transform into thermodynamically stable crystal form I. After the crystal transformation, the melting point and mechanical properties of the product are greatly improved. However, the crystal transformation leads to a longer production cycle of the product, increases the economic cost, and greatly limits the application of polybutene-1. Summary of the invention
[0003] The technical problem to be solved by the present invention is that the existing polybutene-1 will spontaneously and irreversibly undergo a crystal transformation, resulting in a longer production cycle and increased economic costs.
[0004] In order to solve the above technical problems, the present invention provides a technical solution: a method for constructing micro-nano patterns on the surface of a polybutene-1 film based on scanning probe induction, comprising the following steps: Step 1: firstly, a polybutene-1 film is prepared by a spin coating method, and the film is post-treated, the treated film sample is melted and crystallized under a nitrogen protective atmosphere, and then quenched to room temperature; Step 2: Install a silicon nitride probe with a conical tip and a moderate elastic modulus on a scanning probe microscope, and then fix the melt-crystallized polybutene-1 film sample on a sample stage; Step 3: Start the scanning probe microscope and select the peak force tapping mode; Step 4: Use a certain frequency to make the probe draw a force curve on the sample surface, use the tip-sample interaction force as the feedback variable, adjust the needle insertion and scanning parameters, and make the probe scan multiple times on the film surface in a certain direction at a certain scanning frequency according to the set scanning trajectory. By adjusting the number of scanning points, the crystal transformation area is controlled and the shape of the constructed pattern is regulated.
[0005] Furthermore, the process of preparing the polybutene-1 film by spin coating is as follows: 0.08-0.1 g of a 100°C polybutene-1 solution is uniformly and rapidly added to a silicon wafer at 40°C-45°C, and after the addition is completed, the polybutene-1 solution is allowed to stand for 1-3 seconds, and the polybutene-1 solution is cooled from 100°C to 80-90°C at an average cooling rate of 5-7°C / min, and then rotated at a speed of 4000 rpm for 1 minute. The prepared polybutene-1 crystalline film has a thickness of 14-15 nm.
[0006] Furthermore, the polybutene-1 film was prepared by spin coating under a nitrogen atmosphere at a temperature of 0.004 m 3 Nitrogen was continuously introduced into the spin coating apparatus at a gas flow rate of / min for 5-6 min to reduce the humidity above the substrate for preparing the polybutene-1 film from 25-27% to 20%.
[0007] Furthermore, the film post-processing step is: placing the polybutene-1 ultra-thin film prepared by the spin coating method in a drying oven, and after closing the drying oven door, the internal temperature is increased from 24°C to 25°C at a rate of 0.5°C / min; the internal humidity is decreased from 33% to 30% at a rate of 1% / min, and dried in an environment with a temperature of 25°C and a humidity of 30% for 2 hours, so that the water molecule adsorption layer on the surface of the polybutene-1 ultra-thin film is thinned from 2nm to 1nm.
[0008] Furthermore, the process of adjusting the needle insertion parameters is as follows: using the intelligent automatic needle insertion mode of motor-assisted piezoelectric ceramic automatic detection, optimizing the needle insertion force of the probe to 0.1200-0.1500V close to the surface of the polybutene-1 melt crystallization sample; The scanning parameter adjustment process is: using the peak force between the probe and the sample as feedback, adjusting the peak force value to 2.2~3nN to contact the sample surface to induce the II-I crystal phase transformation of the polybutene-1 melt crystallization sample, and the crystal phase transformation rate is 2.13 μm2 / min.
[0009] Furthermore, the probe tip scanned the polybutene-1 melt crystallization sample at a frequency of 0.894-1.1 Hz to accelerate the II-I crystal phase transformation of the sample. The scanning angle of the probe was 0°-15°, and the number of scans was 3 times.
[0010] Furthermore, the number of pixels in the first horizontal and vertical scans is 64×64; the number of pixels in the second scan is 128×128; and the number of pixels in the third scan is 512×512. The number of pixels is the number of times the needle tip hits the sample within the scanning range. The first scan hits the sample 64×64 times within the scanning range. The force of the needle tip induces nucleation of type I crystals and accelerates the II-I crystal transformation. The number of pixels is increased in the subsequent two scans, and the II-I crystal transformation is induced by increasing the number of nucleation sites for type I crystals.
[0011] Furthermore, during the scanning process, the scanning probe approaches the surface of the thin film sample at a speed of 5.5 μm / min. When the interaction force between the tip and the sample surface reaches the set peak force of 2.2~3nN, the probe tip leaves the sample surface at a speed of 1 μm / min, thereby obtaining the sample morphology information and the mechanical properties of the surface of the scanning area.
[0012] Furthermore, when the number of scanning points is 64×64, the nucleation density of type I crystal induced by the lateral scanning of the probe tip is about 3.6 / μm 2 , and because the lateral scanning of the probe tip generates a large force between the tip and the sample, and because the points of interaction between the tip and the sample are relatively small, the shape of the crystal transformation zone in the tip-induced polybutene-1 film is a horizontal line connected by many points; when the number of scanning points is 512×512, due to the increase in the points of interaction between the probe tip and the sample, the shape of the crystal transformation zone is transformed into a plane composed of many horizontal lines.
[0013] Furthermore, the environmental parameters for constructing micro-nano patterns on the surface of polybutene-1 film by using scanning probe to induce crystal transformation are: temperature 22~26 ℃ and humidity 30~40%.
[0014] The beneficial effects of the present invention are: The present invention first prepares a polybutene-1 thin film by spin coating; the polybutene-1 ultra-thin film sample is melt-isothermally crystallized in a nitrogen protective atmosphere, quenched to room temperature to obtain a metastable type II lamellar structure, and a probe is used to scan a specific area on the surface of the polybutene-1 crystalline film. Subsequently, a size- and position-controllable polybutene-1 crystalline pattern array is further constructed by selective "melting and dissolving", thereby achieving regulation of the size and position of the pattern on the surface of the polybutene-1 film at the micro-nano scale, thereby broadening the application of polymer ultra-thin film battery separators, sensors, packaging films and other fields.
[0015] In order to make the above and other purposes, features and advantages of the present invention more obvious and easy to understand, preferred embodiments are given below and described in detail with reference to the accompanying drawings. BRIEF DESCRIPTION OF THE DRAWINGS
[0016] In order to more clearly illustrate the technical solutions in the present invention or the prior art, the drawings required for use in the description of the embodiments will be briefly introduced below. Obviously, the drawings described below are only three of the drawings of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.
[0017] Figure 1 A flow chart of the steps of this method is shown in FIG.
[0018] Figure 2This is an atomic force microscope characterization result diagram of the isothermal crystallized thin film sample after solvent dissolution and atomic force microscope tip induction in Example 1.
[0019] Figure 3 This is a polarizing microscope characterization result diagram of the isothermal crystallized thin film sample after partial melting induced by atomic force microscope tip in Example 2.
[0020] Figure 4 This is an atomic force microscope characterization result diagram of the isothermal crystallized thin film sample after partial melting induced by atomic force microscope tip in Example 2. DETAILED DESCRIPTION
[0021] Embodiments of the present invention will be described in more detail below with reference to the accompanying drawings. Although certain embodiments of the present invention are shown in the accompanying drawings, it should be understood that the present invention can be implemented in various forms and should not be construed as being limited to the embodiments described herein, which are instead provided for a more thorough and complete understanding of the present invention. It should be understood that the drawings and embodiments of the present invention are only for exemplary purposes and are not intended to limit the scope of protection of the present invention.
[0022] It should be understood that the various steps described in the method embodiments of the present invention may be performed in different orders and / or in parallel. In addition, the method embodiments may include additional steps and / or omit the steps shown. The scope of the present invention is not limited in this respect.
[0023] The names of the messages or information exchanged between multiple devices in the embodiments of the present invention are only used for illustrative purposes, and are not used to limit the scope of these messages or information.
[0024] In the embodiment of the present invention, the silicon wafer is a P100 silicon wafer produced by Zhejiang Lijing Optoelectronics Technology Co., Ltd., the ultraviolet oxidation lamp is a 30W ultraviolet oxidation lamp produced by Aerospace Hongda, a double U-shaped sterilization ultraviolet lamp, a hot plate is a JF-956s type, a glue machine is a KW-4A glue machine produced by the Institute of Microelectronics of the Chinese Academy of Sciences, polybutene-1 is purchased from Basell of the Netherlands, the atomic force microscope is an Icon atomic force microscope produced by Bruker of the United States, and the scanning probe model is ScanAsyst-Air. Embodiment 1
[0025] like Figure 1 and Figure 2 As shown, a method for constructing micro-nano patterns on the surface of a polybutene-1 film based on scanning probe induction comprises the following steps: Step S1, preparing a polybutene-1 film by spin coating, and post-treating the film, melting and crystallizing the treated film sample under a nitrogen protective atmosphere, and then quenching to room temperature; Step S2, installing a silicon nitride probe with a conical tip and a moderate elastic modulus on a scanning probe microscope, and then fixing the melt-crystallized polybutene-1 film sample on a sample stage; Step S3, start the scanning probe microscope and select the Peak Force Tapping mode; Step S4, use a certain frequency to make the probe make a force curve on the sample surface, use the tip-sample interaction force as a feedback variable, adjust the needle insertion and scanning parameters, and make the probe scan multiple times on the film surface in a certain direction at a certain scanning frequency according to the set scanning trajectory, and control the crystal transformation area by adjusting the number of scanning points, thereby regulating the shape of the constructed pattern.
[0026] In the above step S1: the process of preparing the polybutene-1 film by spin coating is as follows: Wafer surface treatment: 1cm×1cm P100 silicon wafer (doped with boron) was oxidized by ozone generated by ultraviolet light for 40 minutes, wherein the surface undulation of the silicon wafer was less than 1nm, so that the thickness difference of the polybutene-1 film prepared on the substrate was less than 2nm; Preparation of polybutene-1 solution: using polybutene-1 with a weight average molecular weight of 77 kg / mol as a raw material, using toluene as a solvent to prepare a solution with a mass fraction of 0.3%, and heating the solution on a hot plate at 100°C for 1 hour until the solute is completely dissolved; Spin coating preparation: nitrogen gas is continuously introduced into the spin coating device at a gas flow rate of 0.004m3 / min for 5-6min to reduce the humidity above the substrate for preparing the polybutene-1 film from 25-27% to 20%, and the substrate is placed in a nitrogen atmosphere. 0.08-0.1g of 100℃ polybutene-1 solution is quickly and evenly added on a silicon wafer at 40℃~45℃ (add a layer evenly). After the addition is completed, let it stand for 1-3s. The polybutene-1 solution is cooled from 100℃ to 80-90℃ at an average cooling rate of 5-7℃ / min, and then rotated at 4000rpm for 1min. The prepared polybutene-1 crystalline film has a thickness of 14-15nm.
[0027] Among them, the film post-processing steps are: placing the polybutene-1 ultra-thin film prepared by the spin coating method in a drying oven, and after closing the drying oven door, the internal temperature is increased from 24°C to 25°C at a rate of 0.5°C / min; the internal humidity is reduced from 33% to 30% at a rate of 1% / min, and dried in an environment with a temperature of 25°C and a humidity of 30% for 2 hours, so that the water molecule adsorption layer on the surface of the polybutene-1 ultra-thin film is thinned from 2nm to 1nm.
[0028] The process of melt crystallization and quenching to room temperature is as follows: the dried polybutene-1 film sample is placed on a LinKamTHMS600 hot stage, and melt isothermal crystallization is carried out under a nitrogen protective atmosphere. The specific temperature program is as follows: under a nitrogen protective atmosphere, the polybutene-1 ultra-thin film is heated from 25°C to 140°C at a heating rate of 20°C / min, kept at 140°C for 1 min, then cooled from 140°C to 55°C at a cooling rate of 100°C / min, isothermally crystallized at 55°C for 3 min, quenched to room temperature and placed at room temperature for a period of time; the placed sample is heated from 25°C to 120°C at a heating rate of 20°C / min, kept at 120°C for 1 min, then cooled from 120°C to 85°C at a cooling rate of 10°C / min, isothermally crystallized at 85°C for 8 min, and quenched to room temperature.
[0029] In the above step S2: the crystal position on the scanning probe microscope is marked.
[0030] In the above-mentioned step S4: the process of adjusting the needle insertion parameters is: using the intelligent automatic needle insertion mode of motor-assisted piezoelectric ceramic automatic detection, optimizing the needle insertion force (Peak Force Engage Setpoint) of the probe to 0.1200~0.1500V close to the surface of the polybutene-1 molten crystallization sample; so as to avoid excessive interaction force between the probe and the sample during needle insertion to damage the polybutene-1 film sample or the probe tip.
[0031] The scanning parameter adjustment process is as follows: using the peak force between the probe and the sample as feedback, adjusting the peak force value to 2.2-3nN to contact the sample surface to induce the II-I crystal phase transformation of the polybutene-1 melt crystallization sample, and the crystal phase transformation rate is 2.13 μm 2 / min; if the imaging force is too low, the probe tip cannot maintain good interaction with the sample during scanning, which is not conducive to inducing the crystal transformation of the polybutene-1 film; if it is too high, the polybutene-1 film sample or the probe tip will be damaged to a certain extent.
[0032] The frequency adjustment process is as follows: the probe tip scans the polybutene-1 melt crystallization sample at a frequency of 0.894-1.1 Hz to accelerate the II-I crystal transformation of the sample. The actual limit of the scanning frequency is the maximum frequency that can be scanned while avoiding damage to the probe tip and / or minimal damage to the sample. The scanning angle of the probe is 0°-15°.
[0033] The needle insertion parameters, scanning parameters and frequency set above were used, and the number of scans was 3 times; among them, The number of pixels in the first horizontal and vertical scans is 64×64; the number of pixels in the second scan is 128×128; the number of pixels in the third scan is 512×512 (the pixel point is the scanning point, that is, the contact point or force point between the probe tip and the sample surface, and the number of pixels is the number of times the tip hits the sample within the scanning range); the first scan hits the sample 64×64 times within the scanning range, and the force of the tip induces the nucleation of type I crystals and accelerates the II-I crystal transformation; the number of pixels is increased in the subsequent two scans, and the II-I crystal transformation is induced by increasing the number of nucleation sites for type I crystals.
[0034] During the scanning process, the scanning probe approaches the surface of the thin film sample at a speed of 5.5 μm / min. When the interaction force between the tip and the sample surface reaches the set peak force of 2.2~3nN, the probe tip leaves the sample surface at a speed of 1 μm / min, thereby obtaining the sample morphology information and the mechanical properties of the surface of the scanning area, such as adhesion and modulus.
[0035] When the number of scanning points is 64×64, the nucleation density of type I crystal induced by the lateral scanning of the probe tip is about 3.6 / μm 2 , and because the lateral scanning of the probe tip generates a large force between the tip and the sample, and because the points of interaction between the tip and the sample are relatively small, the shape of the crystal transformation zone in the tip-induced polybutene-1 film is a horizontal line connected by many points; when the number of scanning points is 512×512, due to the increase in the points of interaction between the probe tip and the sample, the shape of the crystal transformation zone is transformed into a plane composed of many horizontal lines.
[0036] The environmental parameters for constructing micro-nano patterns on the surface of polybutene-1 film using scanning probe-induced crystal transformation are: temperature 22~26 ℃ and humidity 30~40%.
[0037] Acquisition of micro-nano patterns on the surface of polybutene film: Place the film sample scanned by a scanning probe microscope on a spin coater; Heat toluene to 65°C, and drop the heated toluene on the film in the spin coater, evenly adding a layer (covering the surface of the film sample). After the addition is completed, let it stand for 2 to 3 seconds, and then rotate at 4000 rpm for 1 minute; after the rotation is completed, blow dry the dissolved film with nitrogen until no solvent remains, and the construction of the micro-nano pattern on the surface of the polybutene film is completed. Embodiment 2
[0038] like Figure 3 and Figure 4 As shown, this embodiment is obtained by changing some parameters and preparation steps and other technical features on the basis of the embodiment 1, and the remaining technical features are the same as those of the embodiment 1, and the similarities are not repeated here. Among them, the difference between this embodiment and the embodiment 1 is that: The process of melt crystallization and quenching to room temperature is as follows: the dried polybutene-1 film sample is placed on a LinKamTHMS600 hot stage, and melt isothermal crystallization is carried out under a nitrogen protective atmosphere. The specific temperature program is as follows: under a nitrogen protective atmosphere, the polybutene-1 ultra-thin film is heated from 25°C to 140°C at a heating rate of 20°C / min, kept at 140°C for 1 minute, then cooled from 140°C to 80°C at a cooling rate of 10°C / min, isothermally crystallized at 80°C for 15 minutes, and quenched to room temperature.
[0039] Acquisition of micro-nano patterns on the surface of polybutene film: The film sample scanned by scanning probe microscope is placed on LinKam THMS600 and melt isothermal crystallization is carried out under nitrogen protective atmosphere. The specific temperature program is as follows: under nitrogen protective atmosphere, the polybutene-1 ultra-thin film is heated from 25°C to 109°C at a heating rate of 20°C / min, kept at 109°C for 1 min, then cooled from 109°C to 95°C at a cooling rate of 10°C / min, isothermally crystallized at 95°C for 1 min, and quenched to room temperature. The construction of micro-nano patterns on the surface of polybutene film is completed.
[0040] Note that the above are only preferred embodiments of the present invention and the technical principles used. Those skilled in the art will understand that the present invention is not limited to the specific embodiments herein, and that various obvious changes, readjustments and substitutions can be made by those skilled in the art without departing from the scope of protection of the present invention. Therefore, although the present invention has been described in more detail through the above embodiments, the present invention is not limited to the above embodiments, and may include more other equivalent embodiments without departing from the concept of the present invention, and the scope of the present invention is determined by the scope of the appended claims.
Claims
1. A method for constructing micro-nano patterns on the surface of a polybutene-1 film based on scanning probe induction, comprising the following steps: Step 1: firstly, a polybutene-1 film is prepared by a spin coating method, and the film is post-treated, the treated film sample is melted and crystallized under a nitrogen protective atmosphere, and then quenched to room temperature; Step 2: Install a silicon nitride probe with a conical tip and a moderate elastic modulus on a scanning probe microscope, and then fix the melt-crystallized polybutene-1 film sample on a sample stage; Step 3: Start the scanning probe microscope and select the peak force tapping mode; Step 4: Use a certain frequency to make the probe draw a force curve on the sample surface, use the tip-sample interaction force as the feedback variable, adjust the needle insertion and scanning parameters, and make the probe scan multiple times on the film surface in a certain direction at a certain scanning frequency according to the set scanning trajectory, and control the crystal transformation area by adjusting the number of scanning points to regulate the shape of the constructed pattern.
2. The method for constructing micro-nano patterns on the surface of a polybutene-1 film based on scanning probe induction according to claim 1 is characterized in that: The process of preparing the polybutene-1 film by spin coating is as follows: 0.08-0.1 g of a 100°C polybutene-1 solution is uniformly and rapidly added to a silicon wafer at 40-45°C, and after the addition is completed, the solution is allowed to stand for 1-3 seconds, the polybutene-1 solution is cooled from 100°C to 80-90°C at an average cooling rate of 5-7°C / min, and then rotated at a speed of 4000 rpm for 1 minute. The prepared polybutene-1 crystalline film has a thickness of 14-15 nm.
3. The method for constructing micro-nano patterns on the surface of a polybutene-1 film based on scanning probe induction according to claim 2 is characterized in that: The polybutene-1 film was prepared by spin coating under a nitrogen protective atmosphere with a thickness of 0.004 m 3 Nitrogen was continuously introduced into the spin coating apparatus at a gas flow rate of / min for 5-6 min to reduce the humidity above the substrate on which the polybutene-1 film was prepared from 25-27% to 20%.
4. The method for constructing micro-nano patterns on the surface of a polybutene-1 film based on scanning probe induction according to claim 1 is characterized in that: The film post-treatment steps are as follows: placing the polybutene-1 ultra-thin film prepared by the spin coating method in a drying oven, and after closing the drying oven door, the internal temperature is increased from 24°C to 25°C at a rate of 0.5°C / min; the internal humidity is decreased from 33% to 30% at a rate of 1% / min, and dried in an environment with a temperature of 25°C and a humidity of 30% for 2 hours, so that the water molecule adsorption layer on the surface of the polybutene-1 ultra-thin film is thinned from 2nm to 1nm.
5. The method for constructing micro-nano patterns on the surface of a polybutene-1 film based on scanning probe induction according to claim 1 is characterized by: The process of adjusting the needle insertion parameters is as follows: using the intelligent automatic needle insertion mode of motor plus piezoelectric ceramic automatic detection, optimizing the needle insertion force of the probe to 0.1200~0.1500V close to the surface of the polybutene-1 melt crystallization sample; The scanning parameter adjustment process is: using the peak force between the probe and the sample as feedback, adjusting the peak force value to 2.2~3nN to contact the sample surface to induce the II-I crystal phase transformation of the polybutene-1 melt crystallization sample, and the crystal phase transformation rate is 2.13 μm2 / min.
6. The method for constructing micro-nano patterns on the surface of a polybutene-1 film based on scanning probe induction according to claim 1 is characterized by: The probe tip scans the polybutene-1 melt crystallization sample at a frequency of 0.894-1.1 Hz to accelerate the II-I crystal phase transformation of the sample. The scanning angle of the probe is 0°-15°, and the number of scans is 3 times.
7. The method for constructing micro-nano patterns on the surface of a polybutene-1 film based on scanning probe induction according to claim 6 is characterized by: The number of pixels in the first horizontal and vertical scans is 64×64; the number of pixels in the second scan is 128×128; the number of pixels in the third scan is 512×512. The number of pixels is the number of times the needle tip hits the sample within the scanning range. The first scan hits the sample 64×64 times within the scanning range. The force of the needle tip induces the nucleation of type I crystals and accelerates the II-I crystal transformation. The number of pixels is increased in the subsequent two scans, which induces the II-I crystal transformation by increasing the number of nucleation sites for type I crystals.
8. The method for constructing micro-nano patterns on the surface of a polybutene-1 film based on scanning probe induction according to claim 7 is characterized by: During the scanning process, the scanning probe approaches the surface of the thin film sample at a speed of 5.5 μm / min. When the interaction force between the tip and the sample surface reaches the set peak force of 2.2~3nN, the probe tip leaves the sample surface at a speed of 1 μm / min, thereby obtaining the sample morphology information and the mechanical properties of the surface of the scanning area.
9. The method for constructing micro-nano patterns on the surface of a polybutene-1 film based on scanning probe induction according to claim 8, characterized in that: When the number of scanning points is 64×64, the nucleation density of type I crystal induced by the lateral scanning of the probe tip is about 3.6 / μm 2 , and because the lateral scanning of the probe tip generates a large force between the tip and the sample, and because the points of interaction between the tip and the sample are relatively small, the shape of the crystal transformation zone in the tip-induced polybutene-1 film is a horizontal line connected by many points; when the number of scanning points is 512×512, due to the increase in the points of interaction between the probe tip and the sample, the shape of the crystal transformation zone is transformed into a plane composed of many horizontal lines.
10. The method for constructing micro-nano patterns on the surface of a polybutene-1 film based on scanning probe induction according to any one of claims 5 to 9, characterized in that: The environmental parameters for constructing micro-nano patterns on the surface of polybutene-1 film using scanning probe-induced crystal transformation are: temperature 22~26 ℃ and humidity 30~40%.