Optical glass and optical element
By adjusting the component ratio of optical glass, reducing the thermal expansion coefficient and increasing Young's modulus, the stability problems of existing optical glass in processing and application are solved, and high-performance optical glass materials are realized.
Patent Information
- Application Number
- CN202411138688.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2022-08-26
- Publication Date
- 2024-10-15
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The high thermal expansion coefficient of existing optical glass makes it easy to break during processing, and the small Young's modulus causes deformation, which limits its application in portable electronic devices.
Optical glass with specific component proportions is used, containing SiO2, B2O3, La2O3, ZrO2, TiO2 and BaO, and the refractive index, Abbe number, thermal expansion coefficient and Young's modulus are adjusted to ensure that they are within the range of 1.87~1.93 and 28~35 , Thermal expansion coefficient ≤95×10-7/K, Young’s modulus ≥10000×107Pa.
It achieves low thermal expansion coefficient and high Young's modulus of optical glass, improves its stability and performance in processing and application, and is suitable for high-performance optoelectronic products.
Smart Images

Figure SMS_1 
Figure SMS_10 
Figure SMS_2
Abstract
Description
[0001] This application is a divisional application for the invention patent application with application number 202211032866.1, application date August 26, 2022, and name “Optical Glass and Optical Elements”. Technical Field
[0002] The invention relates to an optical glass, in particular to an optical glass with a lower thermal expansion coefficient and a higher Young's modulus. Background Art
[0003] With the rapid development of portable electronic devices (such as mobile phones, PADs, etc.), the demand for small-sized lenses has grown rapidly. High-refractive-index optical glass can be used to manufacture small-sized lenses because it can obtain a larger viewing angle with a smaller volume. Therefore, it is very important for the development of portable electronic devices. The manufacture of small-sized lenses requires optical glass to have better performance to meet the needs of processing. The optical glass in the prior art is prone to breakage during processing due to its large thermal expansion coefficient, which reduces the yield rate of the glass; at the same time, the large thermal expansion coefficient will cause the glass to have poor thermal shock resistance, thereby limiting the application of optical glass. On the other hand, when optical glass is processed into smaller or thinner optical components, if its Young's modulus is small, it is easy to deform during use. Therefore, the development of high-refractive-index optical glass with a lower thermal expansion coefficient and a higher Young's modulus plays an important role in the development of high-performance optoelectronic products. Summary of the invention
[0004] The technical problem to be solved by the present invention is to provide an optical glass with a lower thermal expansion coefficient and a higher Young's modulus.
[0005] The technical solution adopted by the present invention to solve the technical problem is:
[0006] (1) Optical glass, whose components, expressed in percentage by weight, contain: SiO2: 1-15%; B2O3: 5-20%; La2O3: 25-50%; ZrO2: 1-12%; TiO2: 5-20%; BaO: 5-20%, wherein TiO2 / BaO is 0.3-3.0.
[0007] (2) The optical glass according to (1), wherein the components, expressed in weight percentage, further contain: SrO: 0-10%; and / or CaO: 0-12%; and / or MgO: 0-10%; and / or Y2O3: 0-8%; and / or Gd2O3: 0-8%; and / or Yb2O3: 0-5%; and / or Nb2O5: 0-12%; and / or ZnO: 0-10%; and / or Rn2O: 0-8%; and / or GeO2: 0-5%; and / or WO3: 0-5%; and / or Ta2O5: 0-5%; and / or Al2O3: 0-5%; and / or a clarifier: 0-1%, wherein the Rn2O is one or more of Li2O, Na2O, and K2O, and the clarifier is one or more of Sb2O3, SnO, SnO2, and CeO2.
[0008] (3) Optical glass comprising SiO2, B2O3, La2O3, ZrO2, TiO2 and BaO, wherein the composition is expressed in weight percentage, wherein TiO2 / BaO is 0.3 to 3.0, and the refractive index of the optical glass is n d is 1.87~1.93, Abbe number v d The thermal expansion coefficient is 28 to 35. -30 / 70℃ 95×10 -7 / K or less, Young's modulus E is 10000×10 7 Pa or above.
[0009] (4) The optical glass according to (3), wherein the components, expressed in weight percentage, are: SiO2: 1-15%; and / or B2O3: 5-20%; and / or La2O3: 25-50%; and / or ZrO2: 1-12%; and / or TiO2: 5-20%; and / or BaO: 5-20%; and / or SrO: 0-10%; and / or CaO: 0-12%; and / or MgO: 0-10%; and / or Y2O3: 0-8%; and / or Gd2O3: 0-8%; and / or Yb2O3: 0-5%; and / or Nb2O5: 0-12%; and / or ZnO: 0-10%; and / or Rn2O: 0-8%; and / or GeO2: 0-5%; and / or WO3: 0-5%; and / or Ta2O5: 0-5%; and / or Al2O3: 0-5%; and / or clarifier: 0-1%, wherein Rn2O is one or more of Li2O, Na2O, and K2O, and the clarifier is one or more of Sb2O3, SnO, SnO2, and CeO2.
[0010] (5) The optical glass according to any one of (1) to (4), wherein the composition is expressed in weight percentage, wherein: TiO2 / BaO is 0.4 to 2.0, preferably TiO2 / BaO is 0.6 to 1.5, and more preferably TiO2 / BaO is 0.8 to 1.3; and / or SiO2 / (CaO+BaO) is 0.05 to 1.5, preferably SiO2 / (CaO+BaO) is 0.1 to 1.0, more preferably SiO2 / (CaO+BaO) is 0.2 to 0.85, and further preferably SiO2 / (CaO+BaO) is 0.35 to 0.75; and / or BaO / Nb2O5 is above 0.8, preferably BaO / Nb2O5 is 1.0-20.0, more preferably BaO / Nb2O5 is 1.5-10.0, and further preferably BaO / Nb2O5 is 2.0-5.0; and / or TiO2 / (La2O3+ZnO) is 0.1-0.6, preferably TiO2 / (La2O3+ZnO) is 0.15-0.55, more preferably TiO2 / (La2O3+ZnO) is 0.2-0.5, and further preferably TiO2 / (La2O3+ZnO) is 0.25-0.45.
[0011] (6) The optical glass according to any one of (1) to (4), wherein the composition is expressed in weight percentage, wherein: (CaO + ZnO) / BaO is 0.1 to 3.0, preferably (CaO + ZnO) / BaO is 0.2 to 2.0, more preferably (CaO + ZnO) / BaO is 0.3 to 1.0, and further preferably (CaO + ZnO) / BaO is 0.3 to 0.8; and / or La2O3 / (ZnO + Nb2O5) is 2.0 to 15.0, preferably La2O3 / (ZnO + Nb2O5) is 2.5 to 10.0, more preferably La2O3 / (ZnO + Nb2O5) is 3.0 to 8.0, and further preferably La2O3 / (ZnO + Nb2O5) is 3.5 to 6.0; and / or (ZnO + Gd2O3 + Y2O3) / Ca O is less than 5.0, preferably (ZnO + Gd2O3 + Y2O3) / CaO is less than 4.0, more preferably (ZnO + Gd2O3 + Y2O3) / CaO is 0.2 ~ 3.0, and further preferably (ZnO + Gd2O3 + Y2O3) / CaO is 0.5 ~ 2.0; and / or CaO / (SiO2 + ZrO2) is 0.02 ~ 1.0, preferably CaO / (SiO2 + ZrO2) is 0.05 ~ 0.8, more preferably CaO / (SiO2 + ZrO2) is 0.1 ~ 0.6, and further preferably CaO / (SiO2 + ZrO2) is 0.1 ~ 0.5; and / or RO: 6 ~ 35%, preferably RO: 10 ~ 25%, more preferably RO: 11 ~ 20%, wherein RO is the total content of MgO, CaO, SrO and BaO.
[0012] (7) The optical glass according to any one of (1) to (4), wherein the components are expressed in weight percentage, wherein: SiO2: 3-12%, preferably SiO2: 5-10%; and / or B2O3: 8-17%, preferably B2O3: 10-15%; and / or La2O3: 31-45%, preferably La2O3: 34-40%; and / or ZrO2: 2-10%, preferably ZrO2: 3-8%; and / or TiO2 : 8-18%, preferably TiO2: 11-16%; and / or BaO: 8-18%, preferably BaO: 11-16%; and / or SrO: 0-5%, preferably SrO: 0-2%; and / or CaO: 1-10%, preferably CaO: 2-8%; and / or MgO: 0-5%, preferably MgO: 0-2%; and / or Y2O3: 0-4%, preferably Y2O3: 0-2%; and / or Gd2O3: 0- 4%, preferably Gd2O3: 0-2%; and / or Yb2O3: 0-3%, preferably Yb2O3: 0-1%; and / or Nb2O5: 1-10%, preferably Nb2O5: 2-7%; and / or ZnO: 1-8%, preferably ZnO: 2-7%; and / or Rn2O: 0-4%, preferably Rn2O: 0-2%; and / or GeO2: 0-3%, preferably GeO2: 0-1%; and / or WO3: 0- 3%, preferably WO3: 0-1%; and / or Ta2O5: 0-3%, preferably Ta2O5: 0-1%; and / or Al2O3: 0-3%, preferably Al2O3: 0-1%; and / or clarifier: 0-0.5%, preferably clarifier: 0-0.2%, the Rn2O is one or more of Li2O, Na2O, K2O, and the clarifier is one or more of Sb2O3, SnO, SnO2, and CeO2.
[0013] (8) The optical glass according to any one of (1) to (4), which does not contain WO3; and / or does not contain Ta2O5; and / or does not contain Rn2O; and / or does not contain Al2O3; and / or does not contain GeO2; and / or does not contain Y2O3; and / or does not contain SrO; and / or does not contain MgO; and / or does not contain Gd2O3; and / or does not contain Yb2O3, and the Rn2O is one or more of Li2O, Na2O, and K2O.
[0014] (9) The optical glass according to any one of (1) to (4), wherein the refractive index n of the optical glass is d is 1.87 to 1.93, preferably 1.88 to 1.92, more preferably 1.89 to 1.91, and the Abbe number v d It is 28-35, preferably 29-34, and more preferably 30-33.
[0015] (10) The optical glass according to any one of (1) to (4), wherein the thermal expansion coefficient α of the optical glass is -30 / 70℃ 95×10 -7 / K or less, preferably 90×10 -7 / K or less, more preferably 85×10 -7 / K or less, more preferably 80×10 -7 / K or less; and / or water resistance stability D W Two or more types, preferably one type; and / or 70 420nm or less, preferably λ 70 415nm or less, preferably λ 70 410nm or less; and / or λ5 is 380nm or less, preferably λ5 is 375nm or less, more preferably λ5 is 370nm or less; and / or weather resistance CR is 2 or more, preferably 1; and / or Knoop hardness H K 580×10 7 Pa or more, preferably 590×10 7 Pa or more, more preferably 600×10 7 Pa or more, more preferably 605×10 7 Pa or more; and / or Young's modulus E is 10000×10 7 Pa or more, preferably 10500×10 7 Pa or more, more preferably 11000×10 7 Pa or more; and / or the bubble degree is A grade or more, preferably A0 grade or more, more preferably A 00 Grade; and / or density ρ is 4.90g / cm 3 Below, preferably 4.80g / cm 3 Below, more preferably 4.70g / cm 3 Below, more preferably 4.60 g / cm 3 Below; and / or wear degree F A 125 to 165, preferably 130 to 160, more preferably 135 to 155; and / or transition temperature T g The temperature is 700°C or lower, preferably 690°C or lower, more preferably 680°C or lower, and further preferably 678°C or lower.
[0016] (11) A glass preform made of the optical glass described in any one of (1) to (10).
[0017] (12) An optical element made of the optical glass described in any one of (1) to (10), or made of the glass preform described in (11).
[0018] (13) An optical instrument comprising the optical glass described in any one of (1) to (10) and / or the optical element described in (12).
[0019] The beneficial effects of the present invention are: through reasonable component design, the optical glass of the present invention has a lower thermal expansion coefficient and a higher Young's modulus. DETAILED DESCRIPTION
[0020] The following will describe the embodiments of the optical glass of the present invention in detail, but the present invention is not limited to the following embodiments, and can be implemented by appropriate changes within the scope of the purpose of the present invention. In addition, although there are appropriate omissions of descriptions of the repeated descriptions, the gist of the invention will not be limited thereby, and in the following content, the optical glass of the present invention is sometimes referred to as glass.
[0021] [Optical glass]
[0022] The following is an explanation of the range of each component (ingredient) of the optical glass of the present invention. In the present invention, unless otherwise specified, the content and total content of each component are all expressed in weight percentage (wt%), that is, the content and total content of each component are expressed in weight percentage relative to the total amount of glass material converted into oxide composition. Here, the "composition converted into oxide" means that when the oxides, complex salts and hydroxides used as raw materials for the optical glass components of the present invention decompose and transform into oxides during melting, the total amount of the oxide material is taken as 100%.
[0023] Unless otherwise specified in specific circumstances, the numerical ranges listed in the present invention include upper and lower limits, "above" and "below" include endpoint values, and all integers and fractions included in the range, without being limited to the specific values listed when the range is defined. "And / or" referred to herein is inclusive, for example, "A and / or B" means only A, or only B, or both A and B.
[0024] <Essential Components and Optional Components>
[0025] SiO2 has the effects of adjusting optical constants, improving the chemical stability of glass, maintaining the viscosity suitable for molten glass, reducing abrasiveness and reducing the erosion of refractory materials. In the present invention, by containing more than 1% SiO2, in order to obtain the above-mentioned effect, preferably SiO2 content is more than 3%, more preferably SiO2 content is more than 5%. If SiO2 content is too high, the melting difficulty of glass increases, and the transition temperature rises. Therefore, in the present invention, SiO2 content is upper limited to 15%, preferably upper limited to 12%, more preferably upper limited to 10%.
[0026] B2O3 can improve the melting property and resistance to devitrification of glass, and is conducive to lowering the transition temperature of glass. The present invention obtains the above-mentioned effect by containing more than 5% B2O3, preferably more than 8% B2O3, and more preferably more than 10% B2O3. If the content of B2O3 is too high, the chemical stability of the glass deteriorates, especially the water resistance deteriorates, and the refractive index and light transmittance of the glass decrease. Therefore, the content of B2O3 is less than 20%, preferably less than 17%, and more preferably less than 15%.
[0027] La2O3 is an effective component for increasing the refractive index of glass, and has a significant effect on improving the chemical stability and resistance to devitrification of glass. If its content is less than 25%, it is difficult to achieve the required optical constants; if the content is higher than 50%, the devitrification tendency of the glass increases and the thermal stability deteriorates. Therefore, the content of La2O3 is limited to 25-50%, preferably 31-45%, and more preferably 34-40%.
[0028] Y2O3 can improve the refractive index and devitrification resistance of glass. If its content exceeds 8%, the chemical stability and weather resistance of glass will deteriorate. Therefore, the content of Y2O3 in the present invention is 0-8%, preferably 0-4%, and more preferably 0-2%. In some embodiments, it is further preferred that Y2O3 is not contained.
[0029] Gd2O3 can improve the refractive index and chemical stability of glass, but if its content is higher than 8%, the devitrification resistance and abrasion resistance of glass will deteriorate. Therefore, the content of Gd2O3 is 0 to 8%, preferably 0 to 4%, and more preferably 0 to 2%. In some embodiments, it is further preferred that Gd2O3 is not contained.
[0030] Yb2O3 is also a component that gives glass high refractive and low dispersion properties. If its content exceeds 5%, the anti-crystallization performance of the glass decreases. Therefore, the content of Yb2O3 is 0-5%, preferably 0-3%, more preferably 0-1%, and more preferably no Yb2O3 is contained.
[0031] ZrO2 can improve the viscosity, hardness, refractive index and chemical stability of optical glass, and can also reduce the thermal expansion coefficient of glass; when the content of ZrO2 is too high, the resistance to devitrification of glass decreases, the difficulty of melting increases, the melting temperature rises, and inclusions appear inside the glass and the light transmittance decreases. Therefore, the content of ZrO2 in the present invention is 1-12%, preferably 2-10%, and more preferably 3-8%.
[0032] MgO can effectively reduce the relative partial dispersion of glass, but when the MgO content is too high, the refractive index of the glass is difficult to meet the design requirements, and the anti-crystallization performance and stability of the glass will decrease. Therefore, the MgO content is limited to 0-10%, preferably 0-5%, and more preferably 0-2%. In some embodiments, it is further preferred that MgO is not contained.
[0033] CaO can adjust the optical constants of glass, improve the chemical stability of glass, improve the processing performance of glass, reduce the high temperature viscosity and surface tension of glass, and reduce the difficulty of glass production. If its content is too high, the devitrification resistance of glass will be reduced. Therefore, the content of CaO is 0-12%, preferably 1-10%, and more preferably 2-8%.
[0034] In some embodiments, the ratio of CaO to the total content of SiO2 and ZrO2 (SiO2+ZrO2) (CaO / (SiO2+ZrO2)) is controlled within the range of 0.02 to 1.0, which can optimize the abrasiveness of the glass and prevent the hardness of the glass from deteriorating. Therefore, it is preferred that CaO / (SiO2+ZrO2) is 0.02 to 1.0, and more preferably CaO / (SiO2+ZrO2) is 0.05 to 0.8. Furthermore, controlling CaO / (SiO2+ZrO2) within the range of 0.1 to 0.6 can further reduce the density of the glass and optimize the weather resistance of the glass. Therefore, it is further preferred that CaO / (SiO2+ZrO2) is 0.1 to 0.6, and it is further preferred that CaO / (SiO2+ZrO2) is 0.1 to 0.5.
[0035] SrO can adjust the refractive index and Abbe number in glass, but if the content is too high, the chemical stability and devitrification resistance of the glass will decrease. Therefore, the content of SrO is limited to 0-10%, preferably 0-5%, and more preferably 0-2%. In some embodiments, it is further preferred that SrO is not contained.
[0036] BaO can increase the refractive index, melting property and thermal stability of glass, improve the abrasiveness and light transmittance of glass, but if its content is too high, the density of glass increases and the resistance to devitrification decreases. Therefore, the content of BaO is 5 to 20%, preferably 8 to 18%, and more preferably 11 to 16%.
[0037] In some embodiments, the ratio of SiO2 / (CaO+BaO) between the content of SiO2 and the total content of CaO and BaO (CaO+BaO) is controlled within the range of 0.05 to 1.5, which can improve the weather resistance of the glass and optimize the abrasion resistance of the glass. Therefore, SiO2 / (CaO+BaO) is preferably 0.05 to 1.5, and SiO2 / (CaO+BaO) is more preferably 0.1 to 1.0. Furthermore, controlling SiO2 / (CaO+BaO) within the range of 0.2 to 0.85 can further improve the Young's modulus of the glass and optimize the thermal expansion coefficient of the glass. Therefore, SiO2 / (CaO+BaO) is further preferably 0.2 to 0.85, and SiO2 / (CaO+BaO) is further preferably 0.35 to 0.75.
[0038] In some embodiments, the total content RO of the alkaline earth metal oxides MgO, CaO, SrO, and BaO is controlled within the range of 6 to 35%, so that the glass can more easily obtain the desired optical constants, optimize the chemical stability of the glass, and prevent the glass from reducing the devitrification resistance. Therefore, RO is preferably 6 to 35%, more preferably 10 to 25%, and further preferably 11 to 20%.
[0039] ZnO can adjust the refractive index and dispersion of glass, and reduce the high temperature viscosity and transition temperature of glass. If the content of ZnO is too high, the devitrification resistance of glass will deteriorate. Therefore, the content of ZnO is 0 to 10%, preferably 1 to 8%, and more preferably 2 to 7%.
[0040] In some embodiments, the ratio (CaO+ZnO) / BaO between the total content of CaO and ZnO CaO+ZnO and the content of BaO is controlled within the range of 0.1 to 3.0, which can improve the light transmittance of the glass while preventing the density of the glass from increasing. Therefore, it is preferred that (CaO+ZnO) / BaO is 0.1 to 3.0, and it is more preferred that (CaO+ZnO) / BaO is 0.2 to 2.0. Furthermore, by controlling (CaO+ZnO) / BaO within the range of 0.3 to 1.0, the bubble degree of the glass can be further improved and the Young's modulus of the glass can be prevented from deteriorating. Therefore, it is further preferred that (CaO+ZnO) / BaO is 0.3 to 1.0, and it is further preferred that (CaO+ZnO) / BaO is 0.3 to 0.8.
[0041] In some embodiments, the ratio of the total content of ZnO, Gd2O3, and Y2O3, ZnO+Gd2O3+Y2O3, to the content of CaO, (ZnO+Gd2O3+Y2O3) / CaO, is controlled to be below 5.0, which can reduce the thermal expansion coefficient of the glass and prevent the reduction of weather resistance. Therefore, it is preferred that (ZnO+Gd2O3+Y2O3) / CaO is below 5.0, and it is more preferred that (ZnO+Gd2O3+Y2O3) / CaO is below 4.0. Furthermore, by controlling (ZnO+Gd2O3+Y2O3) / CaO within the range of 0.2 to 3.0, the bubble degree and hardness of the glass can be further optimized. Therefore, it is further preferred that (ZnO+Gd2O3+Y2O3) / CaO is 0.2 to 3.0, and it is further preferred that (ZnO+Gd2O3+Y2O3) / CaO is 0.5 to 2.0.
[0042] TiO2 can increase the refractive index and dispersion of glass and improve the resistance to devitrification of glass, but too high a content will greatly reduce the dispersion coefficient and increase the tendency of crystallization, and even cause obvious coloration of the glass. Therefore, the TiO2 content is limited to 5-20%, preferably 8-18%, and more preferably 11-16%.
[0043] In some embodiments, the ratio TiO2 / (La2O3+ZnO) between TiO2 and the total content La2O3 and ZnO is controlled within the range of 0.1 to 0.6, which can prevent the light transmittance of the glass from decreasing while lowering the transition temperature of the glass. Therefore, it is preferred that TiO2 / (La2O3+ZnO) is 0.1 to 0.6, and it is more preferred that TiO2 / (La2O3+ZnO) is 0.1 to 0.6, and it is more preferred that TiO2 / (La2O3+ZnO) is 0.15 to 0.55. Furthermore, controlling TiO2 / (La2O3+ZnO) within the range of 0.2 to 0.5 can further increase the Young's modulus of the glass and optimize the wear resistance. Therefore, it is further preferred that TiO2 / (La2O3+ZnO) is 0.2 to 0.5, and it is further preferred that TiO2 / (La2O3+ZnO) is 0.25 to 0.45.
[0044] In some embodiments, the ratio of TiO2 to BaO is controlled within the range of 0.3 to 3.0, which can increase the Young's modulus of the glass and prevent the increase of the thermal expansion coefficient. Therefore, it is preferred that TiO2 / BaO is 0.3 to 3.0, and it is more preferred that TiO2 / BaO is 0.4 to 2.0. Furthermore, controlling TiO2 / BaO within the range of 0.6 to 1.5 can further improve the hardness and chemical stability of the glass. Therefore, it is further preferred that TiO2 / BaO is 0.6 to 1.5, and it is further preferred that TiO2 / BaO is 0.8 to 1.3.
[0045] Nb2O5 is a high-refractive and high-dispersion component, which can increase the refractive index and devitrification resistance of glass and reduce the thermal expansion coefficient of glass. If the content of Nb2O5 exceeds 12%, the thermal stability and weather resistance of the glass will be reduced, and the light transmittance will decrease. Therefore, the content of Nb2O5 in the present invention is 0-12%, preferably 1-10%, and more preferably 2-7%.
[0046] In some embodiments, the ratio of BaO content to Nb2O5 content, BaO / Nb2O5, is controlled to be above 0.8, which can improve the light transmittance and chemical stability of the glass. Therefore, it is preferred that BaO / Nb2O5 is above 0.8, and it is more preferred that BaO / Nb2O5 is 1.0 to 20.0. Further, controlling BaO / Nb2O5 within the range of 1.5 to 10.0 can further reduce the thermal expansion coefficient and transition temperature of the glass. Therefore, it is further preferred that BaO / Nb2O5 is 1.5 to 10.0, and it is further preferred that BaO / Nb2O5 is 2.0 to 5.0.
[0047] In some embodiments, the ratio La2O3 / (ZnO+Nb2O5) between the content of La2O3 and the total content of ZnO and Nb2O5 ZnO+Nb2O5 is controlled within the range of 2.0 to 15.0, which can increase the bubble degree of the glass and reduce the transition temperature of the glass. Therefore, La2O3 / (ZnO+Nb2O5) is preferably 2.0 to 15.0, and La2O3 / (ZnO+Nb2O5) is more preferably 2.5 to 10.0. Furthermore, controlling La2O3 / (ZnO+Nb2O5) within the range of 3.0 to 8.0 can further optimize the density and abrasiveness of the glass. Therefore, La2O3 / (ZnO+Nb2O5) is further preferably 3.0 to 8.0, and La2O3 / (ZnO+Nb2O5) is further preferably 3.5 to 6.0.
[0048] Ta2O5 has the effect of increasing the refractive index and improving the devitrification resistance of glass, but if its content is too high, the thermal stability of the glass will decrease, the density will increase, and the optical constants will be difficult to control within the desired range; on the other hand, compared with other components, Ta2O5 is very expensive, and its usage should be minimized from the perspective of practicality and cost. Therefore, the content of Ta2O5 in the present invention is limited to 0-5%, preferably 0-3%, and more preferably 0-1%. In some embodiments, it is further preferred that Ta2O5 is not contained.
[0049] Alkali metal oxide Rn2O (Rn2O is one or more of Li2O, Na2O, and K2O) can reduce the transition temperature of glass, adjust the optical constants and high-temperature viscosity of glass, and improve the melting property of glass. However, when its content is high, the devitrification resistance and chemical stability of glass are reduced, and the refractive index is reduced. Therefore, the content of Rn2O in the present invention is 0 to 8%, preferably 0 to 4%, and more preferably 0 to 2%. In some embodiments, it is further preferred that Rn2O is not contained.
[0050] WO3 can improve the refractive index and mechanical strength of glass. If the content of WO3 exceeds 5%, the thermal stability of glass decreases and the resistance to devitrification decreases. Therefore, the content of WO3 is upper limited to 5%, preferably upper limited to 3%, and more preferably upper limited to 1%. In some embodiments, it is further preferred not to contain WO3.
[0051] Al2O3 can improve the chemical stability of glass, but when its content exceeds 5%, the meltability and light transmittance of glass deteriorate. Therefore, the content of Al2O3 in the present invention is 0-5%, preferably 0-3%, and more preferably 0-1%. In some embodiments, it is further preferred that Al2O3 is not contained.
[0052] GeO2 has the effect of increasing the refractive index and resistance to devitrification, but if its content is too high, the chemical stability of the glass will decrease; on the other hand, compared with other components, GeO2 is very expensive, and its usage should be minimized from the perspective of practicality and cost. Therefore, the content of GeO2 in the present invention is limited to 0-5%, preferably 0-3%, more preferably 0-1%, and it is further preferred that GeO2 is not contained.
[0053] In the present invention, by containing 0-1% of one or more components of Sb2O3, SnO, SnO2, and CeO2 as a clarifier, the clarification effect of the glass can be improved, and the bubble degree of the glass can be improved. The content of the clarifier is preferably 0-0.5%, and the content of the clarifier is more preferably 0-0.2%. Since the component types and contents of the optical glass of the present invention are reasonably designed and its bubble degree is excellent, it is further preferred in some embodiments that no clarifier is contained. When the Sb2O3 content exceeds 1%, the glass tends to have reduced clarification performance. At the same time, due to its strong oxidizing effect, it promotes the corrosion of platinum or platinum alloy vessels for melting glass and the deterioration of the molding mold. Therefore, the present invention preferably has a Sb2O3 content of 0-1%, more preferably 0-0.5%, further preferably 0-0.2%, and further preferably no Sb2O3. SnO and SnO2 can also be used as clarifiers, but when their content exceeds 1%, the glass tends to color more, or when the glass is heated, softened, and molded again, Sn will become the starting point for nucleation, resulting in a tendency to devitrification. Therefore, the content of SnO2 in the present invention is preferably 0-1%, more preferably 0-0.5%, further preferably 0-0.2%, and further preferably does not contain SnO2; the content of SnO is preferably 0-1%, more preferably 0-0.5%, further preferably 0-0.2%, and further preferably does not contain SnO. The role and content ratio of CeO2 are consistent with SnO2, and its content is preferably 0-1%, more preferably 0-0.5%, further preferably 0-0.2%, and further preferably does not contain CeO2.
[0054] <Components that should not be contained>
[0055] In the glass of the present invention, even if oxides of transition metals such as V, Cr, Mn, Fe, Co, Ni, Cu, Ag and Mo are contained alone or in combination in small amounts, the glass will be colored and absorption will occur at specific wavelengths in the visible light region, thereby weakening the property of the present invention of improving the visible light transmittance. Therefore, it is preferably substantially free of oxides of transition metals such as V, Cr, Mn, Fe, Co, Ni, Cu, Ag and Mo, especially for optical glasses that require transmittance at wavelengths in the visible light region.
[0056] The oxides of Th, Cd, Tl, Os, Be and Se have a tendency to be controlled in recent years as harmful chemical substances, and environmental protection measures are necessary not only in the manufacturing process of glass, but also in the processing process and the disposal after productization. Therefore, in the case of paying attention to the impact on the environment, it is preferred that they are not actually contained except for being inevitably mixed in. Thus, the optical glass does not actually contain substances that pollute the environment. Therefore, even if special environmental countermeasures are not taken, the optical glass of the present invention can be manufactured, processed and discarded.
[0057] In order to achieve environmental friendliness, the optical glass of the present invention preferably does not contain As2O3 and PbO.
[0058] The "does not contain" and "0%" recorded in this article mean that the compound, molecule or element is not intentionally added as a raw material to the optical glass of the present invention; however, as raw materials and / or equipment for producing optical glass, there will be certain impurities or components that are not intentionally added, which will be contained in a small amount or trace amount in the final optical glass, and this situation is also within the scope of protection of the patent of this invention.
[0059] Next, the properties of the optical glass of the present invention will be described.
[0060] <Refractive Index and Abbe Number>
[0061] The refractive index of optical glass (n d ) and the Abbe number (ν d ) Tested according to the method specified in GB / T 7962.1-2010.
[0062] In some embodiments, the refractive index (n d ) has a lower limit of 1.87, a preferred lower limit of 1.88, and a more preferred lower limit of 1.89.
[0063] In some embodiments, the refractive index (n d ) has an upper limit of 1.93, a preferred upper limit of 1.92, and a more preferred upper limit of 1.91.
[0064] In some embodiments, the Abbe number (ν d ) has a lower limit of 28, a preferred lower limit of 29, and a more preferred lower limit of 30.
[0065] In some embodiments, the Abbe number (ν d ) has an upper limit of 35, a preferred upper limit of 34, and a more preferred upper limit of 33.
[0066] <Coefficient of Thermal Expansion>
[0067] Thermal expansion coefficient of optical glass (α -30 / 70℃ )The data at -30~70℃ were tested according to the method specified in GB / T7962.16-2010.
[0068] In some embodiments, the thermal expansion coefficient (α) of the optical glass of the present invention is -30 / 70℃ ) is 95×10 -7 / K or less, preferably 90×10 -7 / K or less, more preferably 85×10 -7 / K or less, more preferably 80×10-7 / K or less.
[0069] <Water resistance stability>
[0070] Water resistance stability of optical glass (D W )(Powder method) Tested according to the method specified in GB / T 17129.
[0071] In some embodiments, the water resistance stability (D W ) is 2 or more, preferably 1.
[0072] <Color>
[0073] The short-wave transmission spectrum characteristics of the glass of the present invention are expressed by the coloration degree (λ 70 and λ5). 70 It refers to the wavelength when the glass transmittance reaches 70%. 70 The measurement is to use a glass with a thickness of 10±0.1mm and two opposite planes parallel to each other and optically polished, and measure the spectral transmittance in the wavelength range from 280nm to 700nm and the wavelength at which the transmittance is 70%. The so-called spectral transmittance or transmittance is the wavelength at which the incident intensity I is perpendicular to the above surface of the glass. in Light of intensity I passes through the glass and emerges from a plane out The light of the case through I out / I in The amount expressed by λ also includes the transmittance of the surface reflection loss on the above surfaces of the glass. The higher the refractive index of the glass, the greater the surface reflection loss. Therefore, in high refractive index glass, λ 70 A small value of means that the glass itself is less colored and has a high light transmittance.
[0074] In some embodiments, the λ of the optical glass of the present invention is 70 420nm or less, preferably λ 70 415nm or less, preferably λ 70 Below 410nm.
[0075] In some embodiments, the λ5 of the optical glass of the present invention is 380 nm or less, preferably λ5 is 375 nm or less, and more preferably λ5 is 370 nm or less.
[0076] <Weather resistance>
[0077] The test method for weather resistance (CR) of optical glass is as follows: place the sample in a test chamber with a saturated water vapor environment of 90% relative humidity, alternately cycle at 40-50°C every 1h, and cycle for 15 cycles. The weather resistance category is divided according to the change in turbidity before and after the sample is placed. The weather resistance classification is shown in Table 1:
[0078] Table 1.
[0079]
[0080] In some embodiments, the weather resistance (CR) of the optical glass of the present invention is Class 2 or higher, preferably Class 1.
[0081] <Knoop hardness>
[0082] Knoop hardness of optical glass (H K ) Test according to the test method specified in GB / T7962.18-2010.
[0083] In some embodiments, the Knoop hardness (H K ) is 580×10 7 Pa or more, preferably 590×10 7 Pa or more, more preferably 600×10 7 Pa or more, more preferably 605×10 7 Pa or above.
[0084] <Young's modulus>
[0085] Young's modulus (E) is calculated using the following formula using ultrasonic testing of the longitudinal wave velocity and transverse wave velocity.
[0086]
[0087]
[0088] Where:
[0089] E is Young's modulus, Pa;
[0090] G is the shear modulus, Pa;
[0091] V T is the shear wave velocity, m / s;
[0092] V S is the longitudinal wave velocity, m / s;
[0093] ρ is the glass density, g / cm 3 .
[0094] In some embodiments, the Young's modulus (E) of the optical glass of the present invention is 10000×10 7 Pa or more, preferably 10500×10 7 Pa or more, more preferably 11000×10 7 Pa or above.
[0095] <Bubble Degree>
[0096] The bubble degree of optical glass is tested according to the method specified in GB / T7962.8-2010.
[0097] In some embodiments, the bubble degree of the optical glass of the present invention is above grade A, preferably above grade A0, and more preferably above grade A1. 00 class.
[0098] <density>
[0099] The density (ρ) of optical glass is tested according to the method specified in GB / T7962.20-2010.
[0100] In some embodiments, the density (ρ) of the optical glass of the present invention is 4.90 g / cm 3 Below, preferably 4.80g / cm 3 Below, more preferably 4.70g / cm 3 Below, more preferably 4.60 g / cm 3 the following.
[0101] <Abrasion>
[0102] Abrasiveness of optical glass (F A ) refers to the value obtained by multiplying the ratio of the wear volume of the sample to the wear volume (volume) of the standard sample (H-K9 glass) under exactly the same conditions by 100, and is expressed by the following formula:
[0103]
[0104] Where:
[0105] V—volume wear of the sample being tested;
[0106] V0—Volume loss of standard sample;
[0107] W—mass wear loss of the sample being tested;
[0108] W0—standard sample mass wear;
[0109] ρ—density of the sample being tested;
[0110] ρ0—standard sample density.
[0111] In some embodiments, the abrasiveness (F A ) has a lower limit of 125, a preferred lower limit of 130, and a more preferred lower limit of 135.
[0112] In some embodiments, the abrasiveness (F A ) has an upper limit of 165, a preferred upper limit of 160, and a more preferred upper limit of 155.
[0113] <Transition Temperature>
[0114] Transition temperature of optical glass (T g ) The test shall be carried out in accordance with the method specified in GB / T7962.16-2010.
[0115] In some embodiments, the transition temperature (T g ) is 700°C or lower, preferably 690°C or lower, more preferably 680°C or lower, and further preferably 678°C or lower.
[0116] [Method for producing optical glass]
[0117] The manufacturing method of the optical glass of the present invention is as follows: the glass of the present invention is produced using conventional raw materials and processes, including but not limited to using oxides, hydroxides, complex salts (such as carbonates, nitrates, sulfates, etc.), boric acid, etc. as raw materials, and after mixing according to conventional methods, the prepared furnace materials are put into a melting furnace (such as platinum or platinum alloy crucible) at 1200-1500°C for melting, and after clarification and homogenization, a homogeneous molten glass without bubbles and undissolved substances is obtained, and the molten glass is cast in a mold and annealed. Those skilled in the art can appropriately select raw materials, process methods and process parameters according to actual needs.
[0118] [Glass preforms and optical components]
[0119] The prepared optical glass can be used to make a glass preform by means of direct drop molding, grinding, or compression molding such as hot press molding. That is, the molten optical glass can be directly precision drop molded into a glass precision preform, or the glass preform can be made by mechanical processing such as grinding and grinding, or the preform for compression molding made of the optical glass can be made by hot press molding and then grinding. It should be noted that the means for preparing the glass preform are not limited to the above means.
[0120] As described above, the optical glass of the present invention is useful for various optical elements and optical designs, and it is particularly preferred to form a preform from the optical glass of the present invention and use the preform to perform re-hot pressing, precision stamping, etc. to produce optical elements such as lenses and prisms.
[0121] The glass preform and optical element of the present invention are both formed of the optical glass of the present invention. The glass preform of the present invention has the excellent properties of optical glass; the optical element of the present invention has the excellent properties of optical glass, and can provide various optical elements such as lenses and prisms with high optical value.
[0122] Examples of the lens include various lenses having spherical or aspherical lens surfaces, such as a concave meniscus lens, a convex meniscus lens, a biconvex lens, a biconcave lens, a plano-convex lens, and a plano-concave lens.
[0123] [Optical instruments]
[0124] The optical element formed by the optical glass of the present invention can be used to manufacture optical instruments such as photographic equipment, video equipment, projection equipment, display equipment, vehicle-mounted equipment and monitoring equipment.
[0125] Example
[0126] <Optical Glass Example>
[0127] In order to further clearly illustrate and describe the technical solution of the present invention, the following non-limiting examples are provided.
[0128] This embodiment adopts the above optical glass manufacturing method to obtain optical glasses having the compositions shown in Tables 2 to 4. In addition, the properties of each glass are measured by the testing method described in the present invention, and the measurement results are shown in Tables 2 to 4.
[0129] Table 2.
[0130]
[0131]
[0132] Table 3.
[0133]
[0134]
[0135] Table 4.
[0136]
[0137]
[0138] <Glass Preform Example>
[0139] The glass obtained from optical glass examples 1 to 24# is used, for example, by grinding processing, or by molding methods such as hot pressing, precision stamping, etc., to make preforms of various lenses, prisms, etc., such as concave meniscus lenses, convex meniscus lenses, biconvex lenses, biconcave lenses, plano-convex lenses, and plano-concave lenses.
[0140] <Optical Element Embodiment>
[0141] The preforms obtained in the above-mentioned glass preform embodiments are annealed to reduce the internal stress of the glass and fine-tune the refractive index so that the optical properties such as the refractive index reach the desired values.
[0142] Next, each preform is ground and polished to produce various lenses and prisms such as concave meniscus lenses, convex meniscus lenses, biconvex lenses, biconcave lenses, plano-convex lenses, and plano-concave lenses. The surface of the obtained optical element may be coated with an anti-reflection film.
[0143] <Optical Instrument Embodiment>
[0144] The optical element obtained by the above-mentioned optical element embodiment is optically designed to form an optical component or optical assembly by using one or more optical elements, and can be used in, for example, imaging equipment, sensors, microscopes, medical technology, digital projection, communications, optical communication technology / information transmission, optics / lighting in the automotive field, lithography technology, excimer lasers, wafers, computer chips, and integrated circuits and electronic devices including such circuits and chips.
Claims
1. Optical glass, characterized in that: Its components, expressed in weight percentage, include: SiO2: 1-12%; B2O3: 5-20%; La2O3: 25-50%; ZrO2: 1-12%; TiO2: 5-20%; BaO: 5-20%, wherein TiO2 / BaO is 0.3-3.
0.
2. The optical glass according to claim 1, characterized in that: Its components are expressed in weight percentage and further contain: SrO: 0-10%; and / or CaO: 0-12%; and / or MgO: 0-10%; and / or Y2O3: 0-8%; and / or Gd2O3: 0-8%; and / or Yb2O3: 0-5%; and / or Nb2O5: 0-12%; and / or ZnO: 0-10%; and / or Rn2O: 0-8%; and / or GeO2: 0-5%; and / or WO3: 0-5%; and / or Ta2O5: 0-5%; and / or Al2O3: 0-5%; and / or clarifier: 0-1%, wherein the Rn2O is one or more of Li2O, Na2O, and K2O, and the clarifier is one or more of Sb2O3, SnO, SnO2, and CeO2.
3. Optical glass, characterized in that: Contains SiO2, B2O3, La2O3, ZrO2, TiO2 and BaO, wherein the components are expressed in weight percentage, wherein TiO2 / BaO is 0.3 to 3.0, and the refractive index of the optical glass is n d is 1.87~1.93, Abbe number v d The thermal expansion coefficient is 28 to 35. -30 / 70℃ 95×10 -7 / K or less, Young's modulus E is 10000×10 7 Pa or above.
4. The optical glass according to claim 3, characterized in that: Its components, expressed in weight percentage, contain: SiO2: 1-12%; and / or B2O3: 5-20%; and / or La2O3: 25-50%; and / or ZrO2: 1-12%; and / or TiO2: 5-20%; and / or BaO: 5-20%; and / or SrO: 0-10%; and / or CaO: 0-12%; and / or MgO: 0-10%; and / or Y2O3: 0-8%; and / or Gd2O3: 0-8%; and / or Yb2O3 : 0-5%; and / or Nb2O5: 0-12%; and / or ZnO: 0-10%; and / or Rn2O: 0-8%; and / or GeO2: 0-5%; and / or WO3: 0-5%; and / or Ta2O5: 0-5%; and / or Al2O3: 0-5%; and / or clarifier: 0-1%, wherein Rn2O is one or more of Li2O, Na2O, and K2O, and the clarifier is one or more of Sb2O3, SnO, SnO2, and CeO2.
5. The optical glass according to any one of claims 1 to 4, characterized in that: The components are expressed in weight percentage, wherein: TiO2 / BaO is 0.4-2.0, preferably TiO2 / BaO is 0.6-1.5, more preferably TiO2 / BaO is 0.8-1.3; and / or SiO2 / (CaO+BaO) is 0.05-1.5, preferably SiO2 / (CaO+BaO) is 0.1-1.0, more preferably SiO2 / (CaO+BaO) is 0.2-0.85, further preferably SiO2 / (CaO+BaO) is 0.35-0.75; and / or BaO / Nb2O 5 is above 0.8, preferably BaO / Nb2O5 is 1.0~20.0, more preferably BaO / Nb2O5 is 1.5~10.0, and further preferably BaO / Nb2O5 is 2.0~5.0; and / or TiO2 / (La2O3+ZnO) is 0.1~0.6, preferably TiO2 / (La2O3+ZnO) is 0.15~0.55, more preferably TiO2 / (La2O3+ZnO) is 0.2~0.5, and further preferably TiO2 / (La2O3+ZnO) is 0.25~0.
45.
6. The optical glass according to any one of claims 1 to 4, characterized in that: Its components are expressed in weight percentage, wherein: (CaO + ZnO) / BaO is 0.1 to 3.0, preferably (CaO + ZnO) / BaO is 0.2 to 2.0, more preferably (CaO + ZnO) / BaO is 0.3 to 1.0, and further preferably (CaO + ZnO) / BaO is 0.3 to 0.8; and / or La2O3 / (ZnO + Nb2O5) is 2.0 to 15.0, preferably La2O3 / (ZnO + Nb2O5) is 2.5 to 10.0, more preferably La2O3 / (ZnO + Nb2O5) is 3.0 to 8.0, and further preferably La2O3 / (ZnO + Nb2O5) is 3.5 to 6.0; and / or (ZnO + Gd2O3 + Y2O3) / CaO is 5.0 or less, preferably ( (ZnO+Gd2O3+Y2O3) / CaO is less than 4.0, more preferably (ZnO+Gd2O3+Y2O3) / CaO is 0.2~3.0, and further preferably (ZnO+Gd2O3+Y2O3) / CaO is 0.5~2.0; and / or CaO / (SiO2+ZrO2) is 0.02~1.0, preferably CaO / (SiO2+ZrO2) is 0.05~0.8, more preferably CaO / (SiO2+ZrO2) is 0.1~0.6, and further preferably CaO / (SiO2+ZrO2) is 0.1~0.5; and / or RO: 6~35%, preferably RO: 10~25%, more preferably RO: 11~20%, wherein RO is the total content of MgO, CaO, SrO and BaO.
7. The optical glass according to any one of claims 1 to 4, characterized in that: Its components are expressed in weight percentage, wherein: SiO2: 3-12%, preferably SiO2: 5-10%; and / or B2O3: 8-17%, preferably B2O3: 10-15%; and / or La2O3: 31-45%, preferably La2O3: 34-40%; and / or ZrO2: 2-10%, preferably ZrO2: 3-8%; and / or TiO2: 8-18%, preferably TiO2: 11-16%; and / or BaO: 8-18%, preferably BaO: 11-1 6%; and / or SrO: 0-5%, preferably SrO: 0-2%, more preferably no SrO; and / or CaO: 1-10%, preferably CaO: 2-8%; and / or MgO: 0-5%, preferably MgO: 0-2%, more preferably no MgO; and / or Y2O3: 0-4%, preferably Y2O3: 0-2%, more preferably no Y2O3; and / or Gd2O3: 0-4%, preferably Gd2O3: 0-2%, more preferably no Gd2O3; and / or Yb2O3 :0~3%, preferably Yb2O3: 0~1%, more preferably no Yb2O3; and / or Nb2O5: 1~10%, preferably Nb2O5: 2~7%; and / or ZnO: 1~8%, preferably ZnO: 2~7%; and / or Rn2O: 0~4%, preferably Rn2O: 0~2%, more preferably no Rn2O; and / or GeO2: 0~3%, preferably GeO2: 0~1%, more preferably no GeO2; and / or WO3: 0~3%, preferably WO3: 0~1 %, more preferably no WO3; and / or Ta2O5: 0-3%, preferably Ta2O5: 0-1%, more preferably no Ta2O5; and / or Al2O3: 0-3%, preferably Al2O3: 0-1%, more preferably no Al2O3; and / or clarifier: 0-0.5%, preferably clarifier: 0-0.2%, the Rn2O is one or more of Li2O, Na2O, K2O, and the clarifier is one or more of Sb2O3, SnO, SnO2, and CeO2.
8. The optical glass according to any one of claims 1 to 4, characterized in that: The refractive index n of the optical glass d is 1.87 to 1.93, preferably 1.88 to 1.92, more preferably 1.89 to 1.91, and the Abbe number v d It is 28-35, preferably 29-34, and more preferably 30-33.
9. The optical glass according to any one of claims 1 to 4, characterized in that: The thermal expansion coefficient of the optical glass is α -30 / 70℃ 95×10 -7 / K or less, preferably 90×10 -7 / K or less, more preferably 85×10 -7 / K or less, more preferably 80×10 -7 / K or less; and / or water resistance stability D W Two or more types, preferably one type; and / or 70 420nm or less, preferably λ 70 415nm or less, preferably λ 70 410nm or less; and / or λ5 is 380nm or less, preferably λ5 is 375nm or less, more preferably λ5 is 370nm or less; and / or weather resistance CR is 2 or more, preferably 1; and / or Knoop hardness H K 580×10 7 Pa or more, preferably 590×10 7 Pa or more, more preferably 600×10 7 Pa or more, more preferably 605×10 7 Pa or more; and / or Young's modulus E is 10000×10 7 Pa or more, preferably 10500×10 7 Pa or more, more preferably 11000×10 7 Pa or more; and / or the bubble degree is A grade or more, preferably A0 grade or more, more preferably A 00 Grade; and / or density ρ is 4.90g / cm 3 Below, preferably 4.80g / cm 3 Below, more preferably 4.70g / cm 3 Below, more preferably 4.60 g / cm 3 Below; and / or wear degree F A 125 to 165, preferably 130 to 160, more preferably 135 to 155; and / or transition temperature T g The temperature is 700°C or lower, preferably 690°C or lower, more preferably 680°C or lower, and further preferably 678°C or lower.
10. A glass preform, characterized in that: Made of the optical glass described in any one of claims 1 to 9.
11. An optical element, characterized in that The optical glass is made of the optical glass described in any one of claims 1 to 9, or the glass preform described in claim 10.
12. An optical instrument, characterized in that Contains the optical glass according to any one of claims 1 to 9, and / or contains the optical element according to claim 11.
Citation Information
Patent Citations
Optical glass, glass gob for press-molding, optical part and process for producing optical part
CN102775060A
Optical glass
CN110510869A
High-refraction and high-dispersion optical glass
CN113582537A
Optical glass and optical element
CN113666635A
Optical glass, glass preform, optical element and optical instrument
CN113735436A
Cited By
Optical glass with high refractive index, preparation method thereof and optical element