Impregnating compound coated on surface of glass fiber for LFT process and preparation method of impregnating compound
By using double coupling agents and cyclic acid anhydride compatibilizers combined with non-ionic emulsion sizing agents, the problems of fluidity and hairiness of glass fiber yarns are solved, mechanical properties and temperature resistance are improved, and production costs are reduced. , achieving better material properties and flowability.
Patent Information
- Application Number
- CN202411168183.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-23
- Publication Date
- 2024-10-15
AI Technical Summary
Existing glass fiber sizing agents lead to poor yarn fluidity and fiber opening during the production process, and a large amount of hairiness, which affects the quality and appearance of the product, and the cost is high.
Using double coupling agent and cyclic acid anhydride compatibilizer, combined with non-ionic emulsion, a wetting agent including glacial acetic acid, coupling agent, compatibilizer, lubricant and emulsion is prepared, which is combined and uniformly dispersed through physical and chemical combination Components to improve the surface properties of glass fiber, reduce the static friction coefficient and improve fluidity and adhesion.
It significantly improves the mechanical properties, temperature resistance and hydrophobicity of glass fiber, reduces hairiness and production costs, and improves the strength and stability of the material.
Smart Images

Figure BDA0005008429440000071 
Figure BDA0005008429440000081
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of sizing agent preparation, and specifically relates to a sizing agent coated on the surface of glass fiber for LFT process and a preparation method thereof. Background Art
[0002] In the field of long glass fiber reinforced polypropylene (LFT-PP), the pelletized LFT process (LFT-G) is currently a very important production process. It has the characteristics of relatively simple production equipment, concise and flexible process, excellent performance of parts, etc., and is widely used. In practical applications, the LFT-G process can be divided into melt impregnation method and cable coating method according to the different pellet production methods. Among them, the cable coating method is fast, efficient, low cost, and suitable for large-scale production, but the capital cost is large, the equipment investment is high, and the pellets after coating need secondary impregnation and dispersion.
[0003] Wetting means that when the liquid phase contacts the solid phase, the liquid phase can continue to expand along the surface of the solid phase and melt into each other. In the process of glass fiber drawing, it is necessary to coat the glass fiber surface with a special surface treatment agent with a multiphase structure based on an organic emulsion, which can effectively lubricate the glass fiber surface, integrate hundreds to thousands of glass fiber filaments into a bundle, change the surface state of the glass fiber surface, meet the requirements of the processing performance of the glass fiber raw yarn in the subsequent process, and promote the combination of glass fiber and reinforced polymer in composite materials. These organic coatings are collectively called glass fiber wetting agents, or wetting agents for short.
[0004] However, the currently prepared wetting agents, when used in the production of glass fiber, often lead to poor fluidity and fiber opening of the glass fiber yarn, and cannot effectively suppress the amount of hairiness in the production process, which can easily cause problems such as material shortage and uneven distribution of glass fiber in the products. It can also cause the glass fiber texture on the surface of the product to affect the appearance and comfort, and even cause quality problems such as blistering and breakage after boiling. Summary of the invention
[0005] In view of the above-mentioned deficiencies in the prior art, the present invention provides a wetting agent coated on the surface of glass fiber for LFT process and a preparation method thereof, which can effectively reduce the fluff of glass fiber, improve its mechanical properties and temperature resistance, and greatly reduce the production cost.
[0006] To achieve the above purpose, the technical solution adopted by the present invention to solve the technical problem is:
[0007] A sizing agent applied to the surface of glass fiber for LFT process, comprising the following components in weight percentage:
[0008] Glacial acetic acid 0.02-0.05%, coupling agent A 0.2-0.5%, coupling agent B 0.5-1.5%, compatibilizer 0.2-0.8%, lubricant 0.1-0.6%, brightener 0.2-0.8%, emulsion D 4-8%, emulsion F 2-7%, and the balance is deionized water.
[0009] Further, the following components are included in weight percentage:
[0010] Glacial acetic acid 0.02-0.05%, coupling agent A 0.2-0.4%, coupling agent B 0.6-1.2%, compatibilizer 0.21-0.55%, lubricant 0.2-0.55%, brightener 0.2-0.8%, emulsion D 4.3-7%, emulsion F 2-6.2%, and the balance is deionized water.
[0011] Furthermore, the coupling agent A is γ-aminopropyltriethoxysilane.
[0012] Furthermore, the coupling agent B is ureidepropyltriethoxysilane.
[0013] Furthermore, the compatibilizer is a cyclic anhydride type reactive compatibilizer, which is a commercially available product, such as ABS-g-MAH, PE-g-MAH or PP-g-MAH.
[0014] Furthermore, the lubricant is fatty acid methyl ester polyoxyethylene ether.
[0015] Furthermore, emulsion D and emulsion F are non-ionic emulsions.
[0016] Furthermore, the nonionic emulsion is acrylic emulsion, modified polypropylene emulsion or polyethylene wax emulsion.
[0017] The method for preparing the above-mentioned impregnating agent is characterized by comprising the following steps:
[0018] (1) Add coupling agent A to water and stir evenly, and adjust its pH value to 6-7;
[0019] (2) Add coupling agent B to water and stir, then add compatibilizer and stir evenly;
[0020] (3) Add the product obtained in step (2) and the lubricant to the product obtained in step (1), stir, then add emulsion D and emulsion F, continue stirring, and finally add the brightener and stir to obtain the wetting agent.
[0021] Beneficial effects of the present invention:
[0022] 1. The present invention uses a double coupling agent when preparing the sizing agent, wherein coupling agent A can be firmly combined with the glass fiber through physical and chemical bonding, while coupling agent B can be firmly combined with the polypropylene resin (PP) in the glass fiber. By combining the two coupling agents in the present invention, the surface of the glass fiber can be changed from hydrophilic to lipophilic, thereby achieving the purpose of close bonding with the polymer, thereby significantly improving the strength, adhesion, electrical properties, hydrophobicity, anti-aging and other properties of the material.
[0023] 2. The present invention uses a cyclic anhydride type reactive compatibilizer as a raw material, which can make the components dispersed evenly, improve the performance of the two-phase interface in the polymer system, increase the adhesion between the phases, and enhance its stability.
[0024] 3. The present invention uses fatty acid methyl ester polyoxyethylene ether as a lubricant, which can reduce the static friction coefficient of glass fiber, reduce the generation of hairiness during glass fiber processing, and effectively improve the fluidity, dispersibility and bulk density of glass fiber chopped yarn.
[0025] 4. The emulsion D and emulsion F used in the present invention have different molecular weights: they are non-toxic, tasteless, non-corrosive non-ionic emulsions, resistant to acid, alkali, hard water, highly water-soluble, stable emulsions, no stratification, no demulsification, no agglomeration when diluted with water in any proportion, long shelf life, high solid content, and good dispersibility. They can effectively enhance the smoothness and good hand feel of the glass fiber coating; they can also increase the gloss of the coating and improve the stain resistance; in addition, they can further enhance the waterproof, abrasion, scratch / scratch resistance, high temperature adhesion resistance and other properties. DETAILED DESCRIPTION
[0026] The specific implementation modes of the present invention are described below so that those skilled in the art can understand the present invention. However, it should be clear that the present invention is not limited to the scope of the specific implementation modes. For those of ordinary skill in the art, as long as various changes are within the spirit and scope of the present invention as defined and determined by the attached claims, these changes are obvious, and all inventions and creations utilizing the concept of the present invention are protected.
[0027] Example 1
[0028] A sizing agent applied to the surface of glass fiber for LFT process, comprising the following components in weight percentage:
[0029] Glacial acetic acid 0.02%, γ-aminopropyl triethoxysilane 0.5%, ureide propyl triethoxysilane 0.5%, PE-g-MAH 0.8%, fatty acid methyl ester polyoxyethylene ether 0.6%, brightener 0.2%, polypropylene wax emulsion 4%, polyethylene wax emulsion 7%, and the balance is deionized water.
[0030] The preparation method of the above-mentioned impregnation agent is as follows:
[0031] (1) Add 35-45% of the total amount of room temperature deionized water to the cleaned preparation tank, and adjust the pH to 6-7 with glacial acetic acid;
[0032] (2) Add γ-aminopropyltriethoxysilane into the preparation tank and stir evenly at a speed of 60 to 70 r / min;
[0033] (3) Add ureide propyl triethoxysilane into water, stir for 30 min, and then add compatibilizer PE-g-MAH;
[0034] (4) Place the lubricant fatty acid methyl ester polyoxyethylene ether in a pretreatment container, turn on the electric stirrer and slowly add 30-40°C deionized water. After observing that the viscosity of the solution changes from thin to thick, stop adding water; continue stirring for 5 minutes until it is uniform, then slowly add deionized water to dilute, stir evenly, and then pour into the preparation tank and dilute it according to 20 times the treatment volume;
[0035] (5) adding the product after treatment in step (3) and step (4) to the preparation tank of step (2), stirring for 10 minutes, then adding emulsion D, continuing to stir for 5 minutes, and then adding emulsion F and stirring evenly;
[0036] (6) Dilute the brightener with more than twice the amount of water in a special plastic bucket and pour it into the preparation tank treated in step (5), then add water to 95% of the total preparation amount and stir to obtain the wetting agent.
[0037] Example 2
[0038] A sizing agent applied to the surface of glass fiber for LFT process, comprising the following components in weight percentage:
[0039] Glacial acetic acid 0.03%, γ-aminopropyltriethoxysilane 0.32%, ureidepropyltriethoxysilane 0.81%, PE-g-MAH 0.42%, fatty acid methyl ester polyoxyethylene ether 0.49%, brightener 0.43%, polyethylene wax emulsion 5.5%, polypropylene wax emulsion 3.7%, and the balance is deionized water.
[0040] The preparation method of the above-mentioned impregnation agent is as follows:
[0041] (1) Add 35-45% of the total amount of room temperature deionized water to the cleaned preparation tank, and adjust the pH to 6-7 with glacial acetic acid;
[0042] (2) Add γ-aminopropyltriethoxysilane into the preparation tank and stir evenly at a speed of 60 to 70 r / min;
[0043] (3) Add ureide propyl triethoxysilane into water, stir for 30 min, and then add compatibilizer PE-g-MAH;
[0044] (4) Place the lubricant fatty acid methyl ester polyoxyethylene ether in a pretreatment container, turn on the electric stirrer and slowly add 30-40°C deionized water. After observing that the viscosity of the solution changes from thin to thick, stop adding water; continue stirring for 5 minutes until it is uniform, then slowly add deionized water to dilute, stir evenly, and then pour into the preparation tank and dilute it according to 20 times the treatment volume;
[0045] (5) adding the product after treatment in step (3) and step (4) to the preparation tank of step (2), stirring for 10 minutes, then adding emulsion D, continuing to stir for 5 minutes, and then adding emulsion F and stirring evenly;
[0046] (6) Dilute the brightener with more than twice the amount of water in a special plastic bucket and pour it into the preparation tank treated in step (5), then add water to 95% of the total preparation amount and stir to obtain the wetting agent.
[0047] Example 3
[0048] A sizing agent applied to the surface of glass fiber for LFT process, comprising the following components in weight percentage:
[0049] Glacial acetic acid 0.03%, γ-aminopropyltriethoxysilane 0.26%, ureidepropyltriethoxysilane 0.79%, PE-g-MAH 0.42%, fatty acid methyl ester polyoxyethylene ether 0.56%, brightener 0.49%, polypropylene wax emulsion 3.9%, acrylic emulsion 4.8%, and the balance is deionized water.
[0050] The preparation method of the above-mentioned impregnation agent is as follows:
[0051] (1) Add 35-45% of the total amount of room temperature deionized water to the cleaned preparation tank, and adjust the pH to 6-7 with glacial acetic acid;
[0052] (2) Add γ-aminopropyltriethoxysilane into the preparation tank and stir evenly at a speed of 60 to 70 r / min;
[0053] (3) Add ureide propyl triethoxysilane into water, stir for 30 min, and then add compatibilizer PE-g-MAH;
[0054] (4) Place the lubricant fatty acid methyl ester polyoxyethylene ether in a pretreatment container, turn on the electric stirrer and slowly add 30-40°C deionized water. After observing that the viscosity of the solution changes from thin to thick, stop adding water; continue stirring for 5 minutes until it is uniform, then slowly add deionized water to dilute, stir evenly, and then pour into the preparation tank and dilute it according to 20 times the treatment volume;
[0055] (5) adding the product after treatment in step (3) and step (4) to the preparation tank of step (2), stirring for 10 minutes, then adding emulsion D, continuing to stir for 5 minutes, and then adding emulsion F and stirring evenly;
[0056] (6) Dilute the brightener with more than twice the amount of water in a special plastic bucket and pour it into the preparation tank treated in step (5), then add water to 95% of the total preparation amount and stir to obtain the wetting agent.
[0057] Example 4
[0058] A sizing agent applied to the surface of glass fiber for LFT process, comprising the following components in weight percentage:
[0059] Glacial acetic acid 0.03%, γ-aminopropyltriethoxysilane 0.36%, ureidepropyltriethoxysilane 0.78%, PE-g-MAH 0.42%, fatty acid methyl ester polyoxyethylene ether 0.51%, brightener 0.51%, polyethylene wax emulsion 4.7%, acrylic emulsion 4.2%, and the balance is deionized water.
[0060] The preparation method of the above-mentioned impregnation agent is as follows:
[0061] (1) Add 35-45% of the total amount of room temperature deionized water to the cleaned preparation tank, and adjust the pH to 6-7 with glacial acetic acid;
[0062] (2) Add γ-aminopropyltriethoxysilane into the preparation tank and stir evenly at a speed of 60 to 70 r / min;
[0063] (3) Add ureide propyl triethoxysilane into water, stir for 30 min, and then add compatibilizer PE-g-MAH;
[0064] (4) Place the lubricant fatty acid methyl ester polyoxyethylene ether in a pretreatment container, turn on the electric stirrer and slowly add 30-40°C deionized water. After observing that the viscosity of the solution changes from thin to thick, stop adding water; continue stirring for 5 minutes until it is uniform, then slowly add deionized water to dilute, stir evenly, and then pour into the preparation tank and dilute it according to 20 times the treatment volume;
[0065] (5) adding the product after treatment in step (3) and step (4) to the preparation tank of step (2), stirring for 10 minutes, then adding emulsion D, continuing to stir for 5 minutes, and then adding emulsion F and stirring evenly;
[0066] (6) Dilute the brightener with more than twice the amount of water in a special plastic bucket and pour it into the preparation tank treated in step (5), then add water to 95% of the total preparation amount and stir to obtain the wetting agent.
[0067] Experimental example
[0068] The performance of the glass fiber prepared by Example 2 of the present invention was tested as an experimental group, and Sichuan WeiBo long glass fiber EW758-2400 for reinforced thermoplastics was used as a control. The results are shown in Table 1.
[0069] Table 1 Performance comparison test
[0070]
[0071]
[0072] According to the test results in Table 1, compared with the glass fiber of the control group, the glass fiber prepared by using the sizing agent of the present invention has significantly improved mechanical properties such as tensile strength and bending strength, and at the same time, the heat deformation temperature is also higher, indicating that it has more excellent heat resistance. In addition, the hairiness is also greatly reduced.
[0073] Finally, it should be noted that the above specific implementation methods are only used to illustrate the technical solution of the present invention rather than to limit it. Although the present invention has been described in detail with reference to examples, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the spirit and scope of the technical solution of the present invention, which should be included in the scope of the claims of the present invention.
Claims
1. A sizing agent applied to the surface of glass fiber for LFT process, characterized in that: The composition includes the following weight percentages: Glacial acetic acid 0.02-0.05%, coupling agent A 0.2-0.5%, coupling agent B 0.5-1.5%, compatibilizer 0.2-0.8%, lubricant 0.1-0.6%, brightener 0.2-0.8%, emulsion D 4-8%, emulsion F 2-7%, and the balance is deionized water.
2. The wetting agent according to claim 1, characterized in that The composition includes the following weight percentages: Glacial acetic acid 0.02-0.05%, coupling agent A 0.2-0.4%, coupling agent B 0.6-1.2%, compatibilizer 0.21-0.55%, lubricant 0.2-0.55%, brightener 0.2-0.8%, emulsion D 4.3-7%, emulsion F 2-6.2%, and the balance is deionized water.
3. The wetting agent according to claim 1 or 2, characterized in that The coupling agent A is γ-aminopropyltriethoxysilane.
4. The wetting agent according to claim 1 or 2, characterized in that The coupling agent B is ureide propyl triethoxy silane.
5. The wetting agent according to claim 1 or 2, characterized in that The compatibilizer is a cyclic anhydride type reactive compatibilizer.
6. The wetting agent according to claim 1 or 2, characterized in that The lubricant is fatty acid methyl ester polyoxyethylene ether.
7. The wetting agent according to claim 1 or 2, characterized in that Both emulsion D and emulsion F are non-ionic emulsions.
8. The sizing agent according to claim 7, characterized in that The non-ionic emulsion is acrylic emulsion, modified polypropylene emulsion or polyethylene wax emulsion.
9. The method for preparing the wetting agent according to any one of claims 1 to 8, characterized in that: The following steps are involved: (1) Add water to coupling agent A and stir evenly, and adjust its pH value to 6-7; (2) Add coupling agent B to water and stir, then add compatibilizer and stir evenly; (3) Add the product obtained in step (2) and the lubricant to the product obtained in step (1), stir, then add emulsion D and emulsion F, continue stirring, and finally add the brightener and stir to obtain the wetting agent.
Citation Information
Patent Citations
Reinforced textile type glass fiber treating compound and preparation thereof
CN101439937A
Impregnating compound applied to surface of glass fiber and preparation method of impregnating compound
CN105731829A
Glass fiber sizing agent for electronic-textile
CN108558234A
Impregnating compound for glass fiber direct yarns for LFT process and preparation method thereof
CN111018366A
Glass fiber impregnating compound for LFT and preparation method thereof
CN118479751A