Expansion type efficient anti-seepage composite grouting material
Through the use of expansion-type high-efficiency anti-seepage composite grouting materials, the problems of poor rheological properties and volume shrinkage after hardening of cement grouting materials during construction are solved, better fluidity and bonding strength are achieved, and the anti-seepage effect is significantly improved. Recurrence of leakage problems is avoided.
Patent Information
- Application Number
- CN202410870215.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-01
- Publication Date
- 2024-10-15
AI Technical Summary
The existing cement grouting materials have unsatisfactory rheological properties during construction and are difficult to pour into small cracks. After hardening, the volume shrinks, causing cracks to regenerate. The bonding strength is low and the anti-seepage performance is limited, resulting in the leakage problem not being fundamentally solved.
Expansive high-efficiency anti-seepage composite grouting material is used, and component A and component B are evenly mixed. Component A includes cement, water-absorbing expandable rubber powder, ultra-fine mineral powder, silica fume, fluidizing agent, water retaining agent, slowing agent, etc. Coagulant, defoaming agent, component B is water-soluble epoxy resin and water, Portland cement is compounded with sulfoaluminate cement, water-absorbing swelling rubber powder and water-soluble epoxy resin jointly improve fluidity and bonding strength , to prevent leakage.
It achieves rapid condensation, good fluidity, and micro-expansion volume of the grouting material, enhances the bonding strength with the rock formation, significantly improves the anti-seepage effect, and avoids the occurrence of secondary cracks.
Smart Images

Figure CN118771802A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of cement grouting materials, in particular to an expansion type high-efficiency anti-seepage composite grouting material. Background Art
[0002] The dam bodies of water conservancy and hydropower projects are often built on bedrock with strong bearing capacity. The bedrock is not a whole. After long-term geological changes, the bedrock often contains numerous cracks and holes of varying sizes. Even if the upper dam body is intact, the lower dam foundation will become a key part prone to leakage. Therefore, it is necessary to implement grouting reinforcement on the dam foundation before the construction of the dam body. In addition, the rockfill dam or concrete dam commonly seen in engineering projects will also crack due to foundation settlement, concrete deformation or other factors, posing hidden dangers. In order to prevent leakage in the dam foundation or dam body, grouting is often performed on the cracks.
[0003] The grouting material commonly used at present is cement-based material. After adding water to make a thin slurry, it is injected into the cracks of the dam foundation or dam body through pressure grouting to achieve the effect of plugging leaks and preventing seepage.
[0004] The main problems with grouting materials at present are: 1) The rheological properties of grouting materials are not ideal, and smaller cracks cannot be poured into the grouting construction; 2) Cement-based grouting materials shrink in the hardening process. After the hardened slurry shrinks in the cracks with fixed width, secondary cracks are regenerated between the rocks and the grouting materials on both sides, making it impossible to fundamentally control the leakage of the dam foundation or dam body; 3) The bonding strength between the grouting materials and the matrix on both sides is not high, and the slurry volume shrinks, which causes the grouting materials to fall off under the action of seepage; 4) The grouting materials themselves have limited anti-seepage performance, and pressurized water can form small seepage in the grouting materials. Summary of the invention
[0005] The invention aims to solve the deficiencies of the prior art and provide an expansive high-efficiency anti-seepage composite grouting material.
[0006] In order to achieve the above object, the present invention adopts the following technical solutions:
[0007] An expansive high-efficiency anti-seepage composite grouting material comprises a component A and a component B, wherein the component A and the component B are uniformly mixed in a mass ratio of 1:(0.5-0.8);
[0008] Component A is prepared from the following raw materials by weight: 45-70 parts of cement, 1-10 parts of water-swellable rubber powder, 10-20 parts of fly ash, 5-20 parts of ultrafine mineral powder, 0-10 parts of silica fume, 0.05-0.4 parts of fluidizing agent, 0-0.2 parts of water retaining agent, 0.2-2 parts of redispersible latex powder, 0-0.04 parts of retarder, and 0.02-0.05 parts of defoaming agent.
[0009] Component B is prepared from the following raw materials according to weight ratio: 2-6 parts of water-soluble epoxy resin and 94-98 parts of water.
[0010] The cement of component A is composited by silicate cement and sulphoaluminate cement, and the mass ratio of silicate cement to sulphoaluminate cement is 7:3 to 9:1.
[0011] The water-swellable rubber powder has a fineness of 100 to 200 meshes and an expansion rate of 50% to 300%.
[0012] The specific surface area of ultrafine mineral powder is not less than 800m 2 / kg.
[0013] Silica fume is highly active silicon dioxide with a particle diameter no greater than 1 micron.
[0014] The fluidizing agent is polycarboxylic acid high-efficiency water reducing agent.
[0015] The water retaining agent is hydroxypropyl methylcellulose or a homologue of hydroxypropyl methylcellulose.
[0016] The retarder is boric acid.
[0017] The beneficial effects of the present invention are as follows: the composite grouting material of the present invention has a fast setting speed, good fluidity, produces a slight volume expansion during the hardening process, has good adhesion with the contacting rock layer, and has a good anti-seepage effect. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] Figure 1 The drying shrinkage strain curves at different sulphoaluminate cement dosages in the specific embodiment;
[0019] Figure 2 It is the strength development curve under different sulphoaluminate cement dosage in the specific embodiment;
[0020] Figure 3 : Drying shrinkage strain curves at different water-swellable rubber powder dosages in a specific embodiment;
[0021] Figure 4 is the tensile bonding strength at different water-soluble epoxy resin dosages in a specific embodiment;
[0022] The following is a detailed description of the embodiments of the present invention with reference to the accompanying drawings. DETAILED DESCRIPTION
[0023] The principles and features of the present invention are described below in conjunction with the accompanying drawings. The embodiments are only used to explain the present invention and are not used to limit the scope of the present invention. The present invention is described in more detail by way of example with reference to the accompanying drawings in the following paragraphs. The advantages and features of the present invention will become clearer according to the following description. It should be noted that the accompanying drawings are all in a very simplified form and are not in precise proportions, and are only used to facilitate and clearly assist in explaining the purpose of the embodiments of the present invention.
[0024] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art of the present invention. The terms used herein in the specification of the present invention are only for the purpose of describing specific embodiments and are not intended to limit the present invention. The term "and / or" used herein includes any and all combinations of one or more related listed items.
[0025] The present invention will be further described below in conjunction with the accompanying drawings and embodiments:
[0026] An expansive high-efficiency anti-seepage composite grouting material, composed of component A and component B. At the construction site, component A and component B are mixed in a certain proportion to form a grouting material.
[0027] Component A consists of cement (Portland cement, sulphoaluminate cement), water-swellable rubber powder, ultrafine mineral powder, silica fume, fluidizing agent, water-retaining agent, redispersible latex powder, retarder and defoaming agent.
[0028] Component B: water-soluble epoxy resin, water.
[0029] A component composition:
[0030] Cement: Cement is the core component of grouting materials, accounting for 45 to 70 parts by weight; among them, sulphoaluminate cement accounts for 10% to 30% of the total weight of the two cements.
[0031] The cement is a compound of silicate cement and sulphoaluminate cement. The compounded cement has a short setting time and can quickly plug leaks. The product ettringite formed by the hydration reaction of sulphoaluminate cement has the characteristic of slight volume expansion, which can avoid secondary cracking between the grouting material and the rock mass.
[0032] Water-swellable rubber powder is a powder made of water-swellable rubber by a special crushing process, with a fineness of 100-200 mesh. The volume of rubber powder particles can expand by 50%-300% after water absorption and expansion. The expansion rate of 50%-100% is the preferred material. The greater the expansion rate, the less the dosage. The proportion of water-swellable rubber powder is 1-10 parts.
[0033] As micro-aggregate, water-swellable rubber powder generates expansion pressure after grouting, driving the grout to flow to finer cracks, making the grouting more complete and denser; at the same time, the grout is in closer contact with the rocks on both sides of the rock cracks. The grouting body is in a humid underground environment for a long time and will not shrink. Even if the grouting body is dehydrated and dried, the grout has completely hardened at this time, and the dehydration shrinkage of the rubber micro-aggregate will not cause the shrinkage of the grouting body.
[0034] The fly ash is secondary or primary fly ash, accounting for 10 to 20 parts by weight.
[0035] The specific surface area of ultrafine mineral powder is not less than 800m 2 / kg, accounting for 5 to 20 parts by weight.
[0036] Silica fume is highly active silicon dioxide with a particle diameter no greater than 1 micron, accounting for 0 to 10 parts by weight.
[0037] Fly ash, ultrafine slag powder, silica fume, these active mineral admixture particles form a good gradation, which makes the slurry have good fluidity, and the formed grouting body is dense and has good impermeability.
[0038] The fluidizing agent is a commercially available polycarboxylic acid high-efficiency water-reducing agent, accounting for 0.05 to 0.4 parts by weight.
[0039] The fluidizer improves the rheological properties of the slurry, allowing it to be poured into finer rock cracks, and the anti-seepage performance is better after grouting.
[0040] The water retaining agent is commercially available hydroxypropyl methylcellulose (HPMC) or its homologues, with a weight proportion of 0 to 0.2 parts.
[0041] Redispersible latex powder is a commercially available industrial product, accounting for 0.2 to 2 parts by weight.
[0042] The retarder is boric acid, with a weight ratio of 0.0 to 0.04 parts.
[0043] The defoaming agent is a commercially available defoaming agent, accounting for 0.02 to 0.05 parts by weight.
[0044] Water-retaining agents, retarders and defoaming agents can adjust the construction performance of the grouting material according to changes in raw material properties, seasonal changes and construction conditions.
[0045] The above materials constitute component A of the expansive high-efficiency anti-seepage composite grouting material of the present invention.
[0046] Composition of component B:
[0047] 2-6 parts of water-soluble epoxy resin; 94-98 parts of water.
[0048] During the coagulation and hardening process of the grouting body, water will be consumed by cement hydration, while the water-soluble epoxy resin will remain in the pores and undergo cross-linking and solidification, thus blocking the pores and greatly improving the anti-penetration ability of the grouting body.
[0049] When used in engineering projects, the grouting material for grouting construction can be obtained by fully mixing the components in a mass ratio of component A: component B = 1: (0.5-0.8). Specific embodiment:
[0051] 1. Test the effect of different sulphoaluminate cement dosages on the expansion properties and strength growth rate of grouting materials.
[0052] Sulphoaluminate cement was added in different proportions in component A, while the other components and proportions remained unchanged.
[0053] The distribution ratio of group A with different sulphoaluminate cement content is shown in Table 1:
[0054] Table 1
[0055]
[0056] Component B is 4 parts of water-soluble epoxy resin and 96 parts of water.
[0057] The mass ratio of component A: component B = 1:0.6 was fully mixed to prepare the grouting material, and the drying shrinkage test was carried out on the grouting material. The measured drying shrinkage data are shown in Table 2, and the drying shrinkage strain curve is shown in Figure 1 As shown in the figure, it can be seen that with the continuous increase of the content of sulphoaluminate cement, the drying shrinkage strain of the grouting material is significantly reduced.
[0058] Table 2
[0059]
[0060] The grouting material was subjected to strength test, and the compressive strength obtained is shown in Table 3. The strength development curve is shown in Figure 2 As shown, it can be seen that with the continuous increase in the dosage of sulphoaluminate cement, the strength of the grouting material increases, and when it reaches a certain amount, it basically remains unchanged.
[0061] Table 3
[0062]
[0063] 2. Test the effect of different dosages of water-swelling rubber powder on the expansion performance of grouting materials.
[0064] The water-swellable rubber powder in component A is added in different proportions, while the other components and proportions remain unchanged.
[0065] The distribution ratio of group A with different water-swellable rubber powder dosages is shown in Table 4:
[0066] Table 4
[0067]
[0068] Component B is 4 parts of water-soluble epoxy resin and 96 parts of water.
[0069] The mass ratio of component A: component B = 1:0.6 was fully mixed to prepare the grouting material, and the drying shrinkage test was carried out on the grouting material. The measured drying shrinkage data are shown in Table 5, and the drying shrinkage strain curve is shown in Figure 3 As shown in the figure, it can be seen that with the increasing amount of water-swellable rubber powder, the drying shrinkage strain of the grouting material is significantly reduced.
[0070] Table 5
[0071]
[0072] 3. Test the effect of different dosages of water-soluble epoxy resin on the bonding strength of grouting materials.
[0073] The composition and ratio of component A remain unchanged, as shown in Table 6.
[0074] Table 6
[0075]
[0076] The distribution ratio of group B with different water-swellable rubber powder dosages is shown in Table 7:
[0077] Table 7
[0078]
[0079] The bonding strength of grouting materials under different water-soluble epoxy resin dosages is as follows Figure 4 As shown, it can be seen that the greater the dosage of water-soluble epoxy resin, the higher the bonding strength of the grouting material.
[0080] The present invention is described above by way of example in conjunction with the accompanying drawings. It is obvious that the specific implementation of the present invention is not limited to the above-mentioned method. As long as various improvements are made using the method concept and technical solution of the present invention, or are directly applied to other occasions without improvement, they are all within the protection scope of the present invention.
Claims
1. An expansive high-efficiency anti-seepage composite grouting material, characterized in that: Comprising component A and component B, component A and component B are uniformly mixed in a mass ratio of 1:(0.5-0.8); Component A is prepared from the following raw materials by weight: 45-70 parts of cement, 1-10 parts of water-swellable rubber powder, 10-20 parts of fly ash, 5-20 parts of ultrafine mineral powder, 0-10 parts of silica fume, 0.05-0.4 parts of fluidizing agent, 0-0.2 parts of water-retaining agent, 0.2-2 parts of redispersible latex powder, 0-0.04 parts of retarder, and 0.02-0.05 parts of defoaming agent. Component B is prepared from the following raw materials in weight ratio: 2-6 parts of water-soluble epoxy resin and 94-98 parts of water.
2. The expansive high-efficiency anti-seepage composite grouting material according to claim 1, characterized in that: The cement of component A is composited from silicate cement and sulphoaluminate cement, and the mass ratio of silicate cement to sulphoaluminate cement is 7:3 to 9:
1.
3. The expansive high-efficiency anti-seepage composite grouting material according to claim 2, characterized in that: The water-swelling rubber powder has a fineness of 100 to 200 meshes and an expansion rate of 50% to 300%.
4. The expansive high-efficiency anti-seepage composite grouting material according to claim 3, characterized in that: The specific surface area of ultrafine mineral powder is not less than 800m 2 / kg.
5. The expansive high-efficiency anti-seepage composite grouting material according to claim 4, characterized in that: Silica fume is highly active silicon dioxide with a particle diameter no greater than 1 micron.
6. The expansive high-efficiency anti-seepage composite grouting material according to claim 5, characterized in that: The fluidizing agent is polycarboxylic acid high-efficiency water reducer.
7. The expansive high-efficiency anti-seepage composite grouting material according to claim 6, characterized in that: The water-retaining agent is hydroxypropyl methylcellulose or a homologue of hydroxypropyl methylcellulose.
8. The expansive high-efficiency anti-seepage composite grouting material according to claim 7, characterized in that: The retarder is boric acid.
Citation Information
Patent Citations
Super-high early-strength grouting material for repairing ballastless track structure of high speed railway
CN102503310A
Cement-based grouting material and preparation method thereof
CN102515651A
Water-borne epoxy resin modified cement grouting material
CN105503068A
Novel leaking stoppage material