Oxide solid electrolyte and preparation method and application thereof
By using titanium oxide, aluminum oxide and boron trioxide in the oxide solid electrolyte, and through granulation, sintering and crushing and screening processes, the problem of insufficient lithium ion conductivity is solved and high ion conductivity and excellent rate performance are achieved. , suitable for high-rate solid-state batteries.
Patent Information
- Application Number
- CN202410847737.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-27
- Publication Date
- 2024-10-15
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The lithium ion conductivity of the oxide solid electrolyte is insufficient to meet the requirements for high-rate charge and discharge.
Using titanium oxide, aluminum oxide and boron trioxide as the main raw materials, through granulation, high-temperature sintering and crushing and screening methods, an oxide solid electrolyte with high ionic conductivity is formed. Through a specific molar fraction ratio and particle size Control, reduce the interface resistance of lithium ions at the grain boundary, and improve conductivity and rate performance.
The ionic conductivity and rate performance of the oxide solid-state electrolyte are significantly improved, and it is suitable for use in high-rate solid-state batteries. The method is simple, low-cost, and suitable for large-scale production.
Smart Images

Figure BDA0004916165090000071 
Figure BDA0004916165090000081
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of lithium-ion batteries, and in particular to an oxide solid electrolyte and a preparation method and application thereof. Background Art
[0002] With the development of lithium-ion battery technology, it has gradually become a dominant player in the field of consumer electronic products such as laptops, mobile phones, and digital cameras. In recent years, it has shown remarkable development prospects in the fields of power tools, automotive power batteries, and energy storage systems. At the same time, higher requirements have been put forward for its energy density and safety. Those skilled in the art have conducted extensive research on new positive and negative electrode materials, electrolytes, and diaphragms.
[0003] Among many technical directions, solid-state batteries are hailed as the next generation of lithium-ion batteries because of their higher safety and ability to match high-energy-density positive and negative electrode materials. Solid-state electrolytes are the core components of solid-state batteries, and are mainly divided into polymer electrolytes, sulfide electrolytes, and oxide electrolytes. Among them, oxide solid-state electrolytes have high ionic conductivity, high chemical stability, wide electrochemical window, and excellent comprehensive performance, making them a research hotspot. However, the lithium-ion conductivity of oxide solid-state electrolytes themselves still cannot meet the requirements of high-rate charging and discharging of batteries. Improving the ionic conductivity of oxide solid-state electrolytes is still the focus of current research in academia and industry. Summary of the invention
[0004] In order to solve the above problems, the present application provides an oxide solid electrolyte and its preparation method and application. The technical problem to be solved is how to reduce the interfacial resistance of lithium ions at the grain boundaries during the transmission process to improve its ionic conductivity and rate performance. The preparation method of the present application is simple, the reaction conditions are mild, the cost is low, and it is suitable for large-scale production. The oxide solid electrolyte of the present application has the advantages of high ionic conductivity and excellent rate performance, and is suitable for application in high-rate solid-state batteries.
[0005] In a first aspect, the present application provides a method for preparing an oxide solid electrolyte, using the following technical solution: A method for preparing an oxide solid electrolyte comprises the following steps: S1. Mix oxide, lithium carbonate, ammonium dihydrogen phosphate and deionized water according to their weight fractions, and then granulate them using a granulation device to obtain small balls with a particle size of 4-5 mm, and then dry the small balls to obtain substance A; S2, sintering material A at high temperature, cooling down, and obtaining material B; S3. Crush and sieve substance B to obtain an oxide solid electrolyte.
[0006] By adopting the above technical scheme, S1, the oxide, lithium carbonate, ammonium dihydrogen phosphate and deionized water are mixed, and then granulated by a granulating device to obtain a small ball with a particle size of 4-5mm, and then the small ball is dried to obtain substance A. The main function of this step is to mix the raw materials evenly, and to make the mixture into small balls by a granulating device, which is convenient for subsequent high-temperature sintering and crushing and screening. S2, substance A is sintered at high temperature, cooled and cooled to obtain substance B. The main function of this step is to react the oxide in substance A with boron trioxide through high-temperature sintering to form a glass phase, thereby improving the conductivity of lithium ions at the grain boundary and improving the ionic conductivity and rate performance of lithium-ion solid-state batteries. S3, substance B is crushed and screened to obtain an oxide solid electrolyte. The main function of this step is to crush and screen the substance B sintered at high temperature to obtain the desired oxide solid electrolyte particle size. The ionic conductivity and rate performance of the oxide solid electrolyte can be further improved by accurately controlling the heating rate, insulation temperature and cooling rate. This is because the heating rate, holding temperature and cooling rate directly affect the grain boundary structure and ion transport characteristics of the oxide solid electrolyte. By precisely controlling these parameters, the performance of the oxide solid electrolyte can be optimized.
[0007] Preferably, in step S1, the mass ratio of the oxide, lithium carbonate, diammonium phosphate and deionized water is (534-545):(88.8-103.6):(690-720):(150-200).
[0008] Preferably, in step S1, the oxide is prepared by mixing titanium oxide, aluminum oxide and boron trioxide in a molar ratio of 3.4:0.3:(0.2-0.3), and the particle sizes of the titanium oxide, aluminum oxide and boron trioxide are all 5-10 μm.
[0009] By adopting the above technical scheme, titanium oxide occupies the largest molar fraction ratio in this mixture, which means that it plays a dominant role in the structure and performance of the final electrolyte. Titanium oxide has good chemical stability and a high dielectric constant, which helps to improve the overall ionic conductivity of the electrolyte. Although the molar fraction of aluminum oxide in the mixture is relatively small, its addition can improve the mechanical strength and thermal stability of the electrolyte. As a high-hardness material, the addition of aluminum oxide can enhance the structural stability of the electrolyte, thereby reducing the generation of cracks during battery charging and discharging. Although the amount of boron trioxide added is not large, since boron is a typical glass network former, it can form a glass phase at the grain boundary during high-temperature calcination, which helps to improve the conductivity of lithium ions at the grain boundary, thereby improving the ionic conductivity and rate performance of lithium-ion solid-state batteries. The particle size of the raw materials directly affects their reactivity and mixing uniformity. Smaller particle size means higher specific surface area, which helps to increase the contact area between the raw materials and promote more sufficient chemical reactions, thereby obtaining a uniform and dense electrolyte structure. During the sintering process, raw materials with smaller particle sizes can reduce the sintering temperature, reduce energy consumption, and help to obtain a finer and more uniform microstructure, which is crucial for improving the ionic conductivity and mechanical properties of the electrolyte. By precisely controlling the molar fraction ratio of titanium oxide, aluminum oxide and boron trioxide, and keeping the particle size of the raw materials at 5-10μm, a more optimized crystal structure can be formed during the sintering process, which is conducive to the rapid transmission of lithium ions, thereby improving the performance of the electrolyte. The optimization of the above composition not only improves the ionic conductivity of the electrolyte, but also enhances its stability and reliability under high-rate discharge conditions, which is of great significance for the development of high-performance solid-state batteries. In summary, the synergistic effect of titanium oxide, aluminum oxide and boron trioxide in the preparation of oxide solid electrolytes is reflected in their contribution to the excellent performance of the final electrolyte through specific molar fraction ratios and particle sizes. By precisely controlling these parameters, the interfacial resistance at the grain boundary during the transmission of lithium ions can be effectively reduced, thereby improving the ionic conductivity and rate performance of the electrolyte, which is of great significance for the development of solid-state batteries.
[0010] Preferably, in step S1, the mixing is performed by a stirring mixer at a stirring rate of 50-100 rpm for a mixing time of 1-3 hours, and the drying is performed by drying the pellets until the mass content of water is 7%-8%.
[0011] Preferably, in step S2, the high temperature sintering process is: heating the temperature to 700-850°C at a heating rate of 5-6°C / min and keeping the temperature for 2-5h.
[0012] By adopting the above technical scheme, the oxide, lithium carbonate, ammonium dihydrogen phosphate and other components in substance A are fully reacted to form an oxide solid electrolyte with good ion conductivity. First, the control of the heating rate can ensure that the components in substance A react at an appropriate temperature, avoiding the decomposition of components or incomplete reaction due to too fast heating. At the same time, the control of the heating rate can also avoid energy waste and reduced production efficiency due to too slow heating. Secondly, the selection of the insulation temperature can ensure that the components in substance A react fully at an appropriate temperature to form an oxide solid electrolyte with good ion conductivity. At the same time, the selection of the insulation temperature can also avoid the structural destruction or performance degradation of the oxide solid electrolyte caused by too high insulation temperature. Through such a high-temperature sintering process, the ionic conductivity and rate performance of the oxide solid electrolyte can be effectively improved, thereby meeting the application requirements of high-rate solid-state batteries.
[0013] Preferably, in step S2, the cooling is performed at a cooling rate of 3-4°C / min to 100-200°C, and then naturally cooled to room temperature.
[0014] By adopting the above technical solution, in step S2, the cooling process is an important link, which directly affects the structure and performance of the oxide solid electrolyte. By cooling to 100-200°C at a cooling rate of 3-4°C / min and then cooling naturally to room temperature, the grain growth and grain boundary formation of substance B can be effectively controlled. First, the control of the cooling rate can affect the growth rate and size of the grains. If the cooling rate is too fast, the grains may be too refined, resulting in an increase in grain boundaries, thereby increasing the interfacial resistance of lithium ions during transmission. On the contrary, if the cooling rate is too slow, the grains may be too large, resulting in a reduction in grain boundaries, which will also affect the conductivity of lithium ions. Therefore, by accurately controlling the cooling rate, a moderate grain size and number can be obtained, thereby optimizing the conduction path of lithium ions. Secondly, cooling to a temperature range of 100-200°C is also critical. In this temperature range, the crystal structure of the oxide solid electrolyte will gradually stabilize and the grain boundaries will gradually form. If the temperature is too low, the crystal structure may be unstable, affecting the performance of the electrolyte. On the contrary, if the temperature is lowered too high, it may lead to excessive formation of grain boundaries, which will also affect the conductivity of lithium ions. Therefore, by precisely controlling the cooling temperature, a stable crystal structure and a suitable number of grain boundaries can be obtained, thereby improving the conductivity of lithium ions. Finally, a natural cooling process to room temperature is also necessary. This process allows the temperature of the oxide solid electrolyte to gradually decrease, avoiding structural changes or stress caused by rapid temperature changes. At the same time, natural cooling can also release the internal stress of the oxide solid electrolyte, further improving its stability and performance. In summary, by precisely controlling the heating rate, insulation temperature, cooling rate, and cooling process, the ionic conductivity and rate performance of the oxide solid electrolyte can be effectively improved.
[0015] Preferably, in step S3, the pulverization is performed by a jet mill, the air source is air, the air temperature is 120-140° C., the pulverization pressure is 0.8-0.9 MPa, and the particle size of the material after pulverization is 1-8 μm.
[0016] Preferably, in step S3, the screening uses an ultrasonic vibration screen, the ultrasonic vibration screen has an ultrasonic vibration frequency of 300-600 Hz, and the screen has a mesh size of 2500.
[0017] In a second aspect, the present application provides an oxide solid electrolyte, which adopts the following technical solution: As a general technical concept, the present application also provides the above-mentioned oxide solid electrolyte, which is prepared by the above-mentioned preparation method of the oxide solid electrolyte.
[0018] In a third aspect, the present application provides an application of an oxide solid electrolyte, using the following technical solution: As a general technical concept, the present application also provides an application of the above-mentioned oxide solid electrolyte in the field of all-solid-state battery technology.
[0019] In summary, the beneficial technical effects of this application are: 1. Reduce the interfacial resistance of lithium ions at the grain boundaries during transmission and improve their ion conductivity and rate performance. By adding a specific proportion of boron trioxide to the oxide and forming a glass phase during high-temperature calcination, the conductivity of lithium ions at the grain boundaries is improved.
[0020] 2. The preparation method is simple, the reaction conditions are mild, the cost is low, and it is suitable for large-scale production. This method uses common oxides, lithium carbonate, ammonium dihydrogen phosphate and deionized water as raw materials, and obtains oxide solid electrolytes through simple granulation, calcination, crushing and screening steps.
[0021] 3. Oxide solid electrolytes have high ionic conductivity and excellent rate performance. Due to the addition of boron and the precise control of heating rate, insulation temperature and cooling rate, oxide solid electrolytes have good application prospects in high-rate solid-state batteries.
[0022] 4. Suitable for high-rate solid-state battery applications. Due to the high ionic conductivity and excellent rate performance of oxide solid electrolytes, they are ideal for high-rate solid-state batteries. DETAILED DESCRIPTION
[0023] The embodiments of the present application will be described in detail below in conjunction with the examples, but it will be appreciated by those skilled in the art that the following examples are only used to illustrate the present application and should not be considered as limiting the scope of the present application. In the examples, if specific conditions are not specified, they are carried out according to normal conditions or the conditions recommended by the manufacturer. If the manufacturer is not specified for the reagents or instruments used, they are all conventional products that can be purchased commercially.
[0024] Example 1 A method for preparing an oxide solid electrolyte comprises the following steps: S1. According to the mass fractions, 534g of oxide, 88.8g of lithium carbonate, 690g of ammonium dihydrogen phosphate and 150g of deionized water were mixed, and a stirring mixer was used at a stirring rate of 50rpm for a mixing time of 3 hours, and then granulated by a granulating device to obtain small balls with a particle size of 4-5mm, and then the small balls were dried to a water content of 7% by mass to obtain substance A; the oxide was prepared by mixing titanium oxide, aluminum oxide and boron trioxide in a molar fraction ratio of 3.4:0.3:0.2, and the particle sizes of the titanium oxide, aluminum oxide and boron trioxide were all 5-10μm; S2, heating material A to 700°C at a rate of 5°C / min and keeping the temperature for 5 hours, sintering at high temperature, cooling to 200°C at a rate of 3°C / min, and then naturally cooling to room temperature to obtain material B; S3. The substance B is crushed by a jet mill, the air source is air, the air temperature is 120°C, the crushing pressure is 0.8MPa, the particle size of the crushed material is 1-8μm, and an ultrasonic vibration screen is used for screening. The ultrasonic vibration screen has an ultrasonic vibration frequency of 300Hz and a sieve of 2500 mesh to obtain an oxide solid electrolyte.
[0025] Example 2 A method for preparing an oxide solid electrolyte comprises the following steps: S1. According to the mass fractions, 545g of oxide, 103.6g of lithium carbonate, 720g of ammonium dihydrogen phosphate and 200g of deionized water were mixed, and a stirring mixer was used at a stirring rate of 100rpm for a mixing time of 1 hour, and then granulated by a granulating device to obtain small balls with a particle size of 4-5mm, and then the small balls were dried to a water content of 8% by mass to obtain substance A; the oxide was prepared by mixing titanium oxide, aluminum oxide and boron trioxide in a molar fraction ratio of 3.4:0.3:0.3, and the particle sizes of the titanium oxide, aluminum oxide and boron trioxide were all 5-10μm; S2, heating material A to 850°C at a rate of 6°C / min and keeping the temperature for 2h, sintering at high temperature, cooling to 100°C at a rate of 4°C / min, and then naturally cooling to room temperature to obtain material B; S3. The substance B is crushed by a jet mill, the air source is air, the air temperature is 140°C, the crushing pressure is 0.9MPa, the particle size of the crushed material is 1-8μm, and the material is sieved by an ultrasonic vibration screen, the ultrasonic vibration frequency of the ultrasonic vibration screen is 600Hz, and the screen is 2500 mesh to obtain an oxide solid electrolyte.
[0026] Example 3 A method for preparing an oxide solid electrolyte comprises the following steps: S1. According to the mass fractions, 541g of oxide, 95g of lithium carbonate, 700g of ammonium dihydrogen phosphate and 180g of deionized water were mixed, and a stirring mixer was used at a stirring rate of 80rpm for a mixing time of 2 hours, and then granulated by a granulating device to obtain small balls with a particle size of 4-5mm, and then the small balls were dried to a water content of 7.6% by mass to obtain substance A; the oxide was prepared by mixing titanium oxide, aluminum oxide and boron trioxide in a molar fraction ratio of 3.4:0.3:0.25, and the particle sizes of the titanium oxide, aluminum oxide and boron trioxide were all 5-10μm; S2, heating material A to 780°C at a rate of 5.5°C / min and keeping the temperature for 3.6h, sintering at high temperature, cooling to 160°C at a rate of 3.5°C / min, and then naturally cooling to room temperature to obtain material B; S3. The substance B is crushed by a jet mill, the air source is air, the air temperature is 130°C, the crushing pressure is 0.85MPa, the particle size of the crushed material is 1-8μm, and an ultrasonic vibration screen is used for screening. The ultrasonic vibration screen has an ultrasonic vibration frequency of 450Hz and a sieve of 2500 mesh to obtain an oxide solid electrolyte.
[0027] Comparative Example 1 The same as Example 3, except that: in step S1, the oxide is prepared by mixing titanium oxide and aluminum oxide in a molar ratio of 3.4:0.3, and the particle sizes of the titanium oxide and aluminum oxide are both 5-10 μm.
[0028] Comparative Example 2 The same as Example 3, except that: in step S1, the oxide is prepared by mixing titanium oxide, aluminum oxide and boron trioxide in a molar ratio of 3.4:0.3:0.5, and the particle sizes of titanium oxide, aluminum oxide and boron trioxide are all 5-10 μm.
[0029] Comparative Example 3 The same as Example 3, except that: in step S2, the heating rate is 7.5°C / min.
[0030] Comparative Example 4 The same as Example 3, except that: in step S2, the heating rate is 3.5°C / min.
[0031] Comparative Example 5 The same as Example 3, except that: in step S2, the cooling rate is 5.5°C / min.
[0032] Comparative Example 6 The same as Example 3, except that: in step S2, the cooling rate is 1°C / min.
[0033] Performance Testing The oxide solid electrolytes prepared in Examples 1 to 3 and Comparative Examples 1 to 6 were sampled, respectively, and then pressed into solid electrolyte sheets with a diameter of 16 mm and a thickness of 1 mm at a pressure of 200 MPa, and tested. The test results are shown in Table 1.
[0034] Ionic conductivity test: The ionic conductivity of the solid electrolyte was obtained by assembling blocking electrodes to perform electrochemical impedance spectroscopy (EIS) test. The specific operation method is as follows: The oxide solid electrolyte sheets prepared in each embodiment and comparative example have stainless steel sheets as blocking electrodes on both sides to form a symmetrical cell; the electrochemical workstation used is DH7001, and the frequency range is 0.01-10 6 Hz, test the EIS of oxide solid electrolyte sheets at 25°C. The ionic conductivity of the solid electrolyte is calculated as follows: δ = L / (R·S) Where, δ is the ionic conductivity (unit S / cm), L is the thickness of the solid electrolyte sheet (unit cm), R is the intrinsic resistance of the solid electrolyte (unit Ω), S is the effective cross-sectional area of the solid electrolyte sheet (unit cm 2 ). The higher the test result of ionic conductivity, the better its ionic conductivity.
[0035] Rate performance test: Make a solid-state battery with lithium cobalt oxide as the positive electrode and metallic lithium as the negative electrode to evaluate the rate performance of the oxide solid electrolyte. The specific operation method is as follows: Lithium cobalt oxide, conductive agent Super P, and binder PVDF (polyvinylidene fluoride) were mixed in a mass ratio of 9:0.5:0.5, and an appropriate amount of solvent NMP (N-methylpyrrolidone) was added and stirred to prepare a positive electrode slurry, which was coated on aluminum foil, dried at 100°C, and then cut into discs with a diameter of 10 mm as positive electrodes. CR2032 button batteries were assembled in the order of positive electrode sheet-oxide solid electrolyte sheet-lithium foil. Battery rate test was performed.
[0036] The operating voltage range of the all-solid-state lithium secondary battery is set to 3V-4.2V, and the current density is 0.15mA / cm 2 ) at a constant current to 4.2 V, and then at a constant voltage to 0.01C cutoff; then discharged to 3 V at currents of 0.1C, 0.5C, 1C, and 5C, respectively, to obtain the gram capacity of the material at 0.1C, 0.5C, 1C, and 5C discharge rates, respectively.
[0037] Table 1 Electrochemical performance test results Analyzing the data in Table 1, we can see that: 1) The oxide solid electrolytes prepared in Examples 1 to 3 have the advantages of high ionic conductivity and excellent rate performance, and are suitable for application in high-rate solid-state batteries.
[0038] 2) The comparative analysis of the performance of the oxide solid electrolytes prepared in combination with Example 3 and Comparative Examples 1-2 shows that precise control of the amount of boron trioxide added can form a glass phase at the grain boundaries during high-temperature calcination, which helps to improve the conductivity of lithium ions at the grain boundaries, thereby improving the ionic conductivity and rate performance of lithium-ion solid-state batteries.
[0039] 3) The comparative analysis of the performance of the oxide solid electrolytes obtained in Example 3 and Comparative Examples 3-4 shows that by precisely controlling the heating rate, the ionic conductivity and rate performance of the oxide solid electrolyte can be effectively improved, thereby meeting the application requirements of high-rate solid-state batteries.
[0040] 4) The comparative analysis of the performance of the oxide solid electrolytes obtained in combination with Example 3 and Comparative Examples 5-6 shows that by precisely controlling the cooling rate, the ionic conductivity and rate performance of the oxide solid electrolyte can be effectively improved, thereby meeting the application requirements of high-rate solid-state batteries.
[0041] The above embodiments are only used to explain the technical solutions of the present application rather than to limit them. Although the above embodiments provide a specific description of the present application, relevant technical personnel should understand that the specific implementation methods of the present application can still be modified or replaced by equivalents, and any modifications and equivalent replacements that do not depart from the spirit and scope of the present application should be included in the protection scope of the present application.
Claims
1. A method for preparing an oxide solid electrolyte, characterized in that: The following steps are involved: S1. Mix oxide, lithium carbonate, ammonium dihydrogen phosphate and deionized water according to their weight fractions, and then granulate them using a granulation device to obtain small balls with a particle size of 4-5 mm, and then dry the small balls to obtain substance A; S2, sintering material A at high temperature, cooling it down, and obtaining material B; S3. Crush and sieve substance B to obtain an oxide solid electrolyte.
2. The method for preparing an oxide solid electrolyte according to claim 1, characterized in that: In step S1, the mass ratio of the oxide, lithium carbonate, ammonium dihydrogen phosphate and deionized water is (534-545): (88.8-103.6): (690-720): (150-200).
3. The method for preparing an oxide solid electrolyte according to claim 1, characterized in that: In step S1, the oxide is prepared by mixing titanium oxide, aluminum oxide and boron trioxide in a molar ratio of 3.4:0.3:(0.2-0.3), and the particle sizes of the titanium oxide, aluminum oxide and boron trioxide are all 5-10 μm.
4. The method for preparing an oxide solid electrolyte according to claim 1, characterized in that: In step S1, the mixing is performed by a stirring mixer at a stirring rate of 50-100 rpm for 1-3 hours, and the drying is performed by drying the pellets until the mass content of water is 7%-8%.
5. The method for preparing an oxide solid electrolyte according to claim 1, characterized in that: In step S2, the high temperature sintering process is: heating the temperature to 700-850°C at a heating rate of 5-6°C / min and keeping the temperature for 2-5h.
6. The method for preparing an oxide solid electrolyte according to claim 1, characterized in that: In step S2, the temperature is lowered to 100-200°C at a rate of 3-4°C / min, and then naturally cooled to room temperature.
7. The method for preparing an oxide solid electrolyte according to claim 1, characterized in that: In step S3, the pulverization is performed by a jet mill, the air source is air, the air temperature is 120-140° C., the pulverization pressure is 0.8-0.9 MPa, and the particle size of the material after pulverization is 1-8 μm.
8. The method for preparing an oxide solid electrolyte according to claim 1, characterized in that: In step S3, the screening is performed by an ultrasonic vibration screen, the ultrasonic vibration frequency of the ultrasonic vibration screen is 300-600 Hz, and the screen size is 2500 meshes.
9. An oxide solid electrolyte prepared according to the method for preparing an oxide solid electrolyte according to any one of claims 1 to 8, characterized in that: The ionic conductivity of the oxide solid electrolyte is ≥3.3×10 4 S / cm.
10. Use of the oxide solid electrolyte according to claim 9 in the field of all-solid-state battery technology.
Citation Information
Patent Citations
Preparation method of solid electrolyte (titanium-lithium-aluminum phosphate) for lithium ion battery
CN108615934A
Preparation method of garnet type solid electrolyte with high ionic conductivity
CN114497714A
Oxide solid electrolyte and preparation method and application thereof
CN115799619A
Pure-phase lithium titanium aluminum phosphate, solid electrolyte material and preparation method thereof
CN116986573A
Lithium titanium aluminum phosphate material, diaphragm, preparation method of lithium titanium aluminum phosphate material and diaphragm, and battery
CN117923454A