High-purity continuous preparation method of bifunctional (methyl) acrylate

By using a bimetallic composite catalyst modified with sulfuric acid, a fixed-bed reactor and a multi-stage molecular distillation system, the problems of long reaction time and product self-polymerization in the preparation of bifunctional (meth)acrylates are solved, achieving high efficiency and low cost. Cost-effective high-purity preparation.

CN118771981APending Publication Date: 2024-10-15SHIMING (LIAONING) NEW MATERIAL CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410765204.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-14
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

The existing technology has problems such as long esterification reaction time, easy self-polymerization of the product, difficulty in wastewater treatment, and difficulty in catalyst recovery when preparing bifunctional (meth)acrylate, resulting in high product cost and difficulty in ensuring purity.

Method used

The bimetallic composite catalyst modified with sulfuric acid is combined with a fixed-bed reactor and a multi-stage molecular distillation system to improve reaction efficiency and product purity by catalyzing the transesterification reaction and performing multi-stage molecular distillation purification.

Benefits of technology

The reaction efficiency and purity of bifunctional (meth)acrylate are significantly improved, the consumption of by-products is reduced, and high-purity continuous preparation is achieved, which is suitable for industrial production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118771981A_ABST
    Figure CN118771981A_ABST
Patent Text Reader

Abstract

The invention discloses a high-purity continuous preparation method of bifunctional (methyl) acrylate, which comprises the following steps: (1) taking vinyl ether containing double bonds as a phase A, uniformly mixing monofunctional (methyl) acrylate with a polymerization inhibitor to obtain a phase B, respectively pumping the phases into a continuous reaction system, and continuously reacting for 2-3 hours; the catalyst is uniformly immobilized in a fixed bed reactor in the continuous reaction system; in the process of gradually heating to a certain temperature, the material forms a flowing homogeneous liquid and is subjected to a catalytic transesterification reaction to prepare a reaction product; and (3) introducing the reaction product obtained in the step (1) into molecular distillation equipment for purification, and continuously pumping raw materials with the same amount as the raw materials in the step (1) to finally obtain the high-purity bifunctional (methyl) acrylate. Under the action of the catalyst, the fixed bed reactor and the multi-stage molecular distillation system are effectively combined, the high-purity bifunctional (methyl) acrylate is produced, and the reaction efficiency, the production efficiency and the product purity are improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of acrylate preparation, and in particular to a high-purity continuous preparation method of difunctional (meth)acrylate. Background Art

[0002] Acrylates are cured by irradiation and heating with active energy rays such as ultraviolet rays or electron beams, and are used in large quantities as reactive diluent components in UV curing materials. The UV monomer mentioned in the present invention is not a conventional bisacryloxy UV monomer, but refers to a UV monomer containing both a (meth)acryloxy group and a terminal vinyl structure. Such monomers can simultaneously satisfy free radical curing and cationic curing, and can avoid the influence of oxygen inhibition on free radical photopolymerization. On the other hand, such monomers usually have extremely low viscosity and excellent dilutability, and can be used in the UV inkjet printing industry with extremely high viscosity requirements. However, the industrial esterification reaction time of the difunctional (meth)acrylate prepared by the intermittent autoclave esterification reaction is generally 6 to 12 hours at a temperature of 80 to 120°C. Since the raw materials and the target product are temperature-sensitive, the target product is very easy to self-polymerize when it stays in the autoclave for a long time under high temperature conditions. At the same time, the post-treatment needs to neutralize the excess acrylic acid or methacrylic acid, which produces a large amount of salt-containing wastewater, and there are problems such as the risk of corrosion of stainless steel equipment and high wastewater treatment costs. On the other hand, if a conventional solid bed reactor (without a molecular sieve gasification permeation membrane) is used, since the esterification rate is a slow reaction and the residence time is long, the risk of self-polymerization of the raw materials and products is also high.

[0003] In the post-processing process, the traditional process uses a packed tower for vacuum distillation separation, and the operating temperature reaches 100-200°C. However, the difunctional (meth) acrylic acid monomer is very easy to polymerize above 60°C, and it is difficult to separate it by heating it to less than 90°C under vacuum using the existing conventional distillation tower, so other equipment must be used for separation. At the same time, the distillation tower is difficult to operate, the process is complicated, and it takes a long time, which does not conform to the market principle of cost-effectiveness first, further causing the product cost to remain high.

[0004] In addition to conventional alcohol acid ester exchange processes, (meth)acrylates can also use less harmful organic tin compounds, titanate compounds or organic phosphorus compounds as catalysts to participate in the ester exchange reaction, but in actual industrial production, there is a problem that the catalyst is difficult to recover. Metal oxides also have good catalytic activity in the ester exchange reaction, but the active components are seriously lost under the conditions of the ester exchange reaction, which seriously affects their application in the industrial field. Summary of the invention

[0005] In order to solve the above technical problems, the purpose of the present invention is to provide a high-purity continuous preparation method of difunctional (meth)acrylate; the present invention uses double-bond-containing vinyl ether and monofunctional (meth)acrylate as raw materials, and under the action of a catalyst, effectively combines a fixed bed reactor with a multi-stage molecular distillation system to produce high-purity difunctional (meth)acrylate, thereby improving the reaction efficiency, production efficiency and product purity.

[0006] In order to achieve the above technical objectives and the above technical effects, the present invention is implemented through the following technical solutions:

[0007] A high-purity continuous preparation method of a difunctional (meth)acrylate comprises the following steps:

[0008] (1) A vinyl ether containing a double bond is used as phase A, and a monofunctional (meth)acrylate and a polymerization inhibitor are uniformly mixed as phase B, and the two are respectively pumped into a continuous reaction system, and the catalyst is uniformly immobilized in a fixed bed reactor in the continuous reaction system; in the process of gradually heating to a certain temperature, the materials form a flowing homogeneous liquid and a catalytic transesterification reaction occurs to obtain a reaction product;

[0009] (2) The reaction product obtained in step (1) is flowed into a molecular distillation device for purification, and the raw material in an amount equal to that in step (1) is continuously pumped in to finally obtain a high-purity bifunctional (meth)acrylate.

[0010] The catalyst is a bimetallic composite material modified by sulfuric acid, and its chemical formula is XMO 3 ·SO 4 2- , wherein X is selected from any one of lithium, sodium, potassium, magnesium, zinc, lead and barium; and M is selected from one of titanium and nickel.

[0011] The bimetallic composite material modified by sulfuric acid is synthesized by a simple hydrothermal method and then modified by sulfuric acid. Specifically, a compound containing the X element is dissolved in distilled water to form an X solution, and a compound containing the M element is dissolved in anhydrous ethanol to form an M solution. The X solution is added dropwise to the M solution and stirred for 2 hours. The mixture is placed in a reactor, heated to 150-200°C and maintained for 24 hours to form a bimetallic composite. After cooling, it is taken out, washed with methanol and deionized water, and vacuum dried to obtain the bimetallic composite catalyst XMO. 3 The catalyst obtained above was added to 0.5 mol / l H 2 SO 4 The solution was immersed for 24 hours, then rinsed with deionized water and heated to 400-500°C and maintained for 2 hours to obtain XMO. 3 ·SO 4 2- .

[0012] Preferably, the amount of the catalyst used is 0.8% to 3% of the total weight of the monomers.

[0013] Preferably, the vinyl ether is selected from at least one of 2-hydroxyethyl vinyl ether, 3-hydroxypropyl vinyl ether and di(poly)ethylene glycol monovinyl ether.

[0014] Preferably, the monofunctional (meth)acrylate is a compound having one (meth)acryloyl group in the molecule, such as general formula (I):

[0015]

[0016] In formula (I), R 1 represents a hydrogen atom or a methyl group, R 2 It represents a saturated alkyl group having 1 to 3 carbon atoms.

[0017] Preferably, the monofunctional (meth)acrylate is selected from at least one of methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, and isopropyl (meth)acrylate. More preferably, the monofunctional (meth)acrylate is selected from at least one of methyl methacrylate and ethyl acrylate.

[0018] Furthermore, the molar ratio of the vinyl ether to the monofunctional (meth)acrylate is 1:(1-5); an excess amount of (meth)acrylate is more conducive to the reaction to form a product.

[0019] Preferably, the polymerization inhibitor is selected from at least one of 2,6-di-tert-butylphenol, 2,4-di-tert-butylphenol, 2-tert-butyl-4,6-dimethylphenol, alkylated diphenylamine, N,N'-diphenyl-p-phenylenediamine, phenothiazine, 4-hydroxy-2,2,6,6-tetramethylpiperidine, 4-benzoyloxy-2,2,6,6-tetramethylpiperidine, 1,4-dihydroxy-2,2,6,6-tetramethylpiperidine, 1-hydroxy-4-benzoyloxy-2,2,6,6-tetramethylpiperidine, hydroquinone, methoxyhydroquinone, and benzoquinone.

[0020] More preferably, the polymerization inhibitor is selected from at least one of phenothiazine, hydroquinone, methoxyhydroquinone and benzoquinone.

[0021] The dosage of the polymerization inhibitor is 200-1000 ppm. During the reaction, too little polymerization inhibitor will lead to partial polymerization of the reactants, making the polymerization inhibition effect insignificant. Too much polymerization inhibitor will affect the color of the product.

[0022] According to the method of the present invention, the reaction of step (1) is as follows:

[0023]

[0024] R 1 =H / CH 3 R 2 =C n H m n=1~3.

[0025] The continuous reaction system of step (1) comprises a fixed bed reactor and a vacuum machine.

[0026] The fixed bed reactor has a feed port, a discharge port, a heating medium port, a heating chamber, a drain port and an inner cylinder, wherein a molecular sieve pervaporation membrane connected to the drain port is provided in the inner cylinder. In step (1), steam is injected into the heating chamber through the heating medium port, and the inner cylinder of the fixed bed reactor is heated to 80-90° C., so that the reaction materials in the inner cylinder stay at this temperature for 3-10 minutes, and an ester exchange reaction occurs under the catalysis of the catalyst; the water molecules and small molecular alcohols generated in the reaction are removed through the molecular sieve pervaporation membrane under the traction of vacuum, and discharged through the drain port connected to the molecular sieve pervaporation membrane, thereby realizing continuous catalytic ester exchange and waste removal, without the need for neutralization and water washing.

[0027] The initial product obtained by the reaction of step (1) flows into the multi-stage molecular distillation equipment described in step (2) under vacuum traction. The molecular distillation equipment in step (2) can be set up as a single-stage, double-stage or triple-stage molecular distillation system. When a double-stage or triple-stage molecular distillation system is used, a flow controller and a temperature control device are provided between each molecular distillation system.

[0028] Each molecular distillation system is equipped with a basic preheater, preheating kettle, scraping motor, reactor, vacuum machine, light component receiving tank, heavy component receiving tank, and cold trap. Heat transfer oil inlet and outlet are set on the outside of the preheating kettle and the reactor. When the preheater is working, the heat transfer oil enters from the heat transfer oil inlet and is discharged from the heat transfer oil outlet to heat the preheating kettle and the reactor.

[0029] When a two-stage or three-stage molecular distillation system is used, the purification of the difunctional (meth) acrylate is to collect the heavy component sample obtained by the previous stage molecular distillation and perform the next stage molecular distillation, repeatedly collect the heavy component sample, and obtain a high-purity difunctional (meth) acrylate finished product after multiple stages of molecular distillation. Preferably, a flow controller and a rotor flowmeter are set between the previous stage heavy component receiving tank and the next stage molecular distillation system. When the previous stage heavy component receiving tank accumulates to a certain amount, the flow controller and the rotor flowmeter are turned on, and the previous stage heavy components enter the next stage molecular distillation system.

[0030] The temperature control devices arranged between the molecular distillation systems at each level are respectively connected to the upper-level heavy component receiving tank and the lower-level molecular distillation system through pipelines.

[0031] The flow rate of the rotor flowmeter between the upper-stage heavy component receiving tank and the lower-stage molecular distillation system is controlled at 800-2000ml / min.

[0032] The reactor temperature range of the difunctional (meth)acrylate purification reaction in step (2) is 30-60°C, and the vacuum is 10-1000Pa. The reaction materials stay at this temperature and vacuum for 3-10 minutes to ensure that the excess raw materials are separated in time. Specifically, when there is a three-stage molecular distillation system, the first-stage molecular distillation can be used to separate the excess monofunctional (meth)acrylate, the temperature is 30-35°C, and the vacuum is 800-1000Pa; the second-stage molecular distillation removes the residual ether compounds, the temperature is controlled at 40-50°C, and the vacuum is 200-300Pa; the third-stage molecular distillation distills and recovers the product to separate it from the solid catalyst, the temperature is 50-60°C, and the vacuum is 10-50Pa.

[0033] The residence time of the product purification reaction in each stage of the molecular distillation system is consistent with the residence time of the reaction in the fixed bed reactor to ensure the continuity of the reaction.

[0034] The beneficial effects of the present invention are:

[0035] The present invention adopts a novel bimetallic composite catalyst modified by sulfuric acid as a reaction catalyst. The bimetallic composite material further improves the catalyst activity on the basis of the single metal material, can provide more active sites for the transesterification reaction, and improves the use repetition rate of the catalyst. In addition, the catalyst modified by sulfuric acid adds a B acid center on the basis of the original L acid center on the surface of the bimetallic composite, which can further improve the conversion rate of the reaction.

[0036] The present invention uses a combination of a fixed bed reactor and a molecular distillation system to promptly remove water molecules and small molecule alcohols produced during the reaction process from the reaction system, promote the forward movement of the equilibrium of the transesterification reaction, improve the conversion rate and reaction rate of the raw materials, and reduce the consumption of the catalyst by the by-products. Through the multi-stage molecular distillation system, the excess high-boiling point ether compound raw materials can be quickly separated from the product at low temperatures without the need for a traditional intermittent distillation device. The combination of a fixed bed reactor and a molecular distillation system can achieve process intensification in industrial applications, and can significantly improve the product purity to more than 99.5%. The process adopts a continuous production method, avoids a large amount of manual operation, has stable product quality, and is conducive to large-scale production. BRIEF DESCRIPTION OF THE DRAWINGS

[0037] Figure 1 This is a schematic structural diagram of a fixed bed reactor combined with a multi-stage molecular distillation system used in an embodiment of the present invention.

[0038] Figure 2This is the infrared spectrum of the difunctional (meth)acrylate obtained in Example 1 of the present invention.

[0039] Figure 3 This is the gas chromatogram of Example 1 of the present invention. DETAILED DESCRIPTION

[0040] The technical solutions in the present invention will be described clearly and completely below in conjunction with specific embodiments. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0041] The present invention provides a high-purity continuous preparation method of a difunctional (meth)acrylate, comprising the following steps:

[0042] (1) A vinyl ether containing a double bond is used as phase A, and a monofunctional (meth)acrylate and a polymerization inhibitor are uniformly mixed as phase B, and the two are respectively pumped into a continuous reaction system, and the catalyst is uniformly immobilized in a fixed bed reactor in the continuous reaction system; in the process of gradually heating to a certain temperature, the materials form a flowing homogeneous liquid and a catalytic transesterification reaction occurs to obtain a reaction product;

[0043] The reaction of step (1) is as follows:

[0044]

[0045] R 1 =H / CH 3 R 2 =C n H m n = 1 to 3;

[0046] (2) The reaction product obtained in step (1) is flowed into a molecular distillation device for purification, and the raw material in an amount equal to that in step (1) is continuously pumped in to finally obtain a high-purity bifunctional (meth)acrylate.

[0047] The catalyst is a bimetallic composite material modified by sulfuric acid, and its chemical formula is XMO 3 ·SO 4 2- , wherein X is selected from any one of lithium, sodium, potassium, magnesium, zinc, lead and barium; and M is selected from one of titanium and nickel.

[0048] The bimetallic composite material modified by sulfuric acid is synthesized by a simple hydrothermal method and then modified by sulfuric acid. Specifically, a compound containing the X element is dissolved in distilled water to form an X solution, and a compound containing the M element is dissolved in anhydrous ethanol to form an M solution. The X solution is added dropwise to the M solution and stirred for 2 hours. The mixture is placed in a reactor, heated to 150-200°C and maintained for 24 hours to form a bimetallic composite. After cooling, it is taken out, washed with methanol and deionized water, and vacuum dried to obtain the bimetallic composite catalyst XMO. 3 The catalyst obtained above was added to 0.5 mol / l H 2 SO 4 The solution was immersed for 24 hours, then rinsed with deionized water and heated to 400-500°C and maintained for 2 hours to obtain XMO. 3 ·SO 4 2- .

[0049] The amount of the catalyst used is 0.8% to 3% of the total mass of the monomers (vinyl ether containing double bonds and monofunctional (meth) acrylate).

[0050] More preferably, the amount of the catalyst is less than 2% by weight of the monomer. When the amount of the catalyst exceeds 2% (w), the rate of side reactions is accelerated, resulting in a sharp decrease in the selectivity of the reaction.

[0051] The vinyl ether is selected from at least one of 2-hydroxyethyl vinyl ether, 3-hydroxypropyl vinyl ether and di(poly)ethylene glycol monovinyl ether.

[0052] The monofunctional (meth)acrylate is a compound having one (meth)acryloyl group in the molecule, such as the general formula (I):

[0053]

[0054] In formula (I), R 1 represents a hydrogen atom or a methyl group, R 2 It represents a saturated alkyl group having 1 to 3 carbon atoms.

[0055] The monofunctional (meth)acrylate is selected from at least one of methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, and isopropyl (meth)acrylate. More preferably, the monofunctional (meth)acrylate is selected from at least one of methyl methacrylate and ethyl acrylate.

[0056] The molar ratio of the vinyl ether to the monofunctional (meth)acrylate is 1:(1-5); an excess amount of (meth)acrylate is more conducive to the reaction proceeding in the direction of generating products.

[0057] Wherein, the polymerization inhibitor is selected from at least one of 2,6-di-tert-butylphenol, 2,4-di-tert-butylphenol, 2-tert-butyl-4,6-dimethylphenol, alkylated diphenylamine, N,N'-diphenyl-p-phenylenediamine, phenothiazine, 4-hydroxy-2,2,6,6-tetramethylpiperidine, 4-benzoyloxy-2,2,6,6-tetramethylpiperidine, 1,4-dihydroxy-2,2,6,6-tetramethylpiperidine, 1-hydroxy-4-benzoyloxy-2,2,6,6-tetramethylpiperidine, hydroquinone, methoxyhydroquinone, and benzoquinone. More preferably, the polymerization inhibitor is selected from at least one of phenothiazine, hydroquinone, methoxyhydroquinone, and benzoquinone.

[0058] The dosage of the polymerization inhibitor is 200-1000 ppm. During the reaction, too little polymerization inhibitor will lead to partial polymerization of the reactants, making the polymerization inhibition effect insignificant. Too much polymerization inhibitor will affect the color of the product.

[0059] like Figure 1 As shown, the continuous reaction system of step (1) includes a fixed bed reactor and a vacuum device. The fixed bed reactor 1 has a feed port, a discharge port, a heating medium port, a heating chamber, a drain port and an inner tube, and a molecular sieve pervaporation membrane connected to the drain port is provided in the inner tube. In step (1), steam is injected into the heating chamber through the heating medium port to heat the inner tube of the fixed bed reactor to 80-90°C, so that the reaction materials in the inner tube stay at this temperature for 3-10 minutes, and the ester exchange reaction occurs under the catalysis of the catalyst; the water molecules and small molecule alcohols produced in the reaction are removed through the molecular sieve pervaporation membrane under the traction of the vacuum formed by the vacuum machine 2, and discharged through the drain port connected to the molecular sieve pervaporation membrane, thereby realizing continuous catalytic ester exchange and waste removal, without the need for neutralization and water washing.

[0060] The initial product obtained by the reaction of step (1) flows into the multi-stage molecular distillation equipment described in step (2) under vacuum traction. The molecular distillation equipment in step (2) can be set up as a single-stage, double-stage or triple-stage molecular distillation system. When a double-stage or triple-stage molecular distillation system is used, a flow controller and a temperature control device are provided between each molecular distillation system.

[0061] like Figure 1 As shown, each stage of molecular distillation system is equipped with a basic preheater 3, a preheating kettle 4, a scraping motor 5, a reactor 6, a vacuum machine 2, a light component receiving tank 7, a heavy component receiving tank 8, and a cold trap 9. A heat transfer oil inlet and a heat transfer oil outlet are arranged on the outside of the preheating kettle 4 and the reactor 6. When the preheater 3 is working, the heat transfer oil enters from the heat transfer oil inlet and is discharged from the heat transfer oil outlet to heat the preheating kettle 4 and the reactor 6.

[0062] When a two-stage or three-stage molecular distillation system is used, the purification of the difunctional (meth) acrylate is to collect the heavy component sample obtained by the previous stage molecular distillation, perform the next stage molecular distillation, repeatedly collect the heavy component sample, and obtain a high-purity difunctional (meth) acrylate finished product after multiple stages of molecular distillation. Preferably, a flow controller and a rotor flowmeter are set between the previous stage heavy component receiving tank and the next stage molecular distillation system. When the previous stage heavy component receiving tank accumulates to a certain amount, the flow controller and the rotor flowmeter are turned on, and the previous stage heavy components enter the next stage molecular distillation system.

[0063] The temperature control devices arranged between the molecular distillation systems at each level are respectively connected to the upper-level heavy component receiving tank and the lower-level molecular distillation system through pipelines.

[0064] The flow rate of the rotor flowmeter between the upper-stage heavy component receiving tank and the lower-stage molecular distillation system is controlled at 800-2000ml / min.

[0065] The reactor temperature range of the difunctional (meth)acrylate purification reaction in step (2) is 30-60°C, and the vacuum is 10-1000Pa. The reaction materials stay at this temperature and vacuum for 3-10 minutes to ensure that the excess raw materials are separated in time. Specifically, when a three-stage molecular distillation system is used, the first-stage molecular distillation can be used to separate the excess monofunctional (meth)acrylate, the temperature is 30-35°C, and the vacuum is 800-1000Pa; the second-stage molecular distillation removes the residual ether compounds, the temperature is controlled at 40-50°C, and the vacuum is 200-300Pa; the third-stage molecular distillation distills and recovers the product to separate it from the solid catalyst, the temperature is 50-60°C, and the vacuum is 10-50Pa.

[0066] The residence time of the product purification reaction in each stage of the molecular distillation system is consistent with the residence time of the reaction in the fixed bed reactor to ensure the continuity of the reaction.

[0067] Example 1

[0068] 6.1 g of PbTiO 3 ·SO 4 2-Uniformly immobilized in a fixed bed reactor, 211.3g of diethylene glycol monovinyl ether as phase A, 400.0g of ethyl methacrylate and 0.17g of phenothiazine are uniformly mixed as phase B, and are pumped into the inner cylinder of the fixed bed reactor of the continuous reaction system. Steam is introduced through the heating medium port to heat the inner cylinder to 80°C, so that the reaction materials in the inner cylinder stay at this temperature for 10 minutes, and the ester exchange reaction occurs with the catalysis of the catalyst. The water molecules and small molecule ethanol produced in the reaction are removed through the molecular sieve pervaporation membrane under the traction of vacuum, and discharged through the drain port connected to the molecular sieve pervaporation membrane. The crude reaction product flows into the three-stage molecular distillation system under the traction of vacuum, and the heavy component flows into the reactor of the first-stage molecular distillation system with a flow rate of 1200ml / min, and the temperature is maintained at 30°C and the vacuum degree is maintained at 1000Pa. The reaction material stays at this temperature and vacuum degree for 10 minutes. The heavy components obtained by distillation in the first-stage molecular distillation system flow into the second-stage molecular distillation system at a flow rate of 1200 ml / min, with the temperature maintained at 40°C and the vacuum maintained at 300 Pa. The reaction materials stay at this temperature and vacuum for 10 minutes. The heavy components obtained by distillation in the second-stage molecular distillation system flow into the third-stage molecular distillation system at a flow rate of 1200 ml / min, with the temperature maintained at 50°C and the vacuum maintained at 50 Pa. They stay at this temperature and vacuum for 10 minutes. The heavy components obtained by distillation in the three-stage molecular distillation system are high-purity difunctional (meth) acrylate products; the infrared spectrum of the obtained difunctional (meth) acrylate (2-vinyloxyethoxyethyl acrylate) product is shown in Figure 2 As shown; by gas chromatography ( Figure 3 ) detection, the purity of the difunctional (meth)acrylate product reached more than 99%.

[0069] Example 2

[0070] 6.1 g of PbTiO 3 ·SO 4 2-Uniformly immobilized in a fixed bed reactor, 211.3g of diethylene glycol monovinyl ether as phase A, 400.0g of ethyl methacrylate and 0.17g of phenothiazine are uniformly mixed as phase B, and are pumped into the inner cylinder of the fixed bed reactor of the continuous reaction system. Steam is introduced through the heating medium port to heat the inner cylinder of the reactor to 80°C, so that the reaction materials in the inner cylinder stay at this temperature for 8 minutes, and the ester exchange reaction occurs with the catalysis of the catalyst. The water molecules and small molecule ethanol produced in the reaction are removed through the molecular sieve pervaporation membrane under the traction of vacuum, and discharged through the drain port connected to the molecular sieve pervaporation membrane. The crude reaction product flows into the three-stage molecular distillation system under the traction of vacuum, and the heavy component flows into the reactor of the first-stage molecular distillation system with a flow rate of 1200ml / min, and the temperature is maintained at 30°C and the vacuum degree is maintained at 1000Pa. The reaction material stays at this temperature and vacuum degree for 8 minutes. The heavy components obtained by distillation of the first-stage molecular distillation system flow into the second-stage molecular distillation system at a flow rate of 1200 ml / min, with the temperature maintained at 40°C and the vacuum maintained at 300 Pa, and the reaction materials stay at this temperature and vacuum for 8 minutes. The heavy components obtained by distillation of the second-stage molecular distillation system flow into the third-stage molecular distillation system at a flow rate of 1200 ml / min, with the temperature maintained at 50°C and the vacuum maintained at 50 Pa, and stay at this temperature and vacuum for 8 minutes. The heavy components obtained by distillation of the three-stage molecular distillation system are high-purity difunctional (meth) acrylate products; the purity of the difunctional (meth) acrylate products reaches more than 98% through testing.

[0071] Example 3

[0072] 6.1 g of PbTiO 3 ·SO 4 2- Uniformly immobilized in a fixed bed reactor, 211.3g of diethylene glycol monovinyl ether as phase A, 400.0g of ethyl methacrylate and 0.17g of phenothiazine are uniformly mixed as phase B, and are pumped into the inner cylinder of the continuous fixed bed reactor respectively. Steam is introduced through the heating medium port to heat the inner cylinder to 80°C, so that the reaction materials in the inner cylinder stay at this temperature for 10 minutes, and the ester exchange reaction occurs with the catalysis of the catalyst. The water molecules and small molecule ethanol produced in the reaction are removed through the molecular sieve pervaporation membrane under the traction of vacuum, and discharged through the drain port connected to the molecular sieve pervaporation membrane. The crude reaction product flows into the single-stage molecular distillation system under the traction of vacuum, and flows into the reactor with a temperature maintained at 50°C and a vacuum maintained at 1000Pa at a flow rate of 1200ml / min. The reaction materials stay at this temperature and vacuum for 10 minutes, and the heavy component obtained by distillation is the difunctional (meth) acrylate product; the purity of the difunctional (meth) acrylate product is detected to be more than 94%.

[0073] Comparative Example 1

[0074] 211.3 g of diethylene glycol monovinyl ether, 400.0 g of ethyl methacrylate, 0.17 g of phenothiazine and 5.5 g of PbTiO 3 ·SO 4 2- The reaction kettle was put into the distillation tower. The reaction kettle was stirred and mixed and heated to 220°C, stirred for 8 hours, and the unreacted materials and the generated by-product ethanol were discharged from the top of the tower to the outside of the reaction system under reduced pressure, and the final product was obtained from the top of the tower. According to the detection, the purity of 2-vinyloxyethoxy ethyl acrylate was 91%.

[0075] It will be apparent to those skilled in the art that the present invention is not limited to the details of the exemplary embodiments described above and that the present invention can be implemented in other specific forms without departing from the spirit or essential features of the present invention. Therefore, the embodiments should be considered exemplary and non-restrictive in all respects, and the scope of the present invention is defined by the appended claims rather than the above description, and it is intended that all changes falling within the meaning and scope of the equivalent elements of the claims be included in the present invention.

[0076] In addition, it should be understood that although the present specification is described according to implementation modes, not every implementation mode contains only one independent technical solution. This description of the specification is only for the sake of clarity. Those skilled in the art should regard the specification as a whole. The technical solutions in each embodiment may also be appropriately combined to form other implementation modes that can be understood by those skilled in the art.

Claims

1. A high-purity continuous preparation method of a difunctional (meth)acrylate, characterized in that: The following steps are involved: (1) A vinyl ether containing a double bond is used as phase A, and a monofunctional (meth)acrylate and a polymerization inhibitor are uniformly mixed as phase B, and the two are respectively pumped into a continuous reaction system, and the catalyst is uniformly immobilized in a fixed bed reactor in the continuous reaction system; in the process of gradually heating to a certain temperature, the materials form a flowing homogeneous liquid and a catalytic transesterification reaction occurs to obtain a reaction product; (2) The reaction product obtained in step (1) is flowed into a molecular distillation device for purification, and the raw material in an amount equal to that in step (1) is continuously pumped in to finally obtain a high-purity bifunctional (meth)acrylate.

2. The high-purity continuous preparation method of a bifunctional (meth)acrylate according to claim 1, characterized in that: The catalyst is a bimetallic composite material modified by sulfuric acid, and the chemical formula is XMO3·SO4 2- , wherein X is selected from any one of lithium, sodium, potassium, magnesium, zinc, lead and barium; and M is selected from one of titanium and nickel.

3. The high-purity continuous preparation method of a bifunctional (meth)acrylate according to claim 1, characterized in that: The amount of the catalyst used is 0.8% to 3% of the total mass of the double-bond-containing vinyl ether and the monofunctional (meth)acrylate monomer.

4. The high-purity continuous preparation method of a bifunctional (meth)acrylate according to claim 1, characterized in that: The vinyl ether is selected from at least one of 2-hydroxyethyl vinyl ether, 3-hydroxypropyl vinyl ether and di(poly)ethylene glycol monovinyl ether.

5. The high-purity continuous preparation method of a bifunctional (meth)acrylate according to claim 1, characterized in that: The monofunctional (meth)acrylate is at least one selected from methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, and isopropyl (meth)acrylate.

6. The high-purity continuous preparation method of a bifunctional (meth)acrylate according to claim 1, characterized in that: The molar ratio of the vinyl ether to the monofunctional (meth)acrylate is 1:(1-5).

7. The high-purity continuous preparation method of a bifunctional (meth)acrylate according to claim 1, characterized in that: The fixed bed reactor comprises a feed port, a discharge port, a heating medium port, a heating chamber, a drain port and an inner cylinder, wherein a molecular sieve pervaporation membrane connected to the drain port is arranged in the inner cylinder; water molecules and small molecular alcohols generated in the reaction are removed through the molecular sieve pervaporation membrane under the traction of vacuum.

8. The high-purity continuous preparation method of a bifunctional (meth)acrylate according to claim 1, characterized in that: In step (1), steam is injected into the fixed bed reactor and heated to 80-90° C., so that the reaction materials in the fixed bed reactor undergo an ester exchange reaction under the catalytic action of the catalyst at this temperature.

9. The high-purity continuous preparation method of a bifunctional (meth)acrylate according to claim 1, characterized in that: The temperature range of the reactor of the molecular distillation equipment is 30-60° C., and the vacuum pressure is 10-1000 Pa.

10. The high-purity continuous preparation method of a bifunctional (meth)acrylate according to claim 1, characterized in that: The residence time of the product after the reaction in the molecular distillation equipment for purification is consistent with the residence time of the reaction in the fixed bed reactor to ensure the continuity of the reaction.