Aromatic skeleton diurea nucleating agent containing methylene furan, heat-resistant polylactic acid composition and preparation method of heat-resistant polylactic acid composition

The diurea nucleating agent containing methylene furan aromatic skeleton prepared through the "one-pot two-step" method of non-isocyanate raw materials and furfurylamine solves the problems of environmental pollution and complexity in the preparation process of polylactic acid nucleating agent, and significantly improves its Crystallization temperature and heat resistance, achieving a more efficient nucleation effect.

CN118772084AActive Publication Date: 2024-10-15YINGKOU KANGHUI PETROCHEM +1
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202410770205.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-14
Publication Date
2024-10-15
Estimated Expiration
2044-06-14

AI Technical Summary

Technical Problem

The existing polylactic acid nucleating agent preparation process has environmental pollution and complexity problems, and the existing nucleating agent is not effective in improving the crystallinity of polylactic acid, affecting its heat resistance.

Method used

Using non-isocyanates as raw materials, the aromatic skeleton diurea nucleating agent containing methylene furan was prepared through the "one-pot two-step" method of furfurylamine, and combined with polylactic acid for preparation, which significantly improved its crystallization temperature and heat resistance.

Benefits of technology

It significantly improves the crystallization temperature and heat resistance of polylactic acid, solves the problem of non-environmental protection of the nucleating agent preparation process, simplifies the process flow, and achieves a more efficient nucleation effect.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118772084A_ABST
    Figure CN118772084A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of high polymer materials, and particularly relates to an aromatic skeleton diurea nucleating agent containing methylene furan, a heat-resistant polylactic acid composition and a preparation method of the heat-resistant polylactic acid composition. According to the invention, a green route taking non-isocyanate as a raw material is adopted, and a series of methylene furan-containing aromatic skeleton diurea polylactic acid nucleating agents are prepared by a biomass-sourced furfuryl amine'one-pot two-step 'method. In the polylactic acid composition, the mass content ratio of polylactic acid to the nucleating agent is 100: (0.1-5). The preparation method comprises the following steps: mixing the dried polylactic acid and the aromatic skeleton diurea nucleating agent containing methylene furan at 150-220 DEG C for 3-15 minutes by using a double-screw internal mixer, thereby obtaining the polylactic acid / methylene furan-containing aromatic skeleton diurea nucleating agent. The crystallization rate and crystallinity of the polylactic acid composition modified by the nucleating agent are remarkably improved, the heat resistance is further enhanced, and the polylactic acid composition has a good industrial prospect.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of polymer materials, and in particular relates to a methylene furan-containing aromatic skeleton diurea nucleating agent, a heat-resistant polylactic acid composition and a preparation method thereof. Background Art

[0002] Seeking sustainable alternatives to traditional petroleum-based plastics is an effective way to deal with the depletion of petroleum resources and reduce environmental pollution. To meet this urgent need in the market, biodegradable plastics extracted from renewable resources have become a promising solution. Among various biodegradable plastics, polylactic acid (PLLA) stands out due to its excellent comprehensive properties. Polylactic acid is derived from renewable resources, has good biodegradability and compatibility, and can be widely used in packaging materials and consumer products.

[0003] However, polylactic acid has obvious defects in heat resistance (Tg = 50-60°C), which is mainly due to its relatively low crystallinity. Therefore, it is crucial to improve the crystallinity of polylactic acid. Modification from the chemical structure and processing technology (such as biaxial stretching, etc.) are two aspects to improve the crystallinity of polylactic acid. Among various modification methods, adding nucleating agents (NAs) is a simple method to accelerate the crystallization rate of polylactic acid. Adding nucleating agents can provide nucleation sites, reduce the nucleation energy barrier, promote rapid crystallization and increase crystallinity. The nucleating agents of polylactic acid can be divided into two categories: inorganic nucleating agents and organic nucleating agents. Inorganic nucleating agents usually include talc, montmorillonite, carbon black, apatite, etc., but the nucleating effect of such nucleating agents is poor. When added in small amounts, the nucleating effect is not obvious. When the content is high, it is easy to make the product brittle, affecting the use effect.

[0004] At present, some patents have disclosed nucleating agents for polylactic acid. For example, the Chinese invention patent with application publication number CN114634617A discloses an organic polylactic acid nucleating agent formed by the polymerization of lactide initiated by hexamethylol melamine, wherein the molecular chain end forms an ester bond with one of the carboxyl groups in the carboxylate group, and the other carboxyl groups and metal cations form ionic bonds. However, the preparation process of this type of nucleating agent that needs to participate in the polymerization of polylactic acid is very complicated, and the raw material melamine has problems such as poor solubility, which is obviously unfavorable for the industrialization of polylactic acid modification additives. For example, the Chinese patent with application publication number CN102634180A discloses a class of polylactic acid nucleating agents containing one or two urea bonds, but the isocyanate obtained by using phosgene to prepare it as a raw material has environmental pollution problems. Therefore, how to use biomass raw materials to develop a green and environmentally friendly nucleating agent and its preparation process route with simple preparation process, especially to develop a class of green and environmentally friendly high-efficiency nucleating agents and preparation methods suitable for polylactic acid, is a technical problem to be solved urgently. Summary of the invention

[0005] In order to solve the environmental pollution problem of the preparation of polylactic acid nucleating agents in the prior art, the present application provides a class of aromatic skeleton diurea nucleating agents containing methylene furan, a heat-resistant polylactic acid composition and a preparation method thereof. Among them, the aromatic skeleton diurea nucleating agent containing methylene furan adopts a green route of non-isocyanate as raw material, and is prepared by a "one-pot two-step" method of furfurylamine from biomass, which can significantly improve the crystallization temperature, crystallization rate and heat resistance of polylactic acid.

[0006] In a first aspect, the present invention provides a method for preparing a type of methylene furan-containing aromatic skeleton diurea nucleating agent, which mainly comprises the following steps:

[0007] S1. Under the protection of inert gas, add furfurylamine, N,N'-carbonyldiimidazole and ether solvent into the reactor, and stir the reaction at 20-35°C for 1-4h;

[0008] S2, continue to add aromatic diamine with a benzene ring skeleton therein, react for 3 to 8 hours, and obtain the aromatic skeleton diurea nucleating agent containing methylene furan after separation and purification.

[0009] Furthermore, the molar ratio of furfurylamine to N,N'-carbonyldiimidazole is 1:1 to 1.2.

[0010] Furthermore, the molar ratio of the aromatic diamine to furfurylamine is 1:2 to 2.2.

[0011] Furthermore, the ether solvent is at least one of diethyl ether, dipropyl ether, diisopropyl ether, ethyl butyl ether, dibutyl ether, dipentyl ether, tetrahydrofuran, 3-methylfuran, diisopentyl ether, dioxolane, 1,4-dioxane, 1,4-dichlorohexane, and ethylene chloride.

[0012] Furthermore, the aromatic diamine is selected from at least one of p-phenylenediamine and m-phenylenediamine.

[0013] Furthermore, the inert gas is nitrogen or argon.

[0014] The specific synthetic route of the above preparation method is as follows:

[0015]

[0016] in, is p-phenylenediamine or m-phenylenediamine, The specific corresponding

[0017]

[0018] In a second aspect, the present invention provides a type of methylene furan-containing aromatic skeleton diurea nucleating agent prepared by the above method, the structural formula of which is as follows:

[0019]

[0020] In a third aspect, the present invention provides a heat-resistant polylactic acid composition, which comprises, by weight, 100 parts of polylactic acid and 0.1 to 5 parts of an aromatic skeleton diurea nucleating agent containing methylene furan.

[0021] Furthermore, the heat-resistant polylactic acid composition comprises, by weight, 100 parts of polylactic acid and 1 to 2 parts of a diurea nucleating agent having an aromatic skeleton containing methylene furan.

[0022] In a fourth aspect, the present invention provides a method for preparing a heat-resistant polylactic acid composition, the specific steps of which are:

[0023] (1) weighing polylactic acid and a diurea nucleating agent containing methylene furan in proportion and drying them in a vacuum oven at 50 to 80° C. for 8 to 24 hours, and then premixing them;

[0024] (2) placing the mixed material in an internal mixer at a mixing temperature of 160 to 220° C., a mixing time of 3 to 15 minutes, and a rotor speed of 15 to 50 rpm to obtain the heat-resistant polylactic acid composition.

[0025] Beneficial effects:

[0026] The methylene furan-containing aromatic skeleton diurea nucleating agent prepared by the present invention adopts a green synthesis route using non-isocyanate as a raw material, and is prepared by a "one-pot two-step" method of furfurylamine from biomass, which not only solves the problem that the nucleating agent synthesis process in the prior art is not environmentally friendly, but also the prepared methylene furan-containing aromatic skeleton diurea nucleating agent can significantly improve the crystallization temperature, crystallization rate and heat resistance of polylactic acid. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 The synthetic route of dimethylene furanyl phenylurea in the embodiment;

[0028] Figure 2 is the methylene furanyl phenylene diurea in Example 1 1 H-NMR spectrum;

[0029] Figure 3 It is the DSC cooling curve diagram of Example 4 and Example 1-3. DETAILED DESCRIPTION

[0030] In order to more clearly understand the above-mentioned objectives, features and advantages of the present invention, the scheme of the present invention will be further described below. It should be noted that the embodiments of the present invention and the features in the embodiments can be combined with each other without conflict.

[0031] In the following description, many specific details are set forth to facilitate a full understanding of the present invention, but the present invention may also be implemented in other ways different from those described herein; it is obvious that the embodiments in the specification are only part of the embodiments of the present invention, rather than all of the embodiments.

[0032] The preferred embodiments of the present invention will be described in detail below in conjunction with examples. It should be understood that the following examples are provided only for the purpose of illustration and are not intended to limit the scope of the present invention. Those skilled in the art may make various modifications and substitutions to the present invention without departing from the purpose and spirit of the present invention.

[0033] Test instrument model: The nuclear magnetic resonance spectrometer used was Bruker AVANCE III 500 (Bruker, Switzerland), and the differential scanning calorimeter used was DSC 25 (TA, USA).

[0034] Example 1 (Preparation of an aromatic skeleton diurea nucleating agent containing methylene furan, dimethylene furan phenylene diurea)

[0035] The round-bottomed reaction flask equipped with a magnetic rod was baked in advance, evacuated with nitrogen three times, and then a tetrahydrofuran solution containing 6.482g (40mmol) N,N'-carbonyldiimidazole and 3.882g (40mmol) furfurylamine were added in sequence under a nitrogen atmosphere. After reacting for 2 hours under vigorous stirring at 25°C, 2.16g (20mmol) 1,4-p-phenylenediamine was added and reacted for 6 hours. After the reaction was completed, the filter was filtered, the filter cake was washed once with tetrahydrofuran, and the filter cake was washed once with anhydrous ethanol. After drying, 6.94g of white powder was obtained, which was an aromatic skeleton diurea nucleating agent containing methylene furan, with a yield of 95.6%. The synthetic route is shown in FIG. Figure 1 .

[0036] The product was characterized by H NMR spectroscopy. Figure 2 .

[0037] Example 2 (Preparation of nucleating agent used in comparative example, dimethylene pyridine phenylene diurea)

[0038] The round-bottomed reaction flask equipped with a magnetic rod was baked in advance, evacuated with nitrogen three times, and then a tetrahydrofuran solution containing 6.482g (40mmol) N, N'-carbonyldiimidazole and 4.33g (40mmol) 2-aminomethylpyridine were added in sequence under a nitrogen atmosphere. After reacting for 2 hours under vigorous stirring at 25°C, 2.16g (20mmol) 1,4-p-phenylenediamine was added and reacted for 6 hours. After the reaction was completed, the filter cake was filtered, washed once with tetrahydrofuran, and once with anhydrous ethanol, and 7.25g of white powder was obtained after drying, which was the nucleating agent, with a yield of 96.4%.

[0039] Example 3 (Preparation of nucleating agent used in comparative example, dibenzyl p-phenylenediurea)

[0040] The round-bottomed reaction flask equipped with a magnetic rod was baked in advance, evacuated with nitrogen three times, and then a tetrahydrofuran solution containing 6.482g (40mmol) N,N'-carbonyldiimidazole and 4.28g (4.0mmol) benzylamine were added in sequence under a nitrogen atmosphere. After reacting for 2 hours under vigorous stirring at 25°C, 2.16g (20mmol) 1,4-p-phenylenediamine was added and reacted for 6 hours. After the reaction was completed, the filter cake was filtered, washed once with tetrahydrofuran, and once with anhydrous ethanol, and 7.04g of white powder was obtained after drying, which was the nucleating agent, with a yield of 92.0%.

[0041] Example 4 (polylactic acid blending)

[0042] The nucleating agent dimethylene furan phenylene urea and polylactic acid prepared in Example 1 were dried in a vacuum oven at 60°C for 12 hours. 60g of polylactic acid and 0.18g of nucleating agent were mixed in a ziplock bag in advance, and then placed in a SU-70B micro-internal mixer for melt mixing. The melt temperature of the internal mixer and the temperatures of the three temperature control zones were set to 180°C, 179°C, 178°C and 175°C, respectively, and the rotor speed was set to 15rpm. According to the DSC non-isothermal crystallization test, the crystallization temperature was 105.6°C and the crystallization peak enthalpy was 32.7J / g.

[0043] Example 5 (polylactic acid blending)

[0044] The nucleating agent dimethylene furan phenylene urea and polylactic acid prepared in Example 1 were dried in a vacuum oven at 60°C for 12 hours. 60g of polylactic acid and 0.06g of nucleating agent were mixed in a ziplock bag in advance, and then placed in a SU-70B micro-internal mixer for melt mixing. The melt temperature of the internal mixer and the temperatures of the three temperature control zones were set to 180°C, 179°C, 178°C and 175°C, respectively, and the rotor speed was set to 15rpm. According to the DSC non-isothermal crystallization test, the crystallization temperature was 98.2°C and the peak enthalpy of crystallization was 22.7J / g.

[0045] Comparative Example 1 (polylactic acid blending)

[0046] The comparative nucleating agent dimethylenepyridine phenylene diurea and polylactic acid prepared in Example 2 were dried in a vacuum oven at 60°C for 12 hours. 60g of polylactic acid and 0.18g of nucleating agent were mixed in a ziplock bag in advance, and then placed in a SU-70B micro-internal mixer for melt mixing. The melt temperature of the internal mixer and the temperatures of the three temperature control zones were set to 180°C, 179°C, 178°C and 175°C, respectively, and the rotor speed was set to 15rpm. According to the DSC non-isothermal crystallization test, the crystallization temperature was 99.1°C and the peak enthalpy of crystallization was 26.4J / g.

[0047] Comparative Example 2 (polylactic acid blending)

[0048] The comparative nucleating agent dibenzyl paraphenylene diurea and polylactic acid prepared in Example 3 were dried in a vacuum oven at 60°C for 12 hours. 60g of polylactic acid and 0.18g of nucleating agent were mixed in a ziplock bag in advance, and then placed in a SU-70B micro-internal mixer for melt mixing. The melt temperature of the internal mixer and the temperatures of the three temperature control zones were set to 180°C, 179°C, 178°C and 175°C, respectively, and the rotor speed was set to 15rpm. According to the DSC non-isothermal crystallization test, the crystallization temperature was 96.8°C and the peak enthalpy of crystallization was 16.3J / g.

[0049] Comparative Example 3 (polylactic acid mixing)

[0050] The polylactic acid was dried in a vacuum oven at 60°C for 12 hours. 60 g of polylactic acid was placed in a SU-70B micro-internal mixer for melt mixing. The melt temperature and the temperatures of the three temperature control zones of the internal mixer were set to 180°C, 179°C, 178°C and 175°C, respectively, and the rotor speed was set to 15 rpm. After DSC non-isothermal crystallization test, no crystallization peak was observed on the cooling curve.

[0051] It can be seen from the above examples and comparative examples that the 2-methylene furan-terminated aromatic skeleton diurea nucleating agent of the present application has a better nucleating effect on polylactic acid (such as Figure 3 ). Its crystallization temperature and crystallization enthalpy have been greatly improved compared with the original ones, indicating that the degree of crystallization has been improved.

Claims

1. A method for preparing a type of aromatic skeleton diurea nucleating agent containing methylene furan, characterized in that: The steps include: S1. Under the protection of inert gas, add furfurylamine, N,N'-carbonyldiimidazole and ether solvent into the reactor, and stir the reaction at 20-35°C for 1-4h; S2, continue to add aromatic diamine thereto, react for 3 to 8 hours, and obtain the aromatic skeleton diurea nucleating agent containing methylene furan after separation and purification.

2. The preparation method according to claim 1, characterized in that: The molar ratio of furfurylamine to N,N'-carbonyldiimidazole is 1:1-1.

2.

3. The preparation method according to claim 2, characterized in that: The molar ratio of the aromatic diamine to furfurylamine is 1:2 to 2.

2.

4. The preparation method according to claim 3, characterized in that: The ether solvent is at least one of diethyl ether, dipropyl ether, diisopropyl ether, ethyl butyl ether, dibutyl ether, dipentyl ether, tetrahydrofuran, 3-methylfuran, diisopentyl ether, dioxolane, 1,4-dioxane, 1,4-dichlorohexane and ethylene chloride.

5. The preparation method according to claim 3, characterized in that: The aromatic diamine is selected from p-phenylenediamine or m-phenylenediamine.

6. A heat-resistant polylactic acid composition, characterized in that: The invention comprises, by weight, 100 parts of polylactic acid and 0.1 to 5 parts of an aromatic skeleton diurea nucleating agent containing methylene furan; the aromatic skeleton diurea nucleating agent containing methylene furan is obtained by the preparation method as described in any one of claims 1 to 5, and has the structural formula:

7. The heat-resistant polylactic acid composition according to claim 6, characterized in that: The invention comprises, by weight, 100 parts of polylactic acid and 1 to 2 parts of an aromatic skeleton diurea nucleating agent containing methylene furan.

8. A method for preparing a heat-resistant polylactic acid composition according to any one of claims 6 or 7, characterized in that: The dried polylactic acid and the aromatic skeleton diurea nucleating agent containing methylene furan are premixed in proportion, and then the mixture is placed in an internal mixer for internal mixing to obtain the heat-resistant polylactic acid composition.

9. The preparation method according to claim 8, characterized in that: The mixing temperature is 160-220°C, the mixing time is 3-15 minutes, and the rotor speed is 15-50 rpm.

10. A type of aromatic skeleton diurea nucleating agent containing methylene furan, characterized in that: The structural formula of the aromatic skeleton diurea nucleating agent containing methylene furan is: The methylene furan-containing aromatic skeleton diurea nucleating agent is prepared by the preparation method described in any one of claims 1 to 5.

Citation Information

Patent Citations

  • Biodegradable resin compositions and molded objects thereof

    CN101080465A

  • Ureas nucleating agent-containing polylactic acid composite and preparation method thereof

    CN102634180A

  • Polylactic resin composition, polylactic resin molding and method for producing polylactic resin molding

    JP2017110122A

  • Arylene-bis-(2-aminothiophene-3-carbonitrile(s) as monomers for preparing polyamides, polyisomethines and polyureas with phenylene groups

    RU2230743C1

  • Ink composition containing a particular type of dye, and corresponding ink jet printing process

    US20030209166A1