General short-oil soybean oil alkyd resin as well as preparation method and application thereof

Short oil soybean oil alkyd resin is directly synthesized by the melting method, taking advantage of the difference in esterification and alcoholysis reaction rates to omit the alcoholysis step, solving the problems of waste and high energy consumption in the existing technology, and achieving the production of clear and transparent resin with excellent performance Same as fatty acid method.

CN118772385APending Publication Date: 2024-10-15JIANGSU SANMU GRP CORP +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410897990.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-05
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

The existing alcoholysis process of short oil soybean oil alkyd resin has problems of waste and high energy consumption, and often uses a two-step method, which increases the difficulty of production.

Method used

The alkyd resin is directly synthesized using the melting method. Through the reaction of soybean oil, glycerol, phthalic anhydride, benzoic acid and xylene, the alcoholysis step is omitted, and the difference in the rates of esterification reaction and alcoholysis reaction is used to achieve the formation of clear and transparent resin.

Benefits of technology

Direct synthesis without alcoholysis step is achieved, and the resin properties are the same as those of the fatty acid method, including dryness, gloss, hardness, impact strength and flexibility, reducing energy consumption and production difficulty.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004929630730000041
    Figure BDA0004929630730000041
Patent Text Reader

Abstract

The invention discloses general short-oil soybean oil alkyd resin and a preparation method thereof. The general short-oil soybean oil alkyd resin is prepared from the following raw materials in parts by mass: 166-174 parts of soybean oil, 200-210 parts of glycerol, 293-307 parts of phthalic anhydride, 68-72 parts of benzoic acid, 1-1.5 parts of a color reducing agent, 20-30 parts of reflux xylene and 270-280 parts of an organic solvent. Various reaction raw material compositions and specific reaction steps are screened out through a large number of experiments, particularly, the difference of the rate difference of alcoholysis reaction and esterification reaction in a melting method and a solvent method is found, and the reaction system becomes a homogeneous system by adopting the melting method and simultaneously adopting the matching of glycerol and benzoic acid. The clear and transparent qualified alkyd resin is directly prepared without an alcoholysis step on the premise that the alkyd resin is produced by using the whole soybean oil, and the properties such as dryness, gloss, hardness, impact strength and flexibility of the resin are the same as those of the alkyd resin prepared by using a fatty acid method, so that the situation that the alcoholysis step is not needed by using the whole soybean oil and the alkyd resin prepared by using the fatty acid method is created. The method is the precedent of directly synthesizing the alkyd resin, and has important application value.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a general short-oil soybean oil alkyd resin and a preparation method thereof. Background Art

[0002] General short-oil soybean oil alkyd resin is mainly used for nitro lacquer, alkyd polyurethane paint and alkyd amino baking varnish, with a wide range of applications and large market demand. There are two main methods for manufacturing alkyd resin. One is the fatty acid method, which directly esterifies polyols, polyacids and fatty acids to produce alkyd resins. Fatty acids can act as solvents for polyols and phthalic anhydride, that is, esterification is completed in a homogeneous system, and the process is relatively simple. The other is the alcoholysis method, which first mixes vegetable oil (except castor oil containing hydroxyl groups) and polyols and heats them to between 240℃ and 250℃, adds an alcoholysis catalyst for alcoholysis reaction, generates incomplete esters of polyols, and then adds phthalic anhydride for esterification reaction.

[0003] Short oil resin has low oil content. If alcoholysis is used, the first step of feeding is too little, accounting for only about 30% of the reactor volume, and the upper 70% of the reactor volume is heated dry without material, resulting in waste; and alcoholysis is a two-step process. After the alcoholysis is completed, the temperature must be lowered to add phthalic anhydride, the remaining polyols and reflux xylene, and then the temperature must be raised to reflux for esterification, which adds a cooling and heating process, increasing energy consumption and production difficulty. The method for manufacturing soybean oil modified alkyd resin disclosed in patent CN201010175278.4 is a common method for alcoholysis short oil alkyd resin, which adopts a two-step method, which is rarely used in actual production, and generally adopts the fatty acid method. Summary of the invention

[0004] Purpose of the invention: The purpose of the present invention is to provide a general short-oil soybean oil alkyd resin and a preparation method thereof. The present invention does not require an alcoholysis step and directly prepares a clear and transparent qualified alkyd resin. The dryness, gloss, hardness, impact strength and flexibility of the resin are the same as those of the alkyd resin produced by the fatty acid method. The present invention creatively uses whole soybean oil without the alcoholysis step to directly synthesize an alkyd resin, which has important application value.

[0005] Technical solution: In order to achieve the above purpose, the technical solution adopted by the present invention is:

[0006] The invention discloses a general-purpose short-oil soybean oil alkyd resin, which is prepared from soybean oil, glycerin, phthalic anhydride, benzoic acid, a color reducing agent, reflux xylene and an organic solvent.

[0007] As a preferred embodiment, a general short-oil soybean oil alkyd resin is prepared from the following raw materials in parts by weight: 166-174 parts of soybean oil, 200-210 parts of glycerol, 293-307 parts of phthalic anhydride, 68-72 parts of benzoic acid, 1-1.5 parts of a color reducing agent, 20-30 parts of reflux xylene and 270-280 parts of an organic solvent.

[0008] As a preferred solution, the soybean oil mentioned above can be selected to meet the first-level quality indicators in the national standard GB / T1535-2017.

[0009] As a preferred embodiment, the above-mentioned color reducing agent is hypophosphorous acid.

[0010] As a preferred embodiment, the organic solvent is one of toluene, xylene, trimethylbenzene, ethyl acetate, dimethyl carbonate, butyl acetate, sec-butyl acetate and propylene glycol methyl ether acetate, or a mixture of any of the above.

[0011] A method for preparing a general short-oil soybean oil alkyd resin comprises the following steps:

[0012] 1) After introducing nitrogen or carbon dioxide protective gas, soybean oil, glycerin, phthalic anhydride, benzoic acid and color reducing agent are put into the reaction kettle and stirred to mix the materials evenly;

[0013] 2) Continue to introduce nitrogen or carbon dioxide protective gas and start to heat up. When the temperature rises to 145°C-150°C, turn off the nitrogen or carbon dioxide protective gas and continue to heat up to above 170°C. When keeping at 170°C-180°C, continue to heat up to above 190°C and keep between 190°C-210°C for melt esterification;

[0014] 3) When the resin changes from mixed to clear, continue to keep warm, take samples to measure the acid value and viscosity, until the acid value and viscosity are qualified, add the refluxing xylene into the reactor, continue to reflux esterification at 190℃-210℃, until the acid value and viscosity are qualified;

[0015] 4) Cool down to 160-170°C and add dilution solvent;

[0016] 5) Filter to obtain universal short oil soybean oil alkyd resin.

[0017] As a preferred embodiment, the preparation method of the above-mentioned general short-oil soybean oil alkyd resin comprises the following steps:

[0018] 1) After nitrogen or carbon dioxide protective gas is introduced for 15 to 30 minutes, soybean oil, glycerol, phthalic anhydride, benzoic acid, and color reducing agent are added to the reaction kettle and stirred to mix the materials evenly;

[0019] 2) Continue to introduce nitrogen or carbon dioxide protective gas and start to heat up. When the temperature rises to 145°C-150°C, turn off the nitrogen or carbon dioxide protective gas and continue to heat up to above 170°C, keep at 170°C-180°C for 2-3 hours, continue to heat up to above 190°C, keep between 190°C-210°C for melt esterification;

[0020] 3) When the resin changes from mixed to clear, continue to keep warm, take samples to measure the acid value and viscosity, until the acid value reaches less than 25, viscosity: 30-40 seconds * format tube / 25℃, xylene to 60 solid content, after the acid value and viscosity are qualified, put the reflux xylene into the reactor, continue to reflux esterification at 190℃-210℃, until the acid value reaches less than 10, viscosity: 90-100 seconds * format tube / 25℃, xylene to 60 solid content;

[0021] 4) Cool down to 160-170°C and add dilution solvent;

[0022] 5) After filtering, the general short oil soybean oil alkyd resin is obtained.

[0023] The present invention mainly realizes the direct synthesis of alkyd resin by whole soybean oil without the step of alcoholysis through the following points:

[0024] 1. The present invention has found in the process screening that the melting method and the solvent method have a great influence on the reaction process and results in the formulation system of the present invention. If the present invention puts soybean oil, glycerin, phthalic anhydride, benzoic acid, a color reducing agent and reflux xylene into a reactor together according to the solvent method, and directly heats up and refluxes for esterification, the resin will not be clear and will gel before forming a homogeneous phase. The present invention puts soybean oil, glycerin, phthalic anhydride, benzoic acid and a color reducing agent into a reactor together according to the melting method, slowly heats up to 190°C, and keeps the temperature between 190°C and 210°C for melting and esterification, the resin will be clear and transparent, forming a homogeneous phase, and then puts reflux xylene into the reactor, and continues to reflux and esterify between 190°C and 210°C, and the ideal resin can be obtained.

[0025] The resin of the present invention also has three main reactions at the initial stage of the reaction, A: esterification of glycerol and phthalic anhydride; D: esterification reaction of glycerol and benzoic acid; E: alcoholysis reaction of soybean oil and glycerol. In the solvent method, the water generated by esterification and xylene are azeotropically dehydrated, and the dehydration speed is fast. The esterification reaction is faster than the alcoholysis reaction speed, that is, the A and D reactions are faster than the E reaction, resulting in the insoluble matter easily generated by glycerol and phthalic anhydride being incompatible with the system, resulting in mixing and gelling. In the melting method, the water generated by esterification will only be discharged from the system in the form of vaporized water vapor, and the dehydration is relatively slow in the solvent method. The A reaction is not as fast as the solvent method, so not too much glycerol will be consumed, so that more glycerol will participate in the E reaction. The rates of the A, D and E reactions are not as different as those of the solvent method. The E reaction in the melting method is easier to carry out than the E reaction in the solvent method, so the resin is easy to form a homogeneous phase, so it is clear and transparent.

[0026] In summary, the present invention mainly discovers that the rate difference between the alcoholysis reaction and the esterification reaction is different in the melting method and the solvent method, utilizes this difference (the rate difference between the alcoholysis reaction and the esterification reaction is smaller in the melting method), and adopts the melting method to realize the direct synthesis of alkyd resin from whole soybean oil without the alcoholysis step, thereby achieving very good and unexpected technical effects.

[0027] 2. The inventors also found in previous patents that alcoholysis would be easier in the environment of monoprotic acid, and benzoic acid is better than general dry or semi-dry vegetable oil acid, but benzoic acid directly participates in alcoholysis, and benzoic acid easily sublimates and blocks the condenser. The present invention further screened and found that in the triol (glycerine, trimethylolethane, trimethylolpropane) system with a lower melting point, benzoic acid is very easy to form a homogeneous phase with the triol and is not easy to sublime. In general industrial triols, the present invention selects glycerine for use, because it is found that glycerine is easier to alcoholyze than tetraol, and can also greatly reduce the sublimation of benzoic acid.

[0028] 3. The inventors have found that the reaction of benzoic acid and triol to form triol monoester makes the alcoholysis reaction of soybean oil in the formula easier to proceed. The inventors have also found that triol monoester can make the alcoholysis reaction of soybean oil easier to proceed in the melting method, achieving a very good and unexpected technical effect.

[0029] Beneficial effects: Compared with the prior art, the present invention has the following advantages:

[0030] The invention screens out various reaction raw material compositions and specific reaction steps through a large number of experiments, and in particular finds that the rate difference between alcoholysis reaction and esterification reaction in the melting method and the solvent method is different. This difference (the rate difference between alcoholysis reaction and esterification reaction is smaller in the melting method) is utilized, and the melting method is adopted, and glycerol and benzoic acid are used to make the reaction system clear into a homogeneous system. Under the premise of using whole soybean oil to produce alkyd resin, the alcoholysis step is not required, and clear and transparent qualified alkyd resin is directly prepared. The dryness, gloss, hardness, impact strength and flexibility of the resin are the same as those of the alkyd resin produced by the fatty acid method. It has created a precedent for directly synthesizing alkyd resin using whole soybean oil without the alcoholysis step, and has important application value. DETAILED DESCRIPTION

[0031] The embodiments of the present invention are described in detail below with reference to the examples. If no specific conditions are specified in the examples, the reaction is carried out according to conventional conditions or conditions recommended by the manufacturer. If no manufacturer is specified for the reagents or instruments used, they are all conventional products that can be obtained commercially.

[0032] The raw material compositions of the following examples are shown in Table 1:

[0033] Table 1 Raw material composition of each embodiment

[0034]

[0035] 1. The preparation method of the general short-oil soybean oil alkyd resin of the present invention comprises the following steps:

[0036] 1) After nitrogen or carbon dioxide protective gas is introduced for 15 minutes, soybean oil, glycerol, phthalic anhydride, benzoic acid and a color reducing agent in the mass fractions of the above Examples 1 to 4 are put into a reaction kettle and stirred to mix the materials evenly;

[0037] 2) Continue to introduce nitrogen or carbon dioxide protective gas and start heating. When the temperature reaches 150°C, turn off the nitrogen or carbon dioxide protective gas and continue to heat to 180°C, keep warm for 3 hours, then continue to heat and keep warm between 190°C and 210°C for melt esterification;

[0038] 3) When the resin changes from mixed to clear, continue to keep warm for one hour, take samples to measure the acid value and viscosity, until the acid value reaches less than 25, viscosity: 30-40 seconds * format tube / 25 ° C (xylene to 60 solid content), after the acid value and viscosity are qualified, put the mass fraction of reflux xylene in the above Examples 1 to 4 into the reactor, continue to reflux esterification between 190 ° C and 210 ° C, until the acid value reaches less than 10, viscosity: 90-100 seconds * format tube / 25 ° C (xylene to 60 solid content).

[0039] 4) Cool down to 160-170°C and add diluent solvent xylene;

[0040] 5) After filtering and packaging, the general short-oil soybean oil alkyd resin of Examples 1 to 4 is obtained.

[0041] 2. Comparative Example 1 (Comparative Example of Fatty Acid Method)

[0042] 163 parts by weight of soybean oil fatty acid, 223 parts by weight of glycerol, 300 parts by weight of phthalic anhydride, 70 parts by weight of benzoic acid, 1 part by weight of a color reducing agent, and 25 parts by weight of reflux xylene were put into a reactor, heated to 180°C and kept warm for 3 hours, then refluxed and esterified at 190°C-210°C until the acid value reached less than 10, and the viscosity was 90-100 seconds*format tube / 25°C (xylene to 60 solid content), cooled to 160-170°C, and 270-280 parts by weight of a diluent solvent xylene were added; and the resin of Comparative Example 1 was obtained after filtering and packaging.

[0043] Application Example 1

[0044] 1. The alkyd resins obtained in Examples 1 to 4 and Comparative Example 1 are prepared into colored paints according to the paint formula in Table 2 using conventional processes:

[0045] Table 2 Paint formula

[0046] raw material Ratio (number of portions) Resin (Examples 1 to 4 and Comparative Example 1) 46 Titanium dioxide 26 Dispersants 0.5 Defoaming agent 0.3 Solvent (xylene) 27.2

[0047] 2. Paint testing

[0048] Take the paints prepared in the above Examples 1-4 and Comparative Example 1, and the polyurethane curing agent 740 and diluent produced by Jiangsu Sanmu Chemical Co., Ltd., prepare the alkyd polyurethane coating spray plate (paint: polyurethane curing agent 740: diluent weight ratio = 100:28:30), and test. Among them, flexibility is in accordance with the standard method of GB / T1731-2020. Impact strength is in accordance with the standard method of GB / T1732-2020. Surface dryness and actual dryness are in accordance with the standard method of GB / T1728-2020. Gloss is in accordance with the standard method of GB / T9754-2007. Hardness is in accordance with the standard method of GB / T6739-2022. Adhesion is in accordance with GB / T1720-2020. The specific alkyd polyurethane coating test results are shown in Table 3.

[0049] Table 3 Paint test results

[0050] Detection indicators Example 1 Example 2 Example 3 Example 4 Comparative Example 1 Surface drying time (min) 22 23 22 23 23 Work hard (h) 7.5 7.5 7.5 7.5 7.5 luster 95-99 95-99 95~99 95~99 95~99 Adhesion 2 2 2 2 2 Flexibility(mm) 2 2 2 2 2 Impact strength (kg.cm) 40 Positive 40 Positive 40 Positive 40 Positive 40 Positive hardness 2H 2H 2H 2H 2H

[0051] The above comparative experimental results show that the present invention screens out various reaction raw material compositions and specific reaction steps through a large number of experiments, and particularly finds that the rate difference between alcoholysis reaction and esterification reaction is different in the melting method and the solvent method, and utilizes this difference, adopts the melting method, and simultaneously adopts the collocation of glycerol and benzoic acid to make the reaction system clear into a homogeneous system. Under the premise of using whole soybean oil to produce alkyd resin, no alcoholysis step is required, and clear and transparent qualified alkyd resin is directly prepared, and the dryness, gloss, hardness, impact strength and flexibility of the resin are the same as the alkyd resin performance of the fatty acid method. Creatively pioneered the use of whole soybean oil without the step of alcoholysis, and directly synthesized alkyd resin, which has important application value.

Claims

1. A general short-oil soybean oil alkyd resin, characterized in that: It is made from soybean oil, glycerol, phthalic anhydride, benzoic acid, a color reducing agent, reflux xylene and an organic solvent.

2. A general-purpose short-oil soybean oil alkyd resin according to claim 1, characterized in that: The invention is prepared from the following raw materials in parts by weight: 166-174 parts of soybean oil, 200-210 parts of glycerol, 293-307 parts of phthalic anhydride, 68-72 parts of benzoic acid, 1-1.5 parts of a color reducing agent, 20-30 parts of reflux xylene and 270-280 parts of an organic solvent.

3. A general-purpose short-oil soybean oil alkyd resin according to claim 1, characterized in that: The color reducing agent is hypophosphorous acid.

4. A general-purpose short-oil soybean oil alkyd resin according to claim 1, characterized in that: The dilution solvent is one of toluene, xylene, trimethylbenzene, ethyl acetate, dimethyl carbonate, butyl acetate, sec-butyl acetate and propylene glycol methyl ether acetate, or a mixture of any of the above.

5. The method for preparing the general short-oil soybean oil alkyd resin according to any one of claims 1 to 4, characterized in that: The following steps are involved: 1) After introducing nitrogen or carbon dioxide protective gas, soybean oil, glycerin, phthalic anhydride, benzoic acid and color reducing agent are put into the reaction kettle and stirred to mix the materials evenly; 2) Continue to introduce nitrogen or carbon dioxide protective gas and start to heat up. When the temperature rises to 145°C-150°C, turn off the nitrogen or carbon dioxide protective gas and continue to heat up to above 170°C. When keeping at 170°C-180°C, continue to heat up to above 190°C and keep between 190°C-210°C for melt esterification; 3) When the resin changes from mixed to clear, continue to keep warm, take samples to measure the acid value and viscosity, until the acid value and viscosity are qualified, add the refluxing xylene into the reactor, continue to reflux esterification at 190℃-210℃, until the acid value and viscosity are qualified; 4) Cool down to 160-170°C and add dilution solvent; 5) Filter to obtain universal short oil soybean oil alkyd resin.

6. The method for preparing the general short-oil soybean oil alkyd resin according to claim 5, characterized in that: The following steps are involved: 1) After nitrogen or carbon dioxide protective gas is introduced for 15 to 30 minutes, soybean oil, glycerin, phthalic anhydride, benzoic acid, and color reducing agent are added to the reaction kettle and stirred to mix the materials evenly; 2) Continue to introduce nitrogen or carbon dioxide protective gas and start to heat up. When the temperature rises to 145°C-150°C, turn off the nitrogen or carbon dioxide protective gas and continue to heat up to above 170°C, keep at 170°C-180°C for 2-3 hours, continue to heat up to above 190°C, keep between 190°C-210°C for melt esterification; 3) When the resin changes from mixed to clear, continue to keep warm, take samples to measure the acid value and viscosity, until the acid value reaches less than 25, viscosity: 30-40 seconds * format tube / 25℃, xylene to 60 solid content, after the acid value and viscosity are qualified, put the reflux xylene into the reactor, continue to reflux esterification between 190℃-210℃, until the acid value reaches less than 10, viscosity: 90-100 seconds * format tube / 25℃, xylene to 60 solid content; 4) Cool down to 160-170°C and add dilution solvent; 5) After filtering, the general short oil soybean oil alkyd resin is obtained.