Method for preparing rod-like Mg-MOF-74 material by taking industrial magnesium hydroxide as raw material
By using industrial magnesium hydroxide and surfactant modification technology, combined with semi-dry method and solvothermal reaction, standardized rod-shaped Mg-MOF-74 materials were successfully prepared, solving the problem of high preparation costs and uncontrollable morphology in the existing technology. problem, realizing the industrial production of materials and efficient carbon dioxide adsorption performance.
Patent Information
- Application Number
- CN202410841937.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-27
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2044-06-27
AI Technical Summary
The existing Mg-MOF-74 material has high preparation costs, poor chemical stability, and uncontrollable morphology, which limits its industrial application. In particular, the rod-shaped material has a short length or a small aspect ratio, making it difficult to achieve large-scale production.
Using industrial magnesium hydroxide as raw material, the modified magnesium oxalate intermediate is prepared through surfactant control. Combined with semi-dry method and solvothermal reaction technology, multiple treatments are performed to obtain standardized rod-shaped Mg-MOF-74 materials.
The industrialized production of rod-shaped Mg-MOF-74 materials was realized, the chemical stability and morphology control of the materials were improved, and a product with an average particle size of 100 nm, an average length of 5 μm, and an aspect ratio greater than 50 was obtained, with a high specific surface area and good Its catalytic performance expands its industrial application prospects.
Smart Images

Figure FT_1 
Figure FT_2 
Figure FT_3
Abstract
Description
Technical Field
[0001] The invention discloses a method for preparing a rod-shaped Mg-MOF-74 material, and specifically relates to a method for preparing a rod-shaped Mg-MOF-74 material by using industrial magnesium hydroxide as a raw material. Background Art
[0002] Mg-MOF-74 is a new type of porous crystalline material, which is mainly formed by the self-assembly of central alkali metal magnesium and organic ligands. This material has the advantages of good thermal stability, regular and orderly pore structure, large specific surface area, high porosity, and adjustable size. Its carbon dioxide adsorption capacity is much higher than that of traditional zeolites and activated carbon. It is the material with the largest carbon dioxide adsorption capacity discovered so far. In recent years, it has been rapidly developed in the fields of carbon dioxide gas adsorption, biomedicine, catalytic reactions, etc. However, the high preparation cost and poor chemical stability of pure Mg-MOF-74 materials limit its industrial application. At present, the preparation methods of Mg-MOF-74 materials reported in the literature include solvent thermal synthesis, microwave synthesis, ultrasonic synthesis, ion thermal synthesis and electrochemical synthesis, mainly using magnesium nitrate hexahydrate and magnesium acetate tetrahydrate as the main raw materials, and both are analytically pure. The above methods are limited to laboratory research, and the market sales are also measured in grams, which are only used for experimental research. As for the morphology of Mg-MOF-74 materials, due to different raw materials and preparation methods, most of the products are powder or granular, and a small amount is rod-shaped, but the rod length is short, or the aspect ratio is very small, and the preparation is uncontrollable. Summary of the invention
[0003] The purpose of the present invention is to provide a method for preparing rod-shaped Mg-MOF-74 materials using industrial magnesium hydroxide as a raw material. The method uses industrial magnesium hydroxide as a raw material, directly opens up a path for the industrial production of Mg-MOF-74 materials; uses surfactants to regulate the preparation of modified magnesium oxalate intermediates, thereby achieving the regulation of crystal form; and uses a semi-dry method to prepare modified magnesium oxalate crystals, thereby saving water.
[0004] The objective of the present invention is achieved through the following technical solutions: A method for preparing a rod-shaped Mg-MOF-74 material using industrial magnesium hydroxide as a raw material. The method uses industrial magnesium hydroxide and oxalic acid as raw materials, adds a surfactant, and adopts a semi-dry method to prepare a modified magnesium oxalate intermediate; the magnesium oxalate intermediate and 2,5-dihydroxyterephthalic acid are further used as raw materials to carry out a solvothermal reaction in a mixed solvent to obtain a primary product 1; the primary product 1 is subjected to a secondary solvothermal treatment to obtain a primary product 2; and the primary product 2 is heated and activated to obtain a white Mg-MOF-74 powder product.
[0005] The method for preparing rod-shaped Mg-MOF-74 material using industrial magnesium hydroxide as raw material, wherein the industrial magnesium hydroxide is a magnesium hydroxide product produced by a brine method, the content of which is greater than 99%, and the rest is hydrochloric acid insoluble impurities.
[0006] In the method for preparing rod-shaped Mg-MOF-74 material using industrial magnesium hydroxide as raw material, the surfactant CTAB, DTAB, or one of them has a concentration (mass percentage) of 2%.
[0007] The method for preparing rod-shaped Mg-MOF-74 material using industrial magnesium hydroxide as raw material, and the semi-dry method, are that the volume ratio of the reactant raw material solid to the surfactant solution is 1:1.
[0008] The method for preparing rod-shaped Mg-MOF-74 material using industrial magnesium hydroxide as raw material, further using magnesium oxalate intermediate and 2,5-dihydroxyterephthalic acid as raw materials, performing solvothermal reaction in a mixed solvent, the molar mass ratio of the raw materials is 1:1, the volume ratio of the mixed solvent (DMF):(CH3CH2OH):(H2O) is 15:1:1, the mixed solution is prepared, the solvothermal reaction temperature is 125°C, and the reaction time is 24h.
[0009] The method for preparing rod-shaped Mg-MOF-74 material using industrial magnesium hydroxide as raw material comprises subjecting the primary product 1 to secondary solvent heat treatment, the solvent is DMF, the reaction temperature is 80°C, and the reaction time is 1h.
[0010] The method for preparing rod-shaped Mg-MOF-74 material using industrial magnesium hydroxide as raw material, wherein the product 2 is heated and activated, the activation reaction temperature is 250° C., and the reaction time is 5 hours.
[0011] The method for preparing a rod-shaped Mg-MOF-74 material using industrial magnesium hydroxide as a raw material, wherein the rod-shaped Mg-MOF-74 material has an average particle size of 100 nm, an average length of 5 μm, and an aspect ratio greater than 50.
[0012] The advantages and effects of the present invention are: 1. The present invention uses industrial magnesium hydroxide as raw material and adopts intermediate surface treatment technology to control the preparation of rod-shaped Mg-MOF-74 materials, opening up the channel for industrial production of rod-shaped Mg-MOF-74 materials, improving the added value of industrial magnesium hydroxide, and obtaining a new rod-shaped Mg-MOF-74 material with an average particle size of 100nm, an average length of 50μm, and an aspect ratio greater than 50. The material is a metal organic framework material with hexagonal pores and a specific surface area of more than 1000m 2 / g, is currently the material with the largest carbon dioxide adsorption capacity. Its regular pores, adjustable pore size and abundant alkaline sites make it a good catalyst and carrier. The large-scale production of rod-shaped Mg-MOF-74 materials has great industrial value and practical significance. The process of the present invention has green characteristics, the product has a wide range of uses, a large demand, and a broad development prospect.
[0013] 2. The present invention opens up an industrial production path for Mg-MOF-74 materials, and obtains rod-shaped Mg-MOF-74 materials with an average particle size of 100 nm, an average length of 5 μm, and an aspect ratio greater than 50. It has broad market application prospects and significant economic and social benefits. BRIEF DESCRIPTION OF THE DRAWINGS
[0014] Figure 1 It is a simplified diagram of the technical route of the present invention; Figure 2 The XRD spectrum of the Mg-MOF-74 crystal of the present invention; Figure 3 This is a scanning electron microscope image of the Mg-MOF-74 crystal of the present invention; Figure 4 This is the infrared spectrum of the Mg-MOF-74 crystal of the present invention. DETAILED DESCRIPTION
[0015] The present invention is described in detail below with reference to the embodiments.
[0016] The invention uses industrial magnesium hydroxide and oxalic acid as raw materials, adds a surfactant, and adopts a semi-dry method to prepare a modified magnesium oxalate intermediate. The magnesium oxalate intermediate and 2,5-dihydroxyterephthalic acid are further used as raw materials to perform a solvothermal reaction in a mixed solvent to obtain a product 1. The product 1 is subjected to a secondary solvothermal treatment to obtain a product 2. The product 2 is heated and activated to obtain a white Mg-MOF-74 powder.
[0017] The invention discloses a method for preparing a rod-shaped Mg-MOF-74 material by using industrial magnesium hydroxide as a raw material, and particularly relates to using industrial magnesium hydroxide as a raw material, adopting a semi-dry method to prepare a surfactant-modified magnesium oxalate intermediate; and carrying out a solvent thermal reaction with 2,5-dihydroxyterephthalic acid in a mixed solvent, continuing to carry out a secondary solvent thermal treatment, and finally heating and activating to obtain a product white Mg-MOF-74 powder.
[0018] The first step is to use industrial magnesium hydroxide and oxalic acid as raw materials, add surfactants, and adopt a semi-dry method to prepare a modified magnesium oxalate intermediate; the second step is to use the magnesium oxalate intermediate and 2,5-dihydroxyterephthalic acid as raw materials, and carry out a solvothermal reaction in a mixed solvent to obtain a preliminary product 1; the third step is to perform a secondary solvothermal treatment on the preliminary product 1 to obtain the preliminary product 2; the fourth step is to heat and activate the preliminary product 2 to obtain the product white Mg-MOF-74 powder.
[0019] 1. Basic scheme of the present invention The first step is to use industrial magnesium hydroxide and oxalic acid as raw materials, add surfactants, and adopt a semi-dry method to prepare a modified magnesium oxalate intermediate; the second step is to use the magnesium oxalate intermediate and 2,5-dihydroxyterephthalic acid as raw materials, and carry out a solvothermal reaction in a mixed solvent to obtain a preliminary product 1; the third step is to perform a secondary solvothermal treatment on the preliminary product 1 to obtain the preliminary product 2; the fourth step is to heat and activate the preliminary product 2 to obtain the product white Mg-MOF-74 powder.
[0020] 2. Technical methods of the present invention The present invention adopts a semi-dry method, uses industrial magnesium hydroxide as a raw material, reacts with oxalic acid, and prepares a modified magnesium oxalate intermediate, thereby realizing the control of the crystal form of magnesium oxalate; adopts a mixed solvent thermal reaction technology to self-assemble and synthesize a Mg-MOF-74 primary product 1; adopts a single solvent thermal reaction technology to refine the Mg-MOF-74 primary product 2; and adopts a heating activation technology to obtain a crystallized Mg-MOF-74 material.
[0021] 3. Specific embodiments of the present invention 1. Preparation of 2% CTAB Weigh 5 g of hexadecyltrimethylammonium bromide (CTAB) and 245 ml of deionized water; add CTAB powder into the deionized water and stir evenly to obtain a CTAB surfactant solution with a mass fraction of 2%.
[0022] 2. Preparation of magnesium oxalate (1) Weigh 10 g of magnesium hydroxide and 22 g of oxalic acid of equal molar mass; place them in a beaker, add 30 ml of 2% CTAB solution, and stir thoroughly; place the beaker in a vacuum drying oven and dry thoroughly. After sufficient drying, take out the beaker and cool it to room temperature.
[0023] (2) The magnesium oxalate crystals are fully ground to obtain a modified magnesium oxalate intermediate.
[0024] 3. Preparation of mixed solvent According to the volume ratio of (DMF):(CH3CH2OH):(H2O)=15:1:1, a mixed solution was prepared. The actual amount used was 61.5 ml of DMF, 4.1 ml of ethanol, and 4.1 ml of deionized water.
[0025] Mixed solvent thermal reaction (1) Self-assembly synthesis: weigh 0.655 g of magnesium oxalate and 0.165 g of 2,5-dihydroxyterephthalic acid, add them to the above mixed solvent, start magnetic stirring, stir for 1 h to mix evenly; transfer to a polytetrafluoroethylene reactor, the reaction temperature is 125 ° C, and the reaction time is 24 h; (2) Washing: Take out the reactor and cool it to room temperature. Use a circulating water vacuum pump to filter it. Then use DMF to wash it repeatedly. After filtering it several times, a white solid primary product 1 is obtained.
[0026] 5. Single solvent thermal reaction (1) Put the initial product 1 into a beaker, add a certain amount of DMF solution, turn on the magnetic stirring again, and stir for 1 hour; put the mixed colloid into a polytetrafluoroethylene kettle, the reaction temperature is 85℃, and the reaction time is 1 hour.
[0027] (2) The reactor was taken out and cooled to room temperature, and filtered again; the filtered solid was placed in a vacuum drying oven for drying to obtain a white solid primary product 2.
[0028] 6. Heating activation (1) The white solid primary product 2 was placed in a mortar and ground thoroughly to obtain a white powder.
[0029] (2) The white powder was activated at 250°C for 5 h to obtain white Mg-MOF-74 powder.
Claims
1. A method for preparing rod-shaped Mg-MOF-74 material using industrial magnesium hydroxide as raw material, characterized in that: The method uses industrial magnesium hydroxide and oxalic acid as raw materials, adds a surfactant, and adopts a semi-dry method to prepare a modified magnesium oxalate intermediate; further uses the magnesium oxalate intermediate and 2,5-dihydroxyterephthalic acid as raw materials, and performs a solvent thermal reaction in a mixed solvent to obtain a primary product 1; the primary product 1 is subjected to a secondary solvent thermal treatment to obtain a primary product 2; and the primary product 2 is heated and activated to obtain a white Mg-MOF-74 powder product.
2. A method for preparing rod-shaped Mg-MOF-74 material using industrial magnesium hydroxide as raw material according to claim 1, characterized in that: The industrial magnesium hydroxide is a magnesium hydroxide product produced by a brine method, the content of which is greater than 99%, and the rest is hydrochloric acid insoluble impurities.
3. A method for preparing rod-shaped Mg-MOF-74 material using industrial magnesium hydroxide as raw material according to claim 1, characterized in that: The surfactant CTAB, DTAB, or one of them has a concentration (mass percentage) of 2%.
4. A method for preparing rod-shaped Mg-MOF-74 material using industrial magnesium hydroxide as raw material according to claim 1, characterized in that: In the semi-dry method, the volume ratio of the reactant raw material solid to the surfactant solution is 1:
1.
5. A method for preparing rod-shaped Mg-MOF-74 material using industrial magnesium hydroxide as raw material according to claim 1, characterized in that: The method continues to use magnesium oxalate intermediate and 2,5-dihydroxyterephthalic acid as raw materials, and conducts a solvothermal reaction in a mixed solvent. The molar mass ratio of the raw materials is 1:1, the volume ratio of the mixed solvent (DMF): (CH3CH2OH): (H2O) is 15:1:1, the mixed solution is prepared, the solvothermal reaction temperature is 125°C, and the reaction time is 24h.
6. A method for preparing rod-shaped Mg-MOF-74 material using industrial magnesium hydroxide as raw material according to claim 1, characterized in that: The product 1 is subjected to secondary solvent thermal treatment, the solvent is DMF, the reaction temperature is 80°C, and the reaction time is 1h.
7. A method for preparing rod-shaped Mg-MOF-74 material using industrial magnesium hydroxide as raw material according to claim 1, characterized in that: The product 2 is heated and activated, the activation reaction temperature is 250° C., and the reaction time is 5 h.
8. A method for preparing rod-shaped Mg-MOF-74 material using industrial magnesium hydroxide as raw material according to claim 1, characterized in that: The rod-shaped Mg-MOF-74 material has an average particle size of 100 nm, an average length of 5 μm, and an aspect ratio greater than 50.
Citation Information
Patent Citations
Preparation method of nano magnesium hydroxide material
CN104528779A
Method for synthesizing medium-micro double-hole MOF-74 material by using crystal defect method
CN107759801A
Synthesis method of sheet-assembled rod-like MOF-74(Mn)
CN110898855A
Synthetic method of Mg-MOF-74
CN118165284A
Cited By
Mg-MOF-trialkyl quaternary ammonium ion adsorbent with pore structure as well as preparation method and application of Mg-MOF-trialkyl quaternary ammonium ion adsorbent in fluorine ion removal
CN122032511A