Preparation method of EP / CF composite material with synergistic flame retardance of polyphosphazene and DOPO
By in-situ synthesizing a high-content PZS spherical structure on carbon fiber and combining it with DOPO, the problems of low preparation efficiency and poor flame retardant performance of EP/CF composite materials are solved, and efficient interface bonding and flame retardant performance improvement are achieved.
Patent Information
- Application Number
- CN202410682245.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-05-29
- Publication Date
- 2024-10-15
AI Technical Summary
The existing EP/CF composite material preparation method is inefficient, uses a large amount of organic solvents and cannot effectively suppress the "candle wick effect" of the fiber, resulting in poor flame retardant properties and difficulty in maintaining mechanical properties in high temperature environments.
Using the synergistic method of polyphosphazene and DOPO, the interfacial polyphosphazene spherical structure is synthesized in situ on carbon fiber, the fiber surface is activated by sulfuric acid and nitric acid, and combined with hexachlorocyclotriphosphazene and bis(4-hydroxyphenyl)sulfone, etc. Chemical substances form a high-content PZS spherical structure to improve the interface bonding and flame retardant properties of fiber and resin.
The use of organic solvents is reduced on a large scale, the interface bonding force and flame retardant properties of composite materials are improved, the strength and flame retardant properties of composite materials are enhanced, and the "candle wick effect" can be effectively suppressed in high temperature environments.
Smart Images

Figure CN118772575A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of composite material preparation, and in particular to a method for preparing a polyphosphazene and DOPO synergistic flame-retardant EP / CF composite material. Background Art
[0002] The overall performance of composite materials depends on many parameters, such as the strength of its components (reinforcement and matrix), interface bonding, manufacturing method, environmental conditions, etc. Among them, the improvement of the strength of the same composite material mainly depends on the microstructure of the reinforcement and matrix and the interaction between the matrix and the reinforcement in the interface area. Although carbon fiber (CF) has the advantages of high strength and high modulus, due to the high-temperature carbonization of CF during the production process, its surface is smooth and has strong chemical inertness and amphiphobicity. Therefore, in the process of preparing composite materials, the interface bonding between CF and epoxy resin is poor, and the mechanical properties of the composite material are difficult to achieve the expected results. Therefore, increasing the active groups on the surface of CF, improving the wetting of resin and fiber, and increasing the interaction between fiber and resin matrix play a vital role in improving performance. In EP / CF composite materials, the interface phase plays a role of connection and fixation between the reinforcement and the matrix. A good interface can effectively transfer the stress borne by the material as a whole from the resin matrix to the reinforcement, and can delay the propagation of microcracks at the interface, thereby improving the overall mechanical properties of the composite material. EP is inherently flammable, and its limiting oxygen index is low, so it cannot pass the combustion test. At the same time, due to the "wick effect" of the fiber during combustion, under the action of external high temperature, the melt of the matrix on the fiber will flow along the fiber direction to the high temperature or burning area, making the combustion more intense. Therefore, the flame retardant performance of EP / CF composite materials is poor.
[0003] However, EP / CF composites are widely used in aerospace, motor vehicles and other fields, and the materials will face high temperature environments for a certain period of time. When an accidental fire occurs, as the material is exposed to high temperature for an increasing period of time, the temperature reaches the glass transition temperature, and the matrix on the surface of the composite begins to soften. At this time, the fiber position begins to be revealed and the composite begins to lose strength. When the temperature reaches the thermal decomposition temperature, cracks appear in the resin matrix, the matrix around the fiber begins to be missing, and the fiber becomes more obvious, resulting in a further reduction in the mechanical properties of the composite. In this case, the matrix inside the material decomposes under high temperature and combustion to produce a large amount of flammable volatile gases. Due to the low air permeability of the composite material, the internal pressure and expansion of the composite material are higher. As a result, delamination cracks appear between layers, resulting in rapid creep, buckling, collapse or other failure of the composite material. Until the matrix of the composite material is completely degraded into volatiles, smoke and char. The fiber / matrix is almost debonded and the composite is completely destroyed. In addition to the toxic mixture of combustion gases, soot particles and heat, there are also very small fiber fragments in the thick smoke, which will cause various health problems not only to people who have experienced the fire, but also to firefighters and accident investigators. Therefore, it is very important to improve the flame retardant properties of composite materials.
[0004] However, in the existing preparation method, only one bundle of fibers can be processed during preparation, which is inefficient and cannot efficiently prepare composite materials. If fiber cloth is used for processing, a large amount of organic solvent will be consumed, which is costly. Although the PZSMS spherical structure obtained on CF is evenly distributed on the fiber, the size of the obtained PZSMS spherical structure is small, which is not enough to achieve the purpose of suppressing the "wick effect" of the fiber. At the same time, there are also problems such as the modification operation is cumbersome and time-consuming, and the fiber bundle is only suitable for experimental operation and is not convenient for actual production. Summary of the invention
[0005] In order to solve the above technical problems, the purpose of the present invention is to provide a method for preparing a polyphosphazene and DOPO synergistic flame-retardant EP / CF composite material, which directly synthesizes the interfacial polyphosphazene spherical structure in situ on the fiber, greatly reduces the amount of organic solvent used, and effectively solves the problems of low preparation efficiency, use of a large amount of organic solvents and inability to suppress the fiber "wick effect" in the prior art, thereby realizing large-scale preparation.
[0006] The technical solution of the present invention to solve the above technical problems is as follows: a method for preparing a polyphosphazene and DOPO synergistic flame-retardant EP / CF composite material is provided, comprising the following steps:
[0007] (1) heating the carbon fiber in a nitrogen environment to remove the sizing agent, then adding it to a mixture of sulfuric acid and nitric acid, oxidizing it at a temperature of 50-70°C for 2-4 hours, and then washing and drying it in sequence to obtain OCF;
[0008] (2) adding the OCF, hexachlorocyclotriphosphazene (HCCP) and triethylamine obtained in step (1) to anhydrous acetonitrile, stirring at 30-50° C. for 2-4 h, then adding bis(4-hydroxyphenyl)sulfone (BPS) and stirring for 4-6 h, adding hexachlorocyclotriphosphazene again and stirring for 2-4 h, washing and drying in sequence to obtain CF@PZS;
[0009] (3) CF@PZS was added to anhydrous ethanol and ultrasonically dispersed. Then, it was dropped into the epoxy resin in an oil bath and stirred until uniformly dispersed. After the anhydrous ethanol was completely evaporated, the temperature was lowered to 80 °C, and the melted 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide (DOPO) and diaminodiphenylmethane (DDM) were added. The mixture was stirred for 10-30 min, and vacuum was applied to remove bubbles. Finally, the mixture was poured into a preheated mold and cured to obtain an EP / CF composite material.
[0010] Furthermore, in step (1), the volume ratio of sulfuric acid to nitric acid is 3:1.
[0011] Furthermore, sulfuric acid and nitric acid are both in high concentration, both higher than 90vt%.
[0012] Furthermore, in step (1), the carbon fiber is heated in a tubular furnace at 900° C. for 30-40 minutes to remove the sizing agent.
[0013] Furthermore, in step (1), the mixture is washed with deionized water until the pH value is 7, and dried at 60-80° C. for 5-7 hours.
[0014] Furthermore, in step (1), the carbon fiber is chopped carbon fiber with a diameter of 7 μm and a length of 200-300 μm.
[0015] Furthermore, in step (2), the mass volume ratio of OCF, hexachlorocyclotriphosphazene, triethylamine and anhydrous acetonitrile is 0.7-0.9 g:0.8-0.9 g:5.1-5.3 mL:60 mL.
[0016] Furthermore, in step (2), the mass volume ratio of OCF, hexachlorocyclotriphosphazene, triethylamine and anhydrous acetonitrile is 0.8 g:0.88 g:5.2 mL:60 mL.
[0017] Furthermore, in step (2), the mass ratio of OCF, bis(4-hydroxyphenyl)sulfone and the hexachlorocyclotriphosphazene added again is 0.7-0.9:3.1-3.2:0.5-0.6.
[0018] Furthermore, in step (2), the mass ratio of OCF, bis(4-hydroxyphenyl)sulfone and the hexachlorocyclotriphosphazene added again is 0.8:3.12:0.56.
[0019] Furthermore, in step (3), the mass volume ratio of CF@PZS and anhydrous ethanol is 4-6 g:40 mL.
[0020] Furthermore, in step (3), the mass volume ratio of CF@PZS and anhydrous ethanol is 5 g:40 mL.
[0021] Furthermore, in step (3), the mass ratio of CF@PZS, epoxy resin, 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide and diaminodiphenylmethane is 4-6:35-36:1.5-3:9-10.
[0022] Furthermore, in step (3), the mass ratio of CF@PZS, epoxy resin, 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide and diaminodiphenylmethane is 5:35.15:3:9.84.
[0023] Furthermore, in step (3), curing is performed at 100° C. and 150° C. for 2 h respectively.
[0024] The present invention also provides an EP / CF composite material prepared by the method for preparing the EP / CF composite material with synergistic flame retardancy of polyphosphazene and DOPO.
[0025] The present invention has the following beneficial effects:
[0026] 1. The present invention adopts short-cut carbon fiber, which can reduce the use of organic solvents in large-scale modification processing and improve the modification efficiency of CF.
[0027] 2. The present invention adopts a one-step method to directly synthesize the PZS spherical structure in situ on the carbon fiber, and then uses it to prepare the composite material; the PZS spherical structure constructed on the CF has a high content and a large size, and can more effectively form a mechanical coupling with the matrix to improve the interface bonding of EP / CF; at the same time, the high content of PZS spherical structure can be beneficial to suppress the "wick effect" of CF and improve the flame retardant properties of the composite material.
[0028] 3. The PZS spherical structure was constructed at the interface of the EP / CF composite material, and 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide (DOPO) was added to the matrix to improve the strength and flame retardant properties of the composite material.
[0029] 4. During the preparation, the sizing agent on the carbon fiber is first removed to reduce the use of organic solvents, and then the CF surface is activated with a mixed acid composed of sulfuric acid and nitric acid to generate hydroxyl (CF-OH) and carboxyl (CF-COOH) to improve the activation degree of the CF surface for subsequent modification; then HCCP is added for the first time, and the P-Cl group in HCCP reacts with the carboxyl group on the fiber to graft HCCP on the fiber; BPS is added, and the -OH group of BPS reacts with the HCCP on the carbon fiber CF to initially polymerize on the fiber to form a PZS structure with a low degree of reaction; finally, HCCP is added, and HCCP will continue to react with the PZS structure on the fiber, and will also react with the BPS in the solution to form a PZS structure. In the subsequent stirring process, the PZS structure on the CF will absorb the molecular chains with a low degree of reaction in the solution and the PZS structure with a preliminary reaction to form a larger PZS structure. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] Figure 1 Schematic diagram of the preparation of CF@PZS;
[0031] Figure 2 The scanning electron microscope micrographs, infrared analysis and thermogravimetric test results of the untreated CF, OCF and CF-PZS in Example 1;
[0032] Figure 3 It is a schematic diagram of vertical combustion;
[0033] Figure 4 Mechanical properties test results. DETAILED DESCRIPTION
[0034] The principles and features of the present invention are described below, and the examples are only used to explain the present invention and are not used to limit the scope of the present invention. If no specific conditions are specified in the embodiments, they are carried out according to normal conditions or conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments is not specified, they are all conventional products that can be purchased commercially.
[0035] Example 1
[0036] A method for preparing a polyphosphazene and DOPO synergistic flame-retardant EP / CF composite material comprises the following steps:
[0037] (1) The carbon fiber was heated in a tubular furnace at 900°C for 35 min in a nitrogen environment to remove the sizing agent, then added to a mixture of sulfuric acid and nitric acid (volume ratio 3:1), oxidized at 60°C for 6 h, washed with deionized water to pH = 7, and dried at 70°C for 6 h to obtain OCF; the carbon fiber was chopped carbon fiber with a diameter of 7 μm and a length of 200-300 μm;
[0038] (2) 0.8 g OCF, 0.88 g hexachlorocyclotriphosphazene (HCCP) and 5.2 mL triethylamine obtained in step (1) were added to 60 mL anhydrous acetonitrile and stirred at 40 °C for 3 h, then 3.12 g bis(4-hydroxyphenyl)sulfone (BPS) was added and stirred for 5 h, and 0.56 g hexachlorocyclotriphosphazene was added and stirred for 3 h, and then washed and dried in sequence to obtain CF@PZS (preparation process as shown in Figure 1 shown);
[0039] (3) 5 g CF@PZS was added to 40 mL anhydrous ethanol and ultrasonically dispersed. Then, the mixture was dropped into 35.15 g epoxy resin in an oil bath at 100 °C and stirred until uniformly dispersed. After the anhydrous ethanol was completely evaporated, the temperature was lowered to 80 °C, and 3 g of melted 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide (DOPO) and 9.84 g of diaminodiphenylmethane (DDM) were added. The mixture was stirred for 10-30 min, and vacuum was applied to remove bubbles. Finally, the mixture was poured into a preheated mold and cured at 100 °C and 150 °C for 2 h, respectively, to obtain the EP / CF composite material EP / 10CF@PZS / 6DOPO.
[0040] Example 2
[0041] A method for preparing a polyphosphazene and DOPO synergistic flame-retardant EP / CF composite material comprises the following steps:
[0042] (1) The carbon fiber was heated in a tubular furnace at 900°C for 35 min in a nitrogen environment to remove the sizing agent, then added to a mixture of sulfuric acid and nitric acid (volume ratio 3:1), oxidized at 60°C for 6 h, washed with deionized water to pH = 7, and dried at 70°C for 6 h to obtain OCF; the carbon fiber was chopped carbon fiber with a diameter of 7 μm and a length of 200-300 μm;
[0043] (2) 0.8 g OCF, 0.88 g hexachlorocyclotriphosphazene (HCCP) and 5.2 mL triethylamine obtained in step (1) were added to 60 mL anhydrous acetonitrile, stirred at 40 °C for 3 h, then 3.12 g bis(4-hydroxyphenyl) sulfone (BPS) was added and stirred for 5 h, and 0.56 g hexachlorocyclotriphosphazene was added again and stirred for 3 h, and then washed and dried in sequence to obtain CF@PZS;
[0044] (3) 5 g CF@PZS was added to 40 mL anhydrous ethanol and ultrasonically dispersed. Then, it was dropped into 35.15 g epoxy resin in an oil bath at 100 °C and stirred until uniformly dispersed. After the anhydrous ethanol was completely evaporated, the temperature was lowered to 80 °C, and 1.5 g of melted 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide (DOPO) and 9.84 g of diaminodiphenylmethane (DDM) were added. The mixture was stirred for 10-30 min, and vacuum was applied to remove bubbles. Finally, the mixture was poured into a preheated mold and cured at 100 °C and 150 °C for 2 h, respectively, to obtain the EP / CF composite material EP / 10CF@PZS / 3DOPO.
[0045] Experimental Example 1
[0046] The surface morphology of the untreated CF, OCF and CF-PZS in Example 1 was observed by scanning electron microscopy, and infrared analysis and thermogravimetric testing were performed on OCF and CF@PZS. The results are as follows: Figure 2 As shown. Among them, Figure 2 In the figure, a, b and c are SEM micrographs of CF, OCF and CF-PZS, respectively; d and e are global and local Fourier transform infrared absorption spectra of OCF and CF@PZS, and f is the thermogravimetric analysis curve of OCF and CF@PZS.
[0047] Depend on Figure 2 It can be seen that the untreated CF surface contains a large amount of impurities and pollutants. After removing the slurry and strong acid oxidation, the surface morphology of the fiber becomes smooth and flat. After subsequent in-situ polymerization modification, a large number of PZS spherical structures are evenly dispersed on the fiber surface (Figure c), and the roughness of the fiber surface is significantly increased, which is conducive to improving the interface bonding with EP. Compared with the prior art, the PZS prepared by the present invention is larger in size.
[0048] Through infrared analysis of OCF and CF@PZS, the modified CF@PZS showed several new peaks compared with OCF. -1 and 1293cm -1 The characteristic peak at 883 cm corresponds to the stretching vibration of the O=S=O group. -1 and 1186cm -1 The absorption peak at 941cm belongs to the stretching vibration of PN and P=N. -1 The absorption peak corresponds to the PO-Ar group. The appearance of this peak also directly indicates that PZS is synthesized in situ on CF by the reaction of BPS and HCCP.
[0049] Thermogravimetric test results show that the unmodified CF still retains 97wt% of the residue at 800℃ after high temperature treatment; the CF@PZS sample only has 73wt% of the residue at 800℃ after high temperature treatment, indicating that the CF is loaded with a higher content of PZS structure. Compared with the prior art, the present invention loads a higher content of PZS on CF.
[0050] Experimental Example 2
[0051] In order to explore the effect of interfacial modification on the flame retardant properties of EP / CF composites, UL-94 tests were carried out on EP / CF, EP / CF@PZS and EP / CF@PZS / DOPO samples. The UL-94 test results are shown in Table 1. The combustion process of the samples is shown in Figure 3 As shown. Among them, Figure 3 Among them, af is EP / 10CF, EP / 10CF / 3DOPO, EP / 10CF / 6DOPO, EP / 10CF@PZS, EP / 10CF@PZS / 3DOPO and EP / 10CF@PZS / 6DOPO respectively.
[0052] Table 1 LOI and UL-94 test results of EP, EP / ZIF-8 and EP / ZIF-L
[0053]
[0054] From Table 1 and Figure 3It can be seen that in the UL-94 test, EP / 10CF burns violently after the flame is removed, and the flame will not extinguish itself without external interference. However, after adding DOPO to the matrix, it is found that the flame retardant properties of the composite material are improved. Among them, the EP / 10CF / 6DOPO sample can be extinguished twice after the flame is removed, and the average burning time is 27s, reaching the V-1 flame retardant grade. After the subsequent modification of the fiber interface, it is found that the combustion degree of EP / 10CF@PZS is reduced when the flame is removed. The flame can be extinguished twice without external interference, and the average burning time is 40s, and there is no flame retardant grade. However, compared with the unmodified sample EP / 10CF, the flame retardant properties of the EP / CF composite material are improved. The subsequent addition of DOPO to the matrix improves the flame retardant properties of the composite material. The experiment found that when 3wt% DOPO was added to the matrix, the average burning time of the EP / 10CF@PZS / 3DOPO sample was improved to 16s, reaching the V-1 flame retardant grade; when 6wt% DOPO was added to the matrix, the average burning time of the composite material was improved to 9.2s, and the flame retardant grade of the composite material reached V-0. The above data prove that the interfacial PZS structure can improve the flame retardant properties of the composite material. After adding DOPO to the matrix, the flame retardant properties of the composite material are further improved. The interfacial PZS structure and DOPO in the matrix synergistically improve the flame retardant properties of the composite material.
[0055] Experimental Example 3
[0056] In order to explore the effect of interface modification on the mechanical properties of EP / CF composites, mechanical properties tests were carried out on EP / CF, EP / CF@PZS and EP / CF@PZS / DOPO samples; the experimental results are shown in Figure 4 As shown. Among them, Figure 4 In the figure, a and b are the tensile strength results and impact strength results, respectively.
[0057] Depend on Figure 4It can be seen that CF has a smooth surface and poor interface bonding with EP. Therefore, when CF is added to EP, it is found that the composite tensile strength and impact strength are reduced. After adding DOPO to EP, since the PH group of DOPO can react with the epoxy group at high temperature, DOPO will participate in the curing process of EP and increase the crosslinking density of the composite material. Therefore, the tensile strength of the composite material is improved, while the impact strength is reduced. After the interface modification of CF, it is found that the tensile strength and impact strength of the EP / 10CF@PZS composite material are improved compared with EP / 10CF. This is because the interface PZS structure increases the surface roughness of CF, has a mechanical coupling effect with EP, and improves the interface bonding. After adding DOPO to the matrix, it is found that the tensile strength of the composite material is increased and the impact strength is reduced, but it is still found that the impact strength of EP / 10CF@PZS / DOPO is higher than that of EP / 10CF / DOPO. The above data prove that the modification of the fiber interface can improve the interface bonding between CF and EP and improve the mechanical strength. After the subsequent addition of DOPO, the interfacial PZS and DOPO in the matrix synergistically improved the tensile strength of the composite material.
[0058] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for preparing a synergistic flame-retardant EP / CF composite material of polyphosphazene and DOPO, It is characterized in that The following steps are involved: (1) heating the carbon fiber in a nitrogen environment to remove the sizing agent, then adding it to a mixture of sulfuric acid and nitric acid, oxidizing it at a temperature of 50-70°C for 2-4 hours, and then washing and drying it in sequence to obtain OCF; (2) adding the OCF, hexachlorocyclotriphosphazene and triethylamine obtained in step (1) to anhydrous acetonitrile, stirring at 30-50° C. for 2-4 h, then adding bis(4-hydroxyphenyl)sulfone and stirring for 4-6 h, adding hexachlorocyclotriphosphazene again and stirring for 2-4 h, washing and drying in sequence to obtain CF@PZS; (3) CF@PZS was added to anhydrous ethanol and ultrasonically dispersed, then dropped into the epoxy resin in an oil bath and stirred until uniformly dispersed. After the anhydrous ethanol was completely evaporated, the temperature was lowered to 80 °C, and the melted 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide and diaminodiphenylmethane were added, stirred for 10-30 min, and vacuumed to remove bubbles. Finally, the mixture was poured into a preheated mold and cured to obtain an EP / CF composite material.
2. The method for preparing the EP / CF composite material with synergistic flame retardancy of polyphosphazene and DOPO as claimed in claim 1, It is characterized in that In step (1), the volume ratio of sulfuric acid to nitric acid is 3:
1.
3. The method for preparing the EP / CF composite material with synergistic flame retardancy of polyphosphazene and DOPO as claimed in claim 1, It is characterized in that In step (1), the product is washed with deionized water until the pH value is 7, and dried at 60-80° C. for 5-7 h.
4. The method for preparing the EP / CF composite material with synergistic flame retardancy of polyphosphazene and DOPO as claimed in claim 1, It is characterized in that In step (1), the carbon fiber is chopped carbon fiber with a diameter of 7 μm and a length of 200-300 μm.
5. The method for preparing the EP / CF composite material with synergistic flame retardancy of polyphosphazene and DOPO as claimed in claim 1, It is characterized in that In step (2), the mass volume ratio of OCF, hexachlorocyclotriphosphazene, triethylamine and anhydrous acetonitrile is 0.7-0.9 g: 0.8-0.9 g: 5.1-5.3 mL: 60 mL.
6. The method for preparing the EP / CF composite material with synergistic flame retardancy of polyphosphazene and DOPO as claimed in claim 1, It is characterized in that In step (2), the mass ratio of OCF, bis(4-hydroxyphenyl)sulfone and the hexachlorocyclotriphosphazene added again is 0.7-0.9:3.1-3.2:0.5-0.
6.
7. The method for preparing the EP / CF composite material with synergistic flame retardancy of polyphosphazene and DOPO as claimed in claim 1, It is characterized in that In step (3), the mass volume ratio of CF@PZS and anhydrous ethanol is 4-6 g:40 mL.
8. The method for preparing the EP / CF composite material with synergistic flame retardancy of polyphosphazene and DOPO as claimed in claim 1, It is characterized in that In step (3), the mass ratio of CF@PZS, epoxy resin, 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide and diaminodiphenylmethane is 4-6:35-36:1.5-3:9-10.
9. The method for preparing the EP / CF composite material with synergistic flame retardancy of polyphosphazene and DOPO as claimed in claim 1, It is characterized in that In step (3), curing is performed at 100° C. and 150° C. for 2 h respectively.
10. The EP / CF composite material obtained by the method for preparing the EP / CF composite material with synergistic flame retardancy of polyphosphazene and DOPO as described in any one of claims 1 to 9.