Microencapsulated flame retardant modified carbon fiber epoxy resin composite material and preparation method thereof
By using polyurethane-coated ammonium polyphosphate microcapsules in carbon fiber epoxy resin composite materials, a "three-source" flame retardant is formed, which solves the problems of flame retardancy and interface compatibility and significantly improves the flame retardancy of the material. performance and overall performance.
Patent Information
- Application Number
- CN202410937827.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-12
- Publication Date
- 2024-10-15
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The poor flame retardancy of carbon fiber epoxy resin composites and the poor interfacial compatibility between ammonium polyphosphate and epoxy resin limit its application in certain fields.
Flame-retardant microcapsule PUAPP is prepared using an in-situ polymerization method. Ammonium polyphosphate is coated with polyurethane to form a "three-source-in-one" flame retardant with carbon source, acid source and gas source to improve its compatibility and water resistance. And evenly disperse it into the epoxy resin to form a carbon fiber epoxy resin composite material.
Significantly improves the flame retardant performance and interface compatibility of carbon fiber epoxy resin composites, enhances its overall performance, reduces fire hazards, while simplifying the production process and reducing costs.
Smart Images

Figure CN118772576A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of flame retardant modification of carbon fiber epoxy resin composite materials and relates to a carbon fiber epoxy resin composite material modified by a microencapsulated flame retardant and a preparation method thereof. Background Art
[0002] Carbon fiber epoxy composites (CFEP) have the advantages of light weight, high strength, high stiffness, corrosion resistance and high design freedom, so they are widely used in automobiles, ships, sporting goods, construction and other industrial fields. Carbon fiber (CF) is used as a reinforcing material in CFEP, thereby improving the mechanical properties of the composite material. Epoxy resin has excellent bonding properties, chemical resistance and high temperature resistance, which can effectively transfer loads and protect carbon fibers. The resin polymer is used as a matrix to bond the fibers to protect them from environmental influences. CFEP has become the preferred material for aerospace equipment because of its integration of structure and manufacturing materials, and the ease of achieving comprehensive performance of large-sized and complex components.
[0003] Epoxy resin and its composite materials can be used as a material with better performance in various aspects because of its high mechanical strength, excellent adhesion, chemical resistance and good electrical insulation, so as to be used as a framework structure in aerospace, automobile, shipbuilding and energy industries. However, due to the high heat released during its combustion process, the large amount of flammable gas and smoke, and the molten dripping during the combustion process, the limiting oxygen index (LOI) is low, only about 20%, and it is a flammable material. It also has defects such as high brittleness and weak resistance to external impact, which limits its application in some fields. Therefore, it is very necessary to develop epoxy resin with flame retardant effect and functionalize epoxy resin with flame retardant. However, some modification methods will affect the viscosity and curing time of epoxy resin, thereby changing the processing conditions of epoxy resin. At present, it is not only necessary to give epoxy resin a flame retardant effect, but also the greater challenge is to develop a flame retardant system that can improve its fire resistance without reducing the mechanical properties of polymer composites.
[0004] Ammonium polyphosphate (APP) is widely used in the field of polymer flame retardancy due to its low cost, low toxicity and good flame retardant effect. Ammonium polyphosphate (APP) is an environmentally friendly flame retardant widely used to improve the flame retardancy of polymers. During the combustion process, APP releases NH3, water and inorganic acids. Inorganic acids can react with hydroxyl groups to form phosphate esters. Coking occurs when the phosphate ester is dehydrated, and then an expanded carbonaceous structure is formed during the release of NH3 and water. The expanded carbonaceous structure acts as a barrier to reduce thermal radiation and isolate pyrolysis products. However, APP has weak water resistance, is easy to absorb moisture, and has poor compatibility with polymers, which limits its application. In addition, during the preparation of the polymer, APP produces a separation layer in the prepolymer, resulting in the destruction of mechanical properties, changes in glass transition temperature, and a decrease in flame retardant efficiency. Summary of the invention
[0005] The purpose of the present invention is to solve the problems in the prior art and provide a method for preparing a flame-retardant microcapsule and its application in a carbon fiber epoxy composite material to solve the technical problems in the prior art that the carbon fiber epoxy resin composite material has poor flame retardancy and the interface compatibility between ammonium polyphosphate and epoxy resin is poor.
[0006] In order to achieve the above object, the present invention adopts the following technical solutions:
[0007] A method for preparing a carbon fiber epoxy resin composite material based on a microencapsulated flame retardant, characterized by comprising:
[0008] S1: Using ammonium polyphosphate as the core material and polyurethane as the wall material, flame-retardant microcapsules PUAPP were prepared by in-situ polymerization;
[0009] S2: The prepared flame-retardant microcapsule PUAPP is evenly dispersed into the epoxy resin E-51, applied on the carbon fiber cloth, and then cured to obtain a carbon fiber epoxy resin composite material.
[0010] Preferably, the S1 specifically includes:
[0011] S101: Dissolve PEG2000 in polyvinyl alcohol solution to obtain solution A
[0012] S102: HDI trimer, emulsifier OP-10, ammonium polyphosphate, catalyst dibutyltin dilaurate and solvent dimethyl sulfoxide are mixed, and stirred with a magnetic stirrer until uniform to obtain solution B;
[0013] S103: adding solution B dropwise into solution A to mix and disperse the mixture, and then taking out the emulsion and letting it stand to obtain a mixed solution C;
[0014] S104: The mixed solution C is heated in a water bath for reaction, a chain extender 1,4-butanediol is added, the temperature is raised for reaction, the temperature is cooled to room temperature, and then centrifuged to obtain PUAPP.
[0015] Preferably, in S101, PEG2000 is dissolved in 150 mL of polyvinyl alcohol solution, and the mass fraction of the polyvinyl alcohol solution is 1.5%.
[0016] Preferably, in S102, HDI trimer and PEG2000 are first reacted to form polyurethane, which is then coated on the surface of ammonium polyphosphate. The molar ratio of HDI trimer and PEG2000 is (1.05-1.2):1; the mass ratio of polyurethane to ammonium polyphosphate is 1:(0.25-1.5).
[0017] Preferably, after the solution B and the solution A are mixed in S103, they are dispersed in a homogenizer at a speed of 8000 to 10000 r / min for 10 to 30 min, and the emulsion is taken out and allowed to stand for 15 to 30 min to obtain a mixed solution C.
[0018] Preferably, in S104, the addition of the chain extender 1,4-butanediol complies with a chain extension coefficient of 0.90.
[0019] Preferably, the S2 specifically includes:
[0020] S201: evenly disperse the flame-retardant microcapsule PUAPP into the epoxy resin system, heat in a water bath and stir until uniform, add curing agent H256, heat in a water bath to make it flowable, and evenly apply it on a 10 cm×10 cm carbon fiber cloth;
[0021] S202: placing the coated carbon fiber cloth into a mold preheated to 90° C., and curing the mold using a three-stage temperature rise method to obtain a carbon fiber epoxy resin composite material.
[0022] Preferably, in S201, the mass ratio of the epoxy resin system to the curing agent H256 is 100:32.
[0023] Preferably, in S202, the three-stage temperature rise curing is to keep the temperature at 90°C and normal pressure for 2 hours, then pressurize to 5MPa, then heat to 120°C and keep it for 2 hours, and in the third stage, keep the temperature at 150°C for 3 hours.
[0024] A carbon fiber epoxy resin composite material based on a microencapsulated flame retardant is prepared by any one of the preparation methods described above.
[0025] Compared with the prior art, the present invention has the following beneficial effects:
[0026] The present invention discloses a method for preparing a microencapsulated flame retardant modified carbon fiber epoxy resin composite material, wherein the flame retardant microcapsule PUAPP is prepared by an in-situ polymerization method, polyurethane is used as the wall material, and after the ammonium polyphosphate core material is coated with polyurethane, a carbon source and a gas source are introduced on the surface of the ammonium polyphosphate, so that the microencapsulated APP particles form a carbon source, an acid source and a gas source. The "three-source-in-one" flame retardant not only has good compatibility and water resistance, but also exhibits good flame retardancy when used alone, and at the same time strengthens the interface compatibility between ammonium polyphosphate and epoxy resin, thereby promoting the improvement of interface performance and overall material performance.
[0027] The intumescent flame retardant (IFR) formula consists of three parts: acid source, carbon source and gas source. It provides flame retardancy to polymers by converting the decomposition mode into a condensation phase mechanism. Ammonium polyphosphate, as the acid source of IFR, has strong polarity and poor interfacial compatibility with the epoxy resin matrix. Polyurethane is coated on the surface of ammonium polyphosphate particles to introduce carbon source and gas source, so that the microencapsulated ammonium polyphosphate particles form carbon source, acid source and gas source. The "three-source-in-one" flame retardant not only has good compatibility and water resistance, but also exhibits good flame retardancy when used alone. In addition, the NH bond in the polyurethane may also participate in the curing of the epoxy resin, thereby improving the bonding strength between ammonium polyphosphate and the epoxy resin matrix. The PU shell layer can isolate and delay the catalytic degradation of APP, increase the thermal decomposition temperature and flame retardancy. In addition, the preparation method of the polyurethane shell layer is simple and easy to industrialize. The flame-retardant microcapsules of the present invention have low cost, are easy to produce, and have a high yield. The preparation process does not cause pollution to the environment, and at the same time solves the key problem of uneven distribution of ammonium polyphosphate in epoxy resin, and reduces stress concentration on the surface of the carbon fiber epoxy resin composite material. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings required for use in the embodiments are briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present invention and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without creative work.
[0029] Figure 1 The infrared spectra of the present invention are as follows; wherein (a) is the infrared spectra of the preparation of the PU shell; (b) is the infrared spectra of ammonium polyphosphate (APP) and PUAPP;
[0030] Figure 2 It is the XRD analysis spectrum of the present invention;
[0031] Figure 3 It is a scanning SEM image of the present invention;
[0032] Figure 4The flame retardant performance test results of carbon fiber epoxy resin composites before and after adding flame retardant microcapsules; (a) is the maximum heat release rate (PHRR) diagram; (b) is the maximum total heat release (THR) diagram; (c) is the fire performance index (FPI) and fire growth index (FGI) diagram;
[0033] Figure 5 It is a flow chart of the preparation method of the present invention. DETAILED DESCRIPTION
[0034] In order to make the purpose, technical solutions and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Generally, the components of the embodiments of the present invention described and shown in the drawings here can be arranged and designed in various different configurations.
[0035] Therefore, the following detailed description of the embodiments of the present invention provided in the accompanying drawings is not intended to limit the scope of the invention claimed for protection, but merely represents selected embodiments of the present invention. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0036] It should be noted that similar reference numerals and letters denote similar items in the following drawings, and therefore, once an item is defined in one drawing, further definition and explanation thereof is not required in subsequent drawings.
[0037] In the description of the embodiments of the present invention, it should be noted that if the terms "upper", "lower", "horizontal", "inner", etc. indicate an orientation or positional relationship based on the orientation or positional relationship shown in the drawings, or the orientation or positional relationship in which the product of the invention is usually placed when in use, it is only for the convenience of describing the present invention and simplifying the description, and does not indicate or imply that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as a limitation on the present invention. In addition, the terms "first", "second", etc. are only used to distinguish the description, and cannot be understood as indicating or implying relative importance.
[0038] In addition, if the term "horizontal" appears, it does not mean that the component must be absolutely horizontal, but can be slightly tilted. For example, "horizontal" only means that its direction is more horizontal than "vertical", which does not mean that the structure must be completely horizontal, but can be slightly tilted.
[0039] In the description of the embodiments of the present invention, it is also necessary to explain that, unless otherwise clearly specified and limited, the terms "set", "install", "connect", and "connect" should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection, or it can be indirectly connected through an intermediate medium, or it can be the internal connection of two components. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.
[0040] The present invention is further described in detail below in conjunction with the accompanying drawings:
[0041] See also Figure 5 The present invention discloses a method for preparing a carbon fiber epoxy resin composite material based on a microencapsulated flame retardant, comprising:
[0042] S1: Using ammonium polyphosphate as the core material and polyurethane as the wall material, flame-retardant microcapsules PUAPP were prepared by in-situ polymerization;
[0043] S2: The prepared flame-retardant microcapsule PUAPP is evenly dispersed into the epoxy resin E-51, applied on the carbon fiber cloth, and then cured to obtain a carbon fiber epoxy resin composite material.
[0044] The flame-retardant microcapsules are prepared by in-situ polymerization, which has a relatively simple process and a fast reaction speed. This method can effectively control the thickness of the wall material, making it suitable for industrial production. The PU shell layer can isolate and delay the catalytic degradation of APP, increase the thermal decomposition temperature and flame retardancy. The NH bonds in the PU shell may also participate in the curing of the epoxy resin, improve the bonding strength between ammonium polyphosphate and the epoxy resin matrix, thereby promoting the improvement of the interface performance and the overall performance of the material, and synergistically improving the flame retardant and mechanical properties of CFRP.
[0045] In some embodiments, the flame-retardant microcapsule PUAPP is prepared by an in-situ polymerization method, which specifically includes:
[0046] S101: Dissolve the measured PEG2000 in 150 ml of polyvinyl alcohol solution to obtain solution A; preferably, the polyvinyl alcohol solution has a mass fraction of 1.5%.
[0047] S102: Add the measured HDI trimer, emulsifier OP-10, ammonium polyphosphate (APP), catalyst dibutyltin dilaurate, and solvent dimethyl sulfoxide (DMSO) into a 100 mL beaker, stir with a magnetic stirrer for 30 min, and obtain solution B after mixing evenly;
[0048] Preferably, n (NCO) :n (OH)=(1.05-1.2):1; 1-2 drops of dibutyltin dilaurate are taken, and the mass ratio of polyurethane to ammonium polyphosphate is 1:(0.25-1.5);
[0049] S103: adding solution B dropwise into solution A and mixing them, dispersing them in a homogenizer at a speed of 10000 r / min for 15 min, taking out the emulsion and letting it stand for 20 min, and then adding it to a 250 mL three-necked flask to obtain a mixed solution C;
[0050] S104: The mixed solution C is slowly heated to 60°C in a water bath and reacted for 0.5h. A measured amount of chain extender 1,4-butanediol (BDO) is added and the temperature is raised to 80°C and reacted for 4h. After cooling to room temperature, the mixed solution is washed by centrifugation and dried in a vacuum oven at 60°C for 24-48h.
[0051] Preferably, the addition of the chain extender BDO complies with a chain extension coefficient of 0.90. After the first centrifugation, the supernatant is poured out and ultrasonically cleaned with ethanol and deionized water respectively.
[0052] In some embodiments, the prepared flame-retardant microcapsule PUAPP is uniformly dispersed into the epoxy resin E-51, applied on the carbon fiber cloth, and then cured to obtain a carbon fiber epoxy resin composite material, which specifically includes the following steps:
[0053] S201: Weigh a certain amount of flame-retardant microcapsule PUAPP and evenly disperse it into the epoxy resin system, stir the mixture in a water bath at 60° C. for 2 h, add curing agent H256, and then heat it in a water bath to make it flowable, and evenly apply it on a 10 cm×10 cm carbon fiber cloth;
[0054] Preferably, the mass ratio of the resin to the curing agent reaches 100:32.
[0055] S202: placing the coated carbon cloth into a mold preheated at 90° C., and placing the mold in a hot press to perform three-stage temperature rise curing to obtain a carbon fiber epoxy resin composite material.
[0056] Preferably, the curing is performed in three stages, i.e., keeping the temperature at 90°C and normal pressure for 2 hours, then pressurizing to 5 MPa, then heating to 120°C and keeping the temperature for 2 hours, and in the third stage keeping the temperature at 150°C for 3 hours.
[0057] In some embodiments, before coating the carbon fiber cloth, the carbon fiber is first cleaned until there is no sizing agent on the surface of the carbon fiber.
[0058] Specifically, polyurethane is used as the wall material, and after the ammonium polyphosphate core material is coated with polyurethane, a carbon source and a gas source are introduced on the surface of the ammonium polyphosphate, so that the microencapsulated APP particles form a carbon source, an acid source and a gas source. The "three-source-in-one" flame retardant not only has good compatibility and water resistance, but also exhibits good flame retardancy when used alone. At the same time, it strengthens the interface compatibility between ammonium polyphosphate and epoxy resin, thereby promoting the improvement of interface performance and overall material performance.
[0059] In some embodiments, a method for preparing a carbon fiber epoxy resin composite material based on a microencapsulated flame retardant comprises the following steps:
[0060] (1) Since carbon fibers need to be sizing before leaving the factory, and the sizing agent usually affects the fiber surface modification and bulk characterization results, the carbon fibers need to be cleaned before use to remove impurities such as the sizing agent. The specific operation is as follows: 6 pieces of carbon fibers are placed in a Soxhlet extractor filled with acetone, refluxed for 48 hours, and vacuum dried at 80°C for 24 hours.
[0061] (2) PUAPP was prepared by in situ polymerization.
[0062] First, 6.6 g of PEG2000 was dissolved in 150 ml of polyvinyl alcohol solution (mass fraction of 1.5%) to obtain solution A; secondly, 2 g of HDI trimer, 0.69 g of emulsifier OP-10, 4.25 g of ammonium polyphosphate (APP), 1 to 2 drops of dibutyltin dilaurate, and solvent dimethyl sulfoxide (DMSO) were added to a 100 mL beaker and magnetically stirred for 30 min to obtain solution B after mixing evenly; then solution B was added dropwise to solution A. The mixture was mixed and dispersed in a homogenizer at a speed of 10000 r / min for 15 min. The emulsion was taken out and allowed to stand for 20 min, then added into a 250 mL three-necked flask to obtain a mixed solution C. Finally, the mixed solution C was slowly heated to 60°C in a water bath, reacted for 0.5 h, 112 μL of 1,4-butanediol (BDO) was added, the temperature was raised to 80°C and maintained for 4 h, and after cooling to room temperature, PUAPP was obtained by centrifugation and dried in a vacuum oven at 60°C for 24 to 48 h.
[0063] (3) Preparation of PUAPP / CF / EP composites
[0064] Weigh PUAPP and evenly disperse it in the epoxy resin system. Stir the mixture in a water bath at 60℃ for 2h, then add curing agent H256 to ensure that the mass ratio of resin and curing agent reaches 100:32, then heat it in a water bath to make it flow, and evenly apply it on a 10cm×10cm carbon fiber cloth, then put the sample into a mold preheated at 90℃, and place the mold in a hot press. The preparation process of the composite material adopts a three-stage heating process, that is, 90℃ normal pressure insulation for 2h, then pressurized to 5MPa, then heated to 120℃ and kept warm for 2h, and the third stage keeps the temperature at 150℃ for 3h. After the mold is cooled to room temperature, demoulding is performed, and the obtained composite material is a PUAPP / CF / EP composite material. According to the test requirements, the obtained samples are cut to appropriate sizes for testing.
[0065] This application starts from the perspective of flame retardant modification of carbon fiber epoxy resin composites. The polyurethane shell layer is coated on the surface of ammonium polyphosphate core material by in-situ polymerization. By adjusting the core-to-wall ratio, the PUAPP morphology is regulated, thereby introducing flame retardant microcapsules into carbon fiber epoxy resin composites to study the changing law of the flame retardant properties of the composites. At the same time, SEM, FTIR, XRD, cone calorimetry and other performance tests are used to test the surface microstructure and surface chemical properties of PUAPP. The effect of the addition of PUAPP on the flame retardant properties of carbon fiber epoxy resin composites is systematically studied. For details, see the following examples: Example 1
[0066] (1) Since carbon fibers need to be sizing before leaving the factory, and the sizing agent usually affects the fiber surface modification and bulk characterization results, the carbon fibers need to be cleaned before use to remove impurities such as the sizing agent. The specific operation is as follows: 6 pieces of carbon fibers are placed in a Soxhlet extractor filled with acetone, refluxed for 48 hours, and vacuum dried at 80°C for 24 hours.
[0067] (2) PUAPP was prepared by in situ polymerization.
[0068] The specific operations are as follows:
[0069] First, 6.6 g of PEG2000 was dissolved in 150 mL of polyvinyl alcohol solution (mass fraction of 1.5%) to obtain solution A; secondly, 1.75 g of HDI trimer, 0.69 g of emulsifier OP-10, 2.09 g of ammonium polyphosphate (APP), 1 to 2 drops of dibutyltin dilaurate, and solvent dimethyl sulfoxide (DMSO) were added to a 100 mL beaker, and magnetic stirring was performed for 30 minutes to obtain solution B after mixing evenly; then solution B was added dropwise to solution A and mixed, and dispersed in a homogenizer at a speed of 10000 r / min for 15 minutes, and the emulsion was taken out and allowed to stand for 15 minutes and then added to a 250 mL three-necked flask to obtain a mixed solution C;
[0070] Finally, the mixed solution C was slowly heated to 60°C in a water bath, reacted for 0.5h, 112μL of 1,4-butanediol (BDO) was added, the temperature was raised to 80°C and maintained for 4h, cooled to room temperature, centrifuged to obtain PUAPP, and dried in a vacuum oven at 60°C for 24-48h.
[0071] (3) Preparation of PUAPP / CF / EP composites
[0072] Weigh PUAPP and evenly disperse it in the epoxy resin system. Stir the mixture in a water bath at 60℃ for 2h, then add curing agent H256 to ensure that the mass ratio of resin and curing agent reaches 100:32, then heat it in a water bath to make it flow, and evenly apply it on a 10cm×10cm carbon fiber cloth, then put the sample into a mold preheated at 90℃, and place the mold in a hot press. The preparation process of the composite material adopts a three-stage heating process, that is, 90℃ normal pressure insulation for 2h, then pressurized to 5MPa, then heated to 120℃ and kept warm for 2h, and the third stage keeps the temperature at 150℃ for 3h. After the mold is cooled to room temperature, demoulding is performed, and the obtained composite material is a PUAPP / CF / EP composite material. According to the test requirements, the obtained samples are cut to appropriate sizes for testing.
[0073] Example 2
[0074] (1) Since carbon fibers need to be sizing before leaving the factory, and the sizing agent usually affects the fiber surface modification and bulk characterization results, the carbon fibers need to be cleaned before use to remove impurities such as the sizing agent. The specific operation is as follows: 6 pieces of carbon fibers are placed in a Soxhlet extractor filled with acetone, refluxed for 48 hours, and vacuum dried at 80°C for 24 hours.
[0075] (2) PUAPP was prepared by in situ polymerization.
[0076] The specific operations are as follows:
[0077] First, 6.6 g of PEG2000 was dissolved in 150 mL of polyvinyl alcohol solution (mass fraction of 1.5%) to obtain solution A; secondly, 1.83 g of HDI trimer, 0.69 g of emulsifier OP-10, 4.215 g of ammonium polyphosphate (APP), 1 to 2 drops of dibutyltin dilaurate, and solvent dimethyl sulfoxide (DMSO) were added to a 100 mL beaker and magnetically stirred for 30 min to obtain solution B after mixing evenly; then solution B was added dropwise to solution A was mixed and dispersed in a homogenizer at a speed of 10000r / min for 15min. The emulsion was taken out and allowed to stand for 20min and then added to a 250mL three-necked flask to obtain a mixed solution C. Finally, the mixed solution C was slowly heated to 60°C in a water bath and reacted for 0.5h. 112μL of 1,4-butanediol (BDO) was added and the temperature was raised to 80°C and maintained for 4h. After cooling to room temperature, PUAPP was obtained by centrifugation and dried in a vacuum oven at 60°C for 24 to 48h.
[0078] (3) Preparation of PUAPP / CF / EP composites
[0079] Weigh PUAPP and evenly disperse it in the epoxy resin system. Stir the mixture in a water bath at 60℃ for 2h, then add curing agent H256 to ensure that the mass ratio of resin and curing agent reaches 100:32, then heat it in a water bath to make it flow, and evenly apply it on a 10cm×10cm carbon fiber cloth, then put the sample into a mold preheated at 90℃, and place the mold in a hot press. The preparation process of the composite material adopts a three-stage heating process, that is, 90℃ normal pressure insulation for 2h, then pressurized to 5MPa, then heated to 120℃ and kept warm for 2h, and the third stage keeps the temperature at 150℃ for 3h. After the mold is cooled to room temperature, demoulding is performed, and the obtained composite material is a PUAPP / CF / EP composite material. According to the test requirements, the obtained samples are cut to appropriate sizes for testing.
[0080] Example 3
[0081] (1) Since carbon fibers need to be sizing before leaving the factory, and the sizing agent usually affects the fiber surface modification and bulk characterization results, the carbon fibers need to be cleaned before use to remove impurities such as the sizing agent. The specific operation is as follows: 6 pieces of carbon fibers are placed in a Soxhlet extractor filled with acetone, refluxed for 48 hours, and vacuum dried at 80°C for 24 hours.
[0082] (2) PUAPP was prepared by in situ polymerization.
[0083] The specific operations are as follows:
[0084] First, 6.6 g of PEG2000 was dissolved in 150 ml of polyvinyl alcohol solution (mass fraction of 1.5%) to obtain solution A; secondly, 2 g of HDI trimer, 0.69 g of emulsifier OP-10, 6.45 g of ammonium polyphosphate (APP), 1 to 2 drops of dibutyltin dilaurate, and solvent dimethyl sulfoxide (DMSO) were added to a 100 mL beaker and magnetically stirred for 30 min to obtain solution B after mixing evenly; then solution B was added dropwise to solution A. The mixture was mixed and dispersed in a homogenizer at a speed of 10000 r / min for 15 min. The emulsion was taken out and allowed to stand for 30 min, then added into a 250 mL three-necked flask to obtain a mixed solution C. Finally, the mixed solution C was slowly heated to 60°C in a water bath, reacted for 0.5 h, 112 μL of 1,4-butanediol (BDO) was added, the temperature was raised to 80°C and maintained for 4 h, and after cooling to room temperature, PUAPP was obtained by centrifugation and dried in a vacuum oven at 60°C for 24 to 48 h.
[0085] (3) Preparation of PUAPP / CF / EP composites
[0086] Weigh PUAPP and evenly disperse it in the epoxy resin system. Stir the mixture in a water bath at 60℃ for 2h, then add curing agent H256 to ensure that the mass ratio of resin and curing agent reaches 100:32, then heat it in a water bath to make it flow, and evenly apply it on a 10cm×10cm carbon fiber cloth, then put the sample into a mold preheated at 90℃, and place the mold in a hot press. The preparation process of the composite material adopts a three-stage heating process, that is, 90℃ normal pressure insulation for 2h, then pressurized to 5MPa, then heated to 120℃ and kept warm for 2h, and the third stage keeps the temperature at 150℃ for 3h. After the mold is cooled to room temperature, demoulding is performed, and the obtained composite material is a PUAPP / CF / EP composite material. According to the test requirements, the obtained samples are cut to appropriate sizes for testing.
[0087] Example 4
[0088] (1) Since carbon fibers need to be sizing before leaving the factory, and the sizing agent usually affects the fiber surface modification and bulk characterization results, the carbon fibers need to be cleaned before use to remove impurities such as the sizing agent. The specific operation is as follows: 6 pieces of carbon fibers are placed in a Soxhlet extractor filled with acetone, refluxed for 48 hours, and vacuum dried at 80°C for 24 hours.
[0089] (2) PUAPP was prepared by in situ polymerization.
[0090] The specific operations are as follows:
[0091] First, 6.6 g of PEG2000 was dissolved in 150 ml of polyvinyl alcohol solution (mass fraction of 1.5%) to obtain solution A; secondly, 2 g of HDI trimer, 0.69 g of emulsifier OP-10, 8.6 g of ammonium polyphosphate (APP), 1 to 2 drops of dibutyltin dilaurate, and solvent dimethyl sulfoxide (DMSO) were added to a 100 mL beaker, and magnetic stirring was performed for 30 minutes to obtain solution B after uniform mixing; then solution B was added dropwise to solution A and mixed, and dispersed in a homogenizer at a speed of 10000 r / min for 15 minutes, and the emulsion was taken out and allowed to stand for 20 minutes and then added to a 250 mL three-necked flask to obtain a mixed solution C;
[0092] Finally, the mixed solution C was slowly heated to 60°C in a water bath, reacted for 0.5h, 112μL of 1,4-butanediol (BDO) was added, the temperature was raised to 80°C and maintained for 4h, cooled to room temperature, centrifuged to obtain PUAPP, and dried in a vacuum oven at 60°C for 24-48h.
[0093] (3) Preparation of PUAPP / CF / EP composites
[0094] Weigh PUAPP and evenly disperse it in the epoxy resin system. Stir the mixture in a water bath at 60℃ for 2h, then add curing agent H256 to ensure that the mass ratio of resin and curing agent reaches 100:32, then heat it in a water bath to make it flow, and evenly apply it on a 10cm×10cm carbon fiber cloth, then put the sample into a mold preheated at 90℃, and place the mold in a hot press. The preparation process of the composite material adopts a three-stage heating process, that is, 90℃ normal pressure insulation for 2h, then pressurized to 5MPa, then heated to 120℃ and kept warm for 2h, and the third stage keeps the temperature at 150℃ for 3h. After the mold is cooled to room temperature, demoulding is performed, and the obtained composite material is a PUAPP / CF / EP composite material. According to the test requirements, the obtained samples are cut to appropriate sizes for testing.
[0095] Example 5
[0096] (1) Since carbon fibers need to be sizing before leaving the factory, and the sizing agent usually affects the fiber surface modification and bulk characterization results, the carbon fibers need to be cleaned before use to remove impurities such as the sizing agent. The specific operation is as follows: 6 pieces of carbon fibers are placed in a Soxhlet extractor filled with acetone, refluxed for 48 hours, and vacuum dried at 80°C for 24 hours.
[0097] (2) PUAPP was prepared by in situ polymerization.
[0098] The specific operations are as follows:
[0099] First, 6.6 g of PEG2000 was dissolved in 150 ml of polyvinyl alcohol solution (mass fraction of 1.5%) to obtain solution A; secondly, 2 g of HDI trimer, 0.69 g of emulsifier OP-10, 12.9 g of ammonium polyphosphate (APP), 1 to 2 drops of dibutyltin dilaurate, and solvent dimethyl sulfoxide (DMSO) were added to a 100 mL beaker and magnetically stirred for 30 min to obtain solution B after mixing evenly; then solution B was added dropwise to solution A. The mixture was mixed and dispersed in a homogenizer at a speed of 10000 r / min for 15 min. The emulsion was taken out and allowed to stand for 20 min, then added into a 250 mL three-necked flask to obtain a mixed solution C. Finally, the mixed solution C was slowly heated to 60°C in a water bath, reacted for 0.5 h, 112 μL of 1,4-butanediol (BDO) was added, the temperature was raised to 80°C and maintained for 4 h, and after cooling to room temperature, PUAPP was obtained by centrifugation and dried in a vacuum oven at 60°C for 24 to 48 h.
[0100] (3) Preparation of PUAPP / CF / EP composites
[0101] Weigh PUAPP and evenly disperse it in the epoxy resin system. Stir the mixture in a water bath at 60℃ for 2h, then add curing agent H256 to ensure that the mass ratio of resin and curing agent reaches 100:32, then heat it in a water bath to make it flow, and evenly apply it on a 10cm×10cm carbon fiber cloth, then put the sample into a mold preheated at 90℃, and place the mold in a hot press. The preparation process of the composite material adopts a three-stage heating process, that is, 90℃ normal pressure insulation for 2h, then pressurized to 5MPa, then heated to 120℃ and kept warm for 2h, and the third stage keeps the temperature at 150℃ for 3h. After the mold is cooled to room temperature, demoulding is performed, and the obtained composite material is a PUAPP / CF / EP composite material. According to the test requirements, the obtained samples are cut to appropriate sizes for testing.
[0102] In order to characterize the morphological features, the target product was tested by Fourier transform infrared spectroscopy (FTIR). Figure 1 (a) is the infrared spectrum of the preparation of PU shell, Figure 1 (b) is the infrared spectrum of ammonium polyphosphate (APP) and PUAPP. In (a), the infrared spectrum of HDI trimer is 2943, 2860 cm -1 It is the -CH3, -CH2 stretching vibration peak, 2264cm -1 The stretching vibration peak of -NCO is at 1682cm -1 It is the overlapping stretching vibration peak of C=O and C=C. After being made into PU shell, it is at 3362cm -1 The stretching vibration peaks of the carbamate group are generated at 2931 and 2858 cm -1The stretching vibration peaks of -CH3 and -CH2 are at 2264 cm -1 The stretching vibration peak of NCO at 40° disappeared, proving the successful preparation of PU shell.
[0103] (b) 3207cm in the figure -1 is the stretching vibration peak of the carbamate group, 1452 cm -1 It is the bending vibration peak of NH in APP, 1258cm -1 is the PO absorption peak, 1072cm -1 It is the POP symmetric stretching vibration peak, 1018cm -1 It is the symmetrical vibration peak of PO2 and PO3, 885cm -1 It is the asymmetric stretching vibration peak of PO, which preliminarily proves that the polyurethane shell is successfully coated on the surface of ammonium polyphosphate.
[0104] In order to verify the crystal structure characteristics of the material, the product was tested by X-ray powder diffraction (XRD). Figure 2 The analysis spectra of APP before and after coating and PU shell. The I(110) / I(200) ratio is 2.27. The I(110) / I(200) ratio of PUAPP coated with PU shell is reduced to 2.00, which proves that the growth of APP (110) lattice plane is inhibited and some new diffraction peaks are generated. After polymerization, it is believed that PU is coated on the surface of APP.
[0105] Figure 3 Scanning diagram of APP before and after coating. Ammonium polyphosphate without any treatment has sharp edges, sharp ends and smooth surface. After microencapsulation, the surface of PUAPP is rough, the edges disappear and it becomes spherical. Scaly structure can be seen on the coating layer. This is because the capsule material PU synthesized during the surface modification process accumulates on the surface of APP, which changes the surface morphology and roughness of APP.
[0106] Figure 4For flame retardant performance test. Among them, (a) is the maximum heat release rate (PHRR) diagram; (b) is the maximum total heat release (THR) diagram; (c) is the fire performance index (FPI) and fire growth index (FGI) bar graph. It can be observed from the figure that the carbon fiber epoxy composite material without any flame retardant has the highest maximum heat release rate (PHRR) and maximum total heat release (THR). After adding flame retardant microcapsules PUAPP to the carbon fiber epoxy resin composite material, the PHRR and THR values of the composite material have decreased to varying degrees, the FPI value increased, the FGI value decreased, and the fire hazard decreased. It shows that the addition of PUAPP is very effective in giving the material a flame retardant effect. This is mainly because after the ammonium polyphosphate core material is coated with polyurethane, a carbon source and a gas source are introduced on the surface of the ammonium polyphosphate, so that the microencapsulated APP particles form a carbon source, an acid source and a gas source, and more effectively form a hard carbon layer, which prevents oxygen and fire sources from contacting the surface of the composite material, thereby achieving the purpose of flame retardancy.
[0107] Table 1 further shows the test results of cone calorimetry. It can be clearly seen that after adding PUAPP, the PHRR of the carbon fiber epoxy composite material decreased by 11.47%, the THR decreased by 15.84%, and the FPI value increased and the FGI value decreased, which can all indicate that after adding PUAPP, the fire hazard is reduced. It is more intuitive that the addition of PUAPP improves the flame retardant properties of the carbon fiber epoxy composite material.
[0108] Table 1 Cone calorimetry test results of composite materials
[0109]
[0110] In summary, the present invention enhances the interfacial compatibility between epoxy resin and ammonium polyphosphate without sacrificing the original performance of ammonium polyphosphate, improves the flame retardant properties of carbon fiber epoxy composite materials, designs and prepares a flame retardant microcapsule with polyurethane as shell material and ammonium polyphosphate as core material, and adds it to the carbon fiber epoxy resin composite material. At the same time, the changes in the morphology, thermal stability and flame retardant properties of PUAPP when it acts on the carbon fiber epoxy matrix are studied. After APP is coated with a polyurethane shell, the poor water resistance of APP is changed, and the compatibility with the epoxy resin matrix is improved. The isocyanate group in the polyurethane shell will form a graft copolymer with the hydroxyl group in the epoxy resin to form a multi-scale enhancement, enhance the mechanical properties of the epoxy resin, and the polyurethane shell and ammonium polyphosphate can also achieve a synergistic flame retardant effect. A bridge is established between APP and the epoxy resin matrix to achieve the effect of strengthening and toughening the carbon fiber epoxy resin composite material and greatly improving the flame retardancy.
[0111] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A method for preparing a carbon fiber epoxy resin composite material based on microencapsulated flame retardant, characterized in that: include: S1: Using ammonium polyphosphate as the core material and polyurethane as the wall material, flame-retardant microcapsules PUAPP were prepared by in-situ polymerization; S2: The prepared flame-retardant microcapsule PUAPP is evenly dispersed into the epoxy resin E-51, applied on the carbon fiber cloth, and then cured to obtain a carbon fiber epoxy resin composite material.
2. The method for preparing a carbon fiber epoxy resin composite material based on microencapsulated flame retardant according to claim 1, characterized in that: The S1 specifically includes: S101: Dissolve PEG2000 in polyvinyl alcohol solution to obtain solution A S102: HDI trimer, emulsifier OP-10, ammonium polyphosphate, catalyst dibutyltin dilaurate and solvent dimethyl sulfoxide are mixed, and stirred with a magnetic stirrer until uniform to obtain solution B; S103: adding solution B dropwise into solution A to mix and disperse the mixture, and then taking out the emulsion and letting it stand to obtain a mixed solution C; S104: The mixed solution C is heated in a water bath for reaction, a chain extender 1,4-butanediol is added, the temperature is raised for reaction, the temperature is cooled to room temperature, and then centrifuged to obtain PUAPP.
3. The method for preparing a carbon fiber epoxy resin composite material based on microencapsulated flame retardant according to claim 2, characterized in that: In the S101, PEG2000 is dissolved in 150 mL of polyvinyl alcohol solution, and the mass fraction of the polyvinyl alcohol solution is 1.5%.
4. The method for preparing a carbon fiber epoxy resin composite material based on microencapsulated flame retardant according to claim 2, characterized in that: In S102, HDI trimer and PEG2000 are first reacted to generate polyurethane, which is then coated on the surface of ammonium polyphosphate. The molar ratio of HDI trimer and PEG2000 is (1.05-1.2):1; the mass ratio of polyurethane to ammonium polyphosphate is 1:(0.25-1.5).
5. The method for preparing a carbon fiber epoxy resin composite material based on microencapsulated flame retardant according to claim 2, characterized in that: In S103, solution B and solution A are mixed and dispersed in a homogenizer at a speed of 8000 to 10000 r / min for 10 to 30 minutes. The emulsion is taken out and allowed to stand for 15 to 30 minutes to obtain a mixed solution C.
6. The method for preparing a carbon fiber epoxy resin composite material based on microencapsulated flame retardant according to claim 2, characterized in that: In the S104, the addition of the chain extender 1,4-butanediol complies with the chain extension coefficient of 0.
90.
7. The method for preparing a carbon fiber epoxy resin composite material based on microencapsulated flame retardant according to claim 1, characterized in that: The S2 specifically includes: S201: evenly disperse the flame-retardant microcapsule PUAPP into the epoxy resin system, heat in a water bath and stir until uniform, add curing agent H256, heat in a water bath to make it flowable, and evenly apply it on a 10 cm×10 cm carbon fiber cloth; S202: placing the coated carbon fiber cloth into a mold preheated to 90° C., and curing the mold using a three-stage temperature rise method to obtain a carbon fiber epoxy resin composite material.
8. The method for preparing a carbon fiber epoxy resin composite material based on microencapsulated flame retardant according to claim 7, characterized in that: In the S201, the mass ratio of the epoxy resin system to the curing agent H256 is 100:
32.
9. The method for preparing a carbon fiber epoxy resin composite material based on microencapsulated flame retardant according to claim 7, characterized in that: In S202, the three-stage temperature rise curing is to keep the temperature at 90°C and normal pressure for 2 hours, then pressurize to 5MPa, then heat to 120°C and keep the temperature for 2 hours, and in the third stage, keep the temperature at 150°C for 3 hours.
10. A carbon fiber epoxy resin composite material based on microencapsulated flame retardant, characterized in that: The method is prepared by any one of claims 1 to 9.
Citation Information
Patent Citations
Aqueous polyurethane micro-encapsulated halogen-free flame retardant and preparation thereof
CN101503526A
Microencapsulation expansion type flame retardant and application in epoxy resin composite material thereof
CN101812186A
Flame-retardant bio-based polyurethane hose and production method thereof
CN108253207A
Continuous carbon fiber reinforced flame-retardant epoxy resin composite material and preparation method thereof
CN115819922A