Yellow fluorescent material excited by purple light as well as preparation and application of yellow fluorescent material
By developing the yellow fluorescent material Cs2Mn1-xEuxCl4 excited by violet light, the problems of unstable color temperature and blue light hazard in the existing white light LED technology have been solved, and the efficient emission of yellow light under violet light excitation has been achieved. It is suitable for a variety of LED applications and provides health benefits. and efficient lighting solutions.
Patent Information
- Application Number
- CN202410754089.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-12
- Publication Date
- 2024-10-15
AI Technical Summary
The existing white light LED technology has problems such as unstable color temperature, low color rendering index and blue light hazards, especially the uneven luminous intensity and health risks caused by the strong wave peak of the blue light chip.
Develop a yellow fluorescent material excited by purple light, with the chemical expression Cs2Mn1-xEuxCl4. By reducing an additional 5% of the cesium source compound in the cesium source compound to eliminate the CsCl impurity phase, it is prepared in a reducing atmosphere using high-temperature sintering to form Eu2+ Doped lead-free halide-based 566nm yellow light-emitting phosphor is used to combine with a violet chip to produce white light.
A yellow fluorescent material with a wide excitation band is realized, which can emit 566nm yellow light under excitation of 400nm violet light. It has stable physical and chemical properties and is suitable for white LEDs, solar-like LEDs and full-spectrum LEDs. It avoids the hazards of high color temperature and blue light and meets the requirements meet the demand for healthy lighting.
Smart Images

Figure CN118772874A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of fluorescent materials, and in particular to a yellow fluorescent material excited by violet light and the preparation and application thereof. Background Art
[0002] With the rapid development of the economy, people's living standards are also constantly improving, and the requirements for lighting quality are getting higher and higher. Considering the increasing importance of energy saving and environmental protection, solid-state lighting (SSL) is becoming a very competitive field and may replace existing lighting technologies. White light-emitting diodes (W-LEDs) have been widely studied and applied due to their advantages such as low power consumption, high stability and excellent luminous efficiency. There are currently two common methods to obtain this white light; one is to synthesize white light through a multi-chip set of red, green and blue primary colors and light emission, but due to the different light decay of the three primary color chips, the color temperature is unstable, the control circuit is more complicated, and the cost is higher. Another method is to combine InGaN blue light chips with yellow phosphor Y3Al5O 12 :Ce 3+ (YAG:Ce 3+ ), this method has a strong blue light chip peak, and the blue light part is too strong, resulting in uneven luminous intensity, low color rendering index, high color temperature, and certain blue light hazards that are not conducive to physical and mental health. Therefore, we look for high quantum efficiency yellow phosphors and blue phosphors that are effectively excited in the purple light region and combine them with purple light chips to produce white light. This method can effectively avoid low color rendering index, high color temperature and blue light hazards, and is a method with application prospects. Therefore, the synthesis of yellow phosphors with strong absorption in the purple light region plays an important role in healthy lighting.
[0003] Lead-free halide-based perovskites are gaining increasing attention as an emerging, non-toxic alternative to lead-based perovskites. Summary of the invention
[0004] In order to solve the above problems, the purpose of the present invention is to provide a yellow fluorescent material excited by violet light and its preparation and application. The yellow fluorescent material excited by violet light provided by the present invention is a violet light excited Eu 2+ The doped lead-free halide-based 566nm yellow light-emitting phosphor can meet the current urgent needs of white light LEDs, sunlight-like LEDs, and full-spectrum LEDs.
[0005] The purpose of the present invention can be achieved by the following technical solutions:
[0006] The first object of the present invention is to provide a yellow fluorescent material excited by violet light, the chemical expression of which is Cs2Mn 1-x Eu x Cl4, where 0.01≤x≤0.11.
[0007] In one embodiment of the present invention, x is 0.01, 0.03, 0.05, 0.07, 0.09 or 0.11.
[0008] In one embodiment of the present invention, the yellow fluorescent material is a powdery material.
[0009] In one embodiment of the present invention, the excitation spectrum of the yellow fluorescent material is in the range of 200 to 450 nm, the emission spectrum is in the range of 500 to 700 nm, and the central emission wavelength of yellow light is 566 nm.
[0010] A second object of the present invention is to provide a method for preparing a yellow fluorescent material excited by violet light, comprising the following steps:
[0011] (S1) grinding and mixing the cesium source compound, the manganese source compound, and the europium source compound to obtain a mixed powder;
[0012] (S2) The mixed powder prepared in step (S1) is subjected to sintering treatment and cooling treatment in sequence to obtain a yellow fluorescent material excited by violet light.
[0013] In one embodiment of the present invention, in step (S1), according to the chemical formula of the fluorescent material Cs2Mn 1- x Eu x Cl4, wherein 0.01≤x≤0.11, is prepared on the basis of various raw materials, and then an additional 5% of the cesium source compound is reduced on the basis of the calculated amount of the cesium source compound as the cesium source reduction.
[0014] Among them, according to the chemical expression of fluorescent materials Cs2Mn 1-x Eu x Cl4, where 0.01≤x≤0.11, based on the preparation of various raw materials, when the cesium source compound is added normally, an additional CsCl impurity phase will appear in the product; when the amount of the cesium source compound added is additionally reduced by 5%, the additional CsCl impurity phase disappears, and the XRD phase purity of the product is purer.
[0015] In one embodiment of the present invention, in step (S1), the cesium source compound is CsCl powder, the manganese source compound is MnCl2 powder, and the europium source compound is EuCl3 powder.
[0016] In one embodiment of the present invention, in step (S1), during the grinding process, the grinding time is 5 to 120 minutes.
[0017] In one embodiment of the present invention, in step (S2), the high temperature sintering process is carried out in a reducing atmosphere, the temperature is 500 to 1500° C., and the time is 2 to 12 hours.
[0018] In one embodiment of the present invention, the reducing atmosphere is selected from a mixed gas of CO, H2 and N2, or a mixed gas of CO, H2 and N2.
[0019] In one embodiment of the present invention, the reducing atmosphere is a mixed gas of 5% by volume H2 and 95% by volume N2 (referred to as "5% H2-95% N2").
[0020] The third object of the present invention is to provide a yellow fluorescent material excited by violet light for use in preparing LED chips.
[0021] The fourth object of the present invention is to provide an LED chip containing the yellow fluorescent material excited by the above-mentioned violet light.
[0022] In the fluorescent material system, all-inorganic lead-free halides are considered to be high-brightness fluorescent materials due to their large carrier diffusion length, high photoluminescence quantum yield, adjustable band gap, and excellent optoelectronic properties. At the same time, all-inorganic lead-free halides have good chemical stability and environmental friendliness, and show great application prospects in the fields of light-emitting diodes (LEDs), solar cells, lasers, and bio-imaging. Therefore, the all-inorganic lead-free halide system is a very promising fluorescent material.
[0023] Compared with the prior art, the present invention has the following beneficial effects:
[0024] (1) The yellow fluorescent material excited by violet light of the present invention has a wide excitation band, and the effective absorption range covers 200-450nm, and can be excited by violet light. The obtained fluorescent powder can emit yellow light with a central wavelength of 566nm under the excitation of 400nm violet light.
[0025] (2) The yellow fluorescent material excited by violet light of the present invention is Eu 2+ The doped halide-based 566nm yellow light-emitting phosphor has the advantage of stable physical and chemical properties. At the same time, the phosphor can be prepared by a conventional solid-phase reaction method, has the characteristics of simple preparation process and is conducive to industrial production. It can be used as a good candidate material for the widespread application of white light LEDs and has broad application prospects.
[0026] (3) The emission wavelength of the yellow fluorescent material excited by violet light of the present invention is 500 to 700 nm, which can effectively absorb light in the wavelength range of 200 to 450 nm. It can be well matched with the existing violet light chip, meet the needs of the commercial market, and is suitable for applications in white light LEDs, sunlight-like LEDs, full-spectrum LEDs, etc. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1 The photoexcitation / emission spectra of the yellow fluorescent materials excited by violet light prepared in Example 1, Example 2, and Example 3;
[0028] Figure 2 These are the XRD diffraction patterns of the yellow fluorescent materials excited by violet light prepared in Example 1, Example 2, and Example 3. DETAILED DESCRIPTION
[0029] The present invention is described in detail below with reference to the accompanying drawings and specific embodiments.
[0030] In the following examples, unless otherwise specified, all reagents used are commercially available reagents, and all detection means and methods used are conventional detection means and methods in the art.
[0031] Example 1
[0032] This embodiment provides a method for preparing a yellow fluorescent material excited by violet light, and the specific steps are as follows:
[0033] (S1) weighing 1 g of raw material powders of CsCl, MnCl2 and EuCl3 according to the stoichiometric ratio, and further reducing 5% of CsCl (the mass ratio of each raw material is CsCl:MnCl2:EuCl3=0.6896:0.2686:0.0056), and mixing to obtain a raw material mixture;
[0034] (S2) grinding the raw material mixture obtained in step (S1) in an agate mortar for 45 minutes until the raw materials are evenly mixed to obtain a mixture;
[0035] (S3) The mixture prepared in step (S2) is loaded into an alumina crucible, and placed in a reducing atmosphere of hydrogen and nitrogen mixture (5% H2-95% N2) for sintering at 750°C for 8h (pressure is 0MPa), and then cooled to room temperature to obtain a purple light excited yellow fluorescent material (whose photoexcitation / emission spectrum is shown in FIG. Figure 1 As shown, the XRD diffraction pattern is Figure 2 shown).
[0036] analyze:
[0037] The spectral properties of the yellow fluorescent material were tested using a fluorescence spectrometer (HITACHI F-7000). Figure 1The results show that the yellow fluorescent material has a wide excitation band with a peak value near 400nm and a high spectral peak, which can match well with the purple light commercial chip; under the excitation of a 400nm purple light source, the yellow fluorescent material emits yellow light, and the emission spectrum consists of a wide emission band (500-700nm) with a peak value at 566nm.
[0038] The crystal structure of the yellow fluorescent material prepared above was tested by X-ray diffraction (Ultima IV-185). Cu-Kα was used as the target material, and the scanning angle 2θ range was 5 to 80°. The XRD ray diffraction pattern was as follows: Figure 2 As shown, from Figure 2 It can be seen that the yellow fluorescent material is consistent with the standard card (PDF#04-006-8998), indicating that Eu 3+ The doping of ions does not have a significant effect on the crystal structure, and the obtained yellow fluorescent material is a pure phase substance isomorphous with Cs2MnCl4. Its fluorescence emission spectrum data shows that the emission of the yellow fluorescent material is in the yellow light region, and it can be used as a good yellow light emitting fluorescent material suitable for white light LEDs.
[0039] The general formula of the purple light excited Eu doped yellow fluorescent material obtained in this embodiment is Cs2Mn 1-x Eu x Cl4, x is 0.01.
[0040] Example 2
[0041] This embodiment provides a method for preparing a yellow fluorescent material excited by violet light, and the specific steps are as follows:
[0042] (S1) weighing 1 g of raw material powders of CsCl, MnCl2 and EuCl3 according to the stoichiometric ratio, and further reducing 5% of CsCl (the mass ratio of each raw material is CsCl:MnCl2:EuCl3=0.6856:0.2651:0.0111), and mixing to obtain a raw material mixture;
[0043] (S2) grinding the raw material mixture obtained in step (S1) in an agate mortar for 45 minutes until the raw materials are evenly mixed to obtain a mixture;
[0044] (S3) The mixture prepared in step (S2) is loaded into an alumina crucible, and placed in a reducing atmosphere of hydrogen and nitrogen mixture (5% H2-95% N2) for sintering at 700°C for 8h (pressure is 0MPa), and then cooled to room temperature to obtain a yellow fluorescent material excited by violet light (its photoexcitation / emission spectrum is shown in FIG. Figure 1 As shown, the XRD diffraction pattern is Figure 2 shown).
[0045] The general formula of the purple light excited Eu doped yellow fluorescent material obtained in this embodiment is Cs2Mn 1-x Eu x Cl4, x is 0.03.
[0046] Example 3
[0047] This embodiment provides a method for preparing a yellow fluorescent material excited by violet light, and the specific steps are as follows:
[0048] (S1) weighing 1 g of raw material powders of CsCl, MnCl2 and EuCl3 according to the stoichiometric ratio, and further reducing 5% of CsCl (the mass ratio of each raw material is CsCl:MnCl2:EuCl3=0.6818:0.2548:0.0275), and mixing to obtain a raw material mixture;
[0049] (S2) grinding the raw material mixture obtained in step (S1) in an agate mortar for 45 minutes until the raw materials are evenly mixed to obtain a mixture;
[0050] (S3) The mixture prepared in step (S2) is loaded into an alumina crucible, and placed in a reducing atmosphere of hydrogen and nitrogen mixture (5% H2-95% N2) for sintering at 750°C for 10 h (pressure is 0 MPa), and then cooled to room temperature to obtain a purple light excited yellow fluorescent material (whose photoexcitation / emission spectrum is shown in FIG. Figure 1 As shown, the XRD diffraction pattern is Figure 2 shown).
[0051] The general formula of the purple light excited Eu doped yellow light emitting phosphor obtained in this embodiment is Cs2Mn 1-x Eu x Cl4, x is 0.05.
[0052] Example 4
[0053] This embodiment provides a method for preparing a yellow fluorescent material excited by violet light, and the specific steps are as follows:
[0054] (S1) weighing 1 g of raw material powders of CsCl, MnCl2 and EuCl3 according to the stoichiometric ratio, and further reducing 5% of CsCl (the mass ratio of each raw material is CsCl:MnCl2:EuCl3=0.6779:0.2480:0.0383), and mixing them to obtain a raw material mixture;
[0055] (S2) grinding the raw material mixture obtained in step (S1) in an agate mortar for 45 minutes until the raw materials are evenly mixed to obtain a mixture;
[0056] (S3) The mixture prepared in step (S2) is loaded into an alumina crucible, placed in a reducing atmosphere of a hydrogen and nitrogen mixture (5% H2-95% N2) and sintered at 650°C for 12 hours (pressure is 0 MPa), and then cooled to room temperature to obtain a yellow fluorescent material excited by violet light.
[0057] The general formula of the purple light excited Eu doped yellow light emitting phosphor obtained in this embodiment is Cs2Mn 1-x Eu x Cl4, x is 0.07.
[0058] Example 5
[0059] This embodiment provides a method for preparing a yellow fluorescent material excited by violet light, and the specific steps are as follows:
[0060] (S1) weighing 1 g of raw material powders of CsCl, MnCl2 and EuCl3 according to the stoichiometric ratio, and further reducing 5% of CsCl (the mass ratio of each raw material is CsCl:MnCl2:EuCl3=0.6742:0.2414:0.0596), and mixing to obtain a raw material mixture;
[0061] (S2) grinding the raw material mixture obtained in step (S1) in an agate mortar for 45 minutes until the raw materials are evenly mixed to obtain a mixture;
[0062] (S3) The mixture prepared in step (S2) is loaded into an alumina crucible, and placed in a reducing atmosphere of a hydrogen and nitrogen mixture (5% H2-95% N2) for sintering at 700°C for 9 hours (pressure is 0 MPa), and then cooled to room temperature to obtain a yellow fluorescent material excited by violet light.
[0063] The general formula of the purple light excited Eu doped yellow light emitting phosphor obtained in this embodiment is Cs2Mn 1-x Eu x Cl4, x is 0.09.
[0064] Example 6
[0065] This embodiment provides a method for preparing a yellow fluorescent material excited by violet light, and the specific steps are as follows:
[0066] (S1) weighing 1 g of raw material powders of CsCl, MnCl2 and EuCl3 according to the stoichiometric ratio, and further reducing 5% of CsCl (the mass ratio of each raw material is CsCl:MnCl2:EuCl3=0.6704:0.2347:0.0490), and mixing to obtain a raw material mixture;
[0067] (S2) grinding the raw material mixture obtained in step (S1) in an agate mortar for 45 minutes until the raw materials are evenly mixed to obtain a mixture;
[0068] (S3) The mixture prepared in step (S2) is loaded into an alumina crucible, and placed in a reducing atmosphere of a hydrogen and nitrogen mixture (5% H2-95% N2) for sintering at 800°C for 10 hours (pressure is 0 MPa), and then cooled to room temperature to obtain a yellow fluorescent material excited by violet light.
[0069] The general formula of the purple light excited Eu doped yellow light emitting phosphor obtained in this embodiment is Cs2Mn 1-x Eu x Cl4, x is 0.11.
[0070] Table 1 Preparation parameters of Examples 1 to 6
[0071]
[0072]
[0073] The above description of the embodiments is to facilitate the understanding and use of the invention by those skilled in the art. It is obvious that those skilled in the art can easily make various modifications to these embodiments and apply the general principles described herein to other embodiments without creative work. Therefore, the present invention is not limited to the above embodiments, and improvements and modifications made by those skilled in the art based on the explanation of the present invention without departing from the scope of the present invention should be within the scope of protection of the present invention.
Claims
1. A yellow fluorescent material excited by violet light, characterized in that: The chemical expression of the yellow fluorescent material is Cs2Mn 1-x Eu x Cl4, where 0.01≤x≤0.
11.
2. The yellow fluorescent material excited by violet light according to claim 1, characterized in that: x is 0.01, 0.03, 0.05, 0.07, 0.09 or 0.
11.
3. The yellow fluorescent material excited by violet light according to claim 1, characterized in that: The yellow fluorescent material is a powdery material.
4. The yellow fluorescent material excited by violet light according to claim 1, characterized in that: The excitation spectrum range of the yellow fluorescent material is 200-450nm, the emission spectrum range is 500-700nm, and the central emission wavelength of yellow light is 566nm.
5. A method for preparing a yellow fluorescent material excited by violet light as claimed in any one of claims 1 to 4, characterized in that: The following steps are involved: (S1) grinding and mixing the cesium source compound, the manganese source compound, and the europium source compound to obtain a mixed powder; (S2) The mixed powder prepared in step (S1) is subjected to sintering treatment and cooling treatment in sequence to obtain a yellow fluorescent material excited by violet light.
6. The method for preparing a yellow fluorescent material excited by violet light according to claim 5, characterized in that: In step (S1), according to the chemical formula of the fluorescent material Cs2Mn 1-x Eu x Cl4, wherein 0.01≤x≤0.11, an additional 5% of the cesium source compound is reduced based on the calculated amount of the cesium source compound as the cesium source reduction.
7. The method for preparing a yellow fluorescent material excited by violet light according to claim 5, characterized in that: In step (S2), during the high temperature sintering process, the temperature is 500 to 1500° C. and the time is 2 to 12 hours in a reducing atmosphere.
8. The method for preparing a yellow fluorescent material excited by violet light according to claim 7, characterized in that: The reducing atmosphere is a mixed gas of 5% by volume H2 and 95% by volume N2.
9. Use of the yellow fluorescent material excited by violet light as claimed in any one of claims 1 to 4 in the preparation of LED chips.
10. An LED chip, characterized in that: Contains the yellow fluorescent material excited by violet light as claimed in any one of claims 1 to 4.
Citation Information
Patent Citations
Ultraviolet-excited blue fluorescent material as well as preparation method and application thereof
CN119286523A