Method for controlling silicon content in SWRCH22A cold forging steel

By using slag-stopping plugs, sliding plate slag-stopping devices and automated control systems in the production of SWRCH22A cold heading steel, combined with the optimized refining process, the problem of difficult control of silicon content is solved, achieving effective control of silicon content and reduction of production costs.

CN118773401APending Publication Date: 2024-10-15LINGYUAN IRON & STEEL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410900901.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-05
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

In the production process of SWRCH22A cold heading steel, it is difficult to control the silicon content below 0.06%, resulting in the problem of scrapping the steel.

Method used

By using slag-stopping plugs, slag-stopping cones and sliding plate slag-stopping devices combined with automated control systems in converter smelting, the amount of slag and ladle residues can be reduced, the refining time can be shortened, the silica content can be reduced, and clean ladles without residues can be used and deoxidation can be optimized. alloying process.

Benefits of technology

It effectively controls the silicon content of SWRCH22A cold heading steel, reduces production costs, improves product quality, and avoids scrapping of steel.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention belongs to the field of cold forging steel preparation, and discloses a method for controlling the silicon content in SWRCH22A cold forging steel. The method comprises the following steps: performing converter smelting or electric furnace smelting by using an SWRCH22A cold heading steel steelmaking raw material to obtain molten steel, and performing slag-stopping tapping by adopting a slag-stopping plug, a slag-stopping cone, a sliding plate slag-stopping device and slag-tapping detection equipment, so that the molten steel flows into a steel ladle without residues and is deoxidized and alloyed to obtain outbound molten steel; and LF refining treatment is conducted on the outbound molten steel, and LF refined molten steel is obtained. The method is applied to the ferrous metallurgy industry, the content of silicon dioxide is reduced by reducing the slag amount in the molten steel, meanwhile, the refining treatment time is shortened, reduced silicon return in the refining process is reduced, and the silicon content of the SWRCH22A cold forging steel in the production process is controlled to be 0.06% or below.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of cold heading steel preparation, and more specifically, relates to a method for controlling the silicon content in SWRCH22A cold heading steel. Background Art

[0002] Cold heading steel wire is the most widely used raw material in the fastener industry. It is mainly used to manufacture fasteners such as bolts, nuts, screws, and self-tapping screws. It is widely used in the machinery industry, automobile manufacturing industry, and construction industry. Its deformation speed is fast and the deformation amount is large during the processing process, which is easy to cause drawing and cold heading cracking. Cold heading steel wire is required to have good mechanical properties and processing properties. The steel types of cold heading steel wire are generally low-carbon and medium-carbon high-quality carbon structural steel and low-alloy steel. Due to its good cold forming performance, cold heading steel is used in the mechanical processing industry instead of hot-rolled material cutting machine processing. The advantage of this process is that while saving a lot of man-hours, metal consumption can be reduced by 10%-30%, which is in line with clean production and resource-saving enterprises. The large-scale production, the product size accuracy is high, the surface finish is good, and the production efficiency is high. It is an advanced machining process that is promoted. After entering the mid-1980s, high-speed wire production lines were put into production one after another, providing equipment guarantees for the production of cold heading steel wire. Since the beginning of the 21st century, the variety of cold heading steel developed has been increasing, the output has been growing, and the quality has been improving. Obviously, the development and production of cold heading steel wire has formed a certain scale. SWRCH22A cold heading steel wire is a typical steel type for making self-tapping screws. Due to its processing characteristics, the material must have good drawing performance, high cold heading forming and thread rolling pass rate. High silicon content in steel will increase the work hardening rate, causing the strength of the steel wire to increase during the cold drawing process and reduce the cold heading performance of the steel. The silicon content should be strictly controlled to be no more than 0.06%.

[0003] The standard (JIS G3057-1:2005 standard) for SWRCH22A cold heading steel wire rod is: C0.18%-0.23%, Mn 0.70%-1.00%, Si≤0.10%, S≤0.035%, P≤0.030%, Alt≥0.020%. The smelting adopts top and bottom combined blowing converter smelting and deep deoxidation process of aluminum ingots; LF refining adopts white slag operation, calcium treatment, and double-permeable brick argon blowing for the ladle; continuous casting adopts crystallizer electromagnetic stirring and solidification end electromagnetic stirring technology; crystallizer liquid level automatic control technology is adopted. In order to ensure that the silicon content in SWRCH22A cold heading steel is qualified, converter alloying generally does not use silicon-containing materials, but the Si content of some furnaces will still exceed the standard range during the continuous casting process. The reason is:

[0004] 1. During the steel tapping process of the converter, slag stopper and slag stopper cone are used to stop slag during steel tapping, so as to reduce the amount of slag in the converter. However, slag will inevitably occur during steel tapping, and the amount of slag cannot be controlled.

[0005] 2. During the production process, it was found that there was a lot of residue on the bottom and wall of the ladle;

[0006] 3. In order to ensure the retention time of white slag in the refining process and better remove inclusions in the steel, the refining time is extended, resulting in serious silicon return in the refining process; or, in order to achieve a better removal of inclusions during the refining process, more aluminum wire or aluminum particles need to be added to deoxidize the slag. The SiO2 in the slag is reduced to Si by Al and enters the molten steel, resulting in Si return in the LF furnace treatment process. There is an aluminum-oxygen balance in the steel slag, and the principle of aluminum in steel reducing silicon dioxide in the slag is: AL+SiO2=AL2O3+Si.

[0007] The above reasons, such as the amount of slag in the converter, the residue in the ladle and the long-term refining, deoxidation and reduction, result in the silicon content exceeding the standard in the production process, which eventually leads to the steel being scrapped.

[0008] Therefore, it is urgent to propose a method for controlling the silicon content in SWRCH22A cold heading steel so that the silicon content of SWRCH22A cold heading steel is controlled below 0.06% during the production process. Summary of the invention

[0009] The purpose of the present invention is to propose a method for controlling the silicon content in SWRCH22A cold heading steel in view of the deficiencies of the prior art. The present invention is applied in the iron and steel metallurgical industry, and reduces the amount of slag in molten steel, thereby reducing the silicon dioxide content, while reducing the refining treatment time and reducing the silicon reduction in the refining process, so that the silicon content of SWRCH22A cold heading steel is controlled below 0.06% during the production process.

[0010] The present invention is based on the existing method for smelting SWRCH22A cold heading steel (the smelting adopts top and bottom combined blowing converter smelting and aluminum ingot deep deoxidation process; LF refining adopts white slag operation and calcium treatment, and the ladle adopts double-permeable brick argon blowing; continuous casting adopts crystallizer electromagnetic stirring and solidification end electromagnetic stirring technology; and crystallizer liquid level automatic control technology).

[0011] In order to achieve the above object, the present invention provides a method for controlling the silicon content in SWRCH22A cold heading steel, the method comprising the following steps:

[0012] S1: Using SWRCH22A cold heading steel steelmaking raw material to carry out converter smelting or electric furnace smelting to obtain molten steel and using slag blocking plug, slag blocking cone, slide plate slag blocking device and slag lowering detection equipment to carry out slag blocking steel tapping, so that the molten steel flows into a ladle without residue and is deoxidized and alloyed to obtain outlet molten steel;

[0013] S2: performing LF refining treatment on the outgoing molten steel to obtain LF refined molten steel.

[0014] According to the present invention, preferably, the slide plate slag blocking device is installed at the molten steel outlet of the converter or electric furnace;

[0015] The slag detection device is arranged on a fixed building behind the converter or electric furnace, and is interlocked with the slide slag blocking device through an automatic control system; a program for controlling the opening and closing of the slide slag blocking device is preset in the automatic control system;

[0016] The slag detection device is used to detect whether there is smelting final slag in the molten steel discharged during slag blocking and steel tapping; when the slag detection device detects that smelting final slag is discharged, the slide plate slag blocking device is controlled to be closed through the automatic control system to avoid the discharge of smelting final slag.

[0017] According to the present invention, preferably, the method further comprises: sequentially performing continuous casting, billet cutting and rolling on the LF refined molten steel to obtain SWRCH22A cold heading steel.

[0018] In the present invention, the production process of the SWRCH22A cold heading steel of the present invention can be summarized as: converter or electric furnace smelting → steel alloying → argon blowing station → LF furnace refining → continuous casting → ingot cutting → rolling.

[0019] According to the present invention, preferably, after the LF refined steel liquid is continuously cast, the residue in the ladle containing the LF refined steel liquid is poured into a slag pot to obtain the ladle without residue;

[0020] The residue content in the residue-free ladle is 0.1 ton-0.2 ton, and the silicon dioxide content in the residue is 6%-10%.

[0021] According to the present invention, preferably, the material used for the deoxidation alloying is at least one of aluminum ingots, calcium carbide and aluminum particles; further preferably, the material used for the deoxidation alloying is: aluminum ingots 1.0-3.0 kg / t, calcium carbide 0.6-2.5 kg / t, aluminum particles 0.3-2.0 kg / t.

[0022] According to the present invention, preferably, the method further comprises: before the LF refining treatment, blowing argon into the outgoing molten steel until it enters the LF refining station.

[0023] According to the present invention, preferably, the method for controlling silicon content in SWRCH22A cold heading steel according to claim 1, wherein the LF refining treatment includes electrification, white slag refining, component quenching and tempering, and calcium feeding wire treatment;

[0024] The time for the white slag refining treatment is 45-55 min / furnace.

[0025] According to the present invention, preferably, the deoxidizer used in the LF refining process is calcium carbide and / or aluminum particles; further preferably, the deoxidizer used in the LF refining process is: calcium carbide 0.6-1.0 kg / t, aluminum particles 0.3-1.0 kg / t.

[0026] According to the present invention, preferably, based on the total weight of the SWRCH22A cold heading steel, Si≤0.06%, C 0.19%-0.22%, Mn 0.81%-0.85%, S≤0.010%, P≤0.020%, and Alt≥0.025% in the SWRCH22A cold heading steel.

[0027] According to the present invention, preferably, the size of the SWRCH22A cold heading steel is φ6-7mm.

[0028] The beneficial effects of the technical solution of the present invention are as follows:

[0029] The present invention controls the silicon content in the molten steel of the converter steel tapping by reducing the amount of slag during the steel tapping process and using a clean ladle without residue to avoid the presence of a large amount of SiO2. The present invention adopts a slag blocking method that combines slag blocking with slag plugs, slag blocking cones, and slide plates with slag detection during the converter steel tapping, thereby reducing the amount of converter slag, thereby reducing the silicon dioxide content in the molten steel (this is because the converter smelting is an oxidizing atmosphere, and the silicon element in the molten iron is almost completely oxidized into the slag after the converter smelting, and the SiO2 content in the converter final slag is generally 12%-20%, with an average content of 17.5%), thereby reducing the generation of silicon elements at the source. The present invention overcomes the problems of unstable converter slag amount, inconvenient operation and precise control that are easy to occur in the existing process.

[0030] The ladle used in the present invention is a clean ladle without residue, because, usually, the residue in the ladle is mainly refined slag and covering agent components, and the SiO2 content in the residue is generally 6%-10%, with an average content of 8.2%. Reducing the residue in the ladle and using a clean ladle without residue can effectively reduce the subsequent refining deoxidation reduction back to silicon.

[0031] The present invention reduces the refining treatment time from 90 min / furnace to 45-55 min / furnace, thereby greatly reducing the further increase of silicon return caused by long-term deoxidation in the refining process.

[0032] The present invention can reduce the amount of slag while ensuring that the actual production and use of SWRCH22A cold heading steel meet the standard requirements, thereby reducing the consumption of deoxidizers (aluminum, calcium carbide, etc.) used in the converter steelmaking and refining process, and shortening the refining time. Therefore, the present invention also effectively reduces the production cost.

[0033] Other features and advantages of the present invention will be described in detail in the following detailed description. DETAILED DESCRIPTION

[0034] The preferred embodiments of the present invention will be described in more detail below. Although the preferred embodiments of the present invention are described below, it should be understood that the present invention can be implemented in various forms and should not be limited by the embodiments set forth herein. On the contrary, these embodiments are provided to make the present invention more thorough and complete, and to fully convey the scope of the present invention to those skilled in the art.

[0035] Example 1

[0036] This embodiment provides a method for controlling the silicon content in SWRCH22A cold heading steel, the method comprising the following steps:

[0037] S1: Using SWRCH22A cold heading steel steelmaking raw material to carry out top and bottom double blowing converter smelting to obtain molten steel and using slag blocking plug, slag blocking cone, slide plate slag blocking device and slag lowering detection equipment to carry out slag blocking steel tapping, so that the molten steel flows into a ladle without residue and is deoxidized and alloyed to obtain outlet molten steel;

[0038] in:

[0039] The slide slag blocking device is installed at the molten steel outlet of the converter or electric furnace; the slag lowering detection device is arranged on a fixed building behind the converter or electric furnace, and is interlocked with the slide slag blocking device through an automatic control system; a program for controlling the opening and closing of the slide slag blocking device is preset in the automatic control system; the slag lowering detection device is used to detect whether there is smelting final slag in the molten steel discharged during slag blocking and steel tapping; when the slag lowering detection device detects that smelting final slag is discharged, the slide slag blocking device is controlled to be closed through the automatic control system to avoid the discharge of smelting final slag;

[0040] The materials used for the deoxidation alloying are 1.5 kg / t of aluminum ingot, 0.8 kg / t of calcium carbide, and 0.5 kg / t of aluminum granules;

[0041] S2: Blowing argon into the outgoing molten steel until it enters the LF refining station and undergoes LF refining treatment to obtain LF refined molten steel;

[0042] The LF refining process includes electrification, white slag refining, component tempering and calcium feeding line treatment;

[0043] The time of the white slag refining treatment is 50min / furnace;

[0044] The deoxidizer used in the LF refining process is 0.8kg / t of calcium carbide and 0.5kg / t of aluminum particles;

[0045] S3: sequentially performing continuous casting, billet cutting and rolling on the LF refined molten steel to obtain SWRCH22A cold heading steel;

[0046] After the LF refined steel liquid is continuously cast, the residue in the ladle containing the LF refined steel liquid is poured into a slag pot to obtain the ladle without residue, which is used in step S1; the residue content in the ladle without residue is 0.1 ton-0.2 ton, and the silicon dioxide content in the residue is 6%-10%.

[0047] Based on the total weight of the SWRCH22A cold heading steel described in this embodiment, Si≤0.06%, C 0.19%-0.22%, Mn 0.81%-0.85%, S≤0.010%, P≤0.020%, and Alt≥0.025% in the SWRCH22A cold heading steel described in this embodiment.

[0048] The size of the SWRCH22A cold heading steel is φ6.5 mm.

[0049] Example 2

[0050] This embodiment provides a method for controlling the silicon content in SWRCH22A cold heading steel. The difference between this embodiment and Example 1 is that the time of the white slag refining treatment is 90 min / furnace, and the deoxidizers used in the LF refining treatment are calcium carbide and aluminum particles, with an amount of 2.0 kg / t of calcium carbide and 1.5 kg / t of aluminum particles.

[0051] Based on the total weight of the SWRCH22A cold heading steel described in this embodiment, Si≤10%, C 0.19%-0.23%, Mn 0.81%-0.86%, S≤0.008%, P≤0.020%, Alt≥0.025% in the SWRCH22A cold heading steel described in this embodiment. When the refining treatment time is extended to 90min / furnace, the consumption of the refining deoxidizer increases, and as the refining time increases, the deoxidation reduction back to silicon is serious in the refining process.

[0052] Example 3

[0053] This embodiment provides a method for controlling the silicon content in SWRCH22A cold heading steel. The difference between this embodiment and Example 1 is that the time of the white slag refining treatment is 35 min / furnace, and the deoxidizer used in the LF refining treatment is 0.8 kg / t of calcium carbide and 0.5 kg / t of aluminum particles.

[0054] Based on the total weight of the SWRCH22A cold heading steel described in this embodiment, Si≤6%, C 0.18%-0.23%, Mn 0.78%-0.88%, S≤0.020%, P≤0.020%, Alt≥0.030% in the SWRCH22A cold heading steel described in this embodiment. After the refining treatment time is shortened to 35min / furnace, the control range of the refined outgoing composition is increased, and the fluctuation of the chemical composition leads to unstable product performance.

[0055] Comparative Example 1

[0056] This comparative example provides a method for preparing SWRCH22A cold heading steel. The difference between this comparative example and Example 1 is that: no slag detection equipment is set when slag blocking and steel tapping;

[0057] The molten steel is flowed into a ladle having a residue content of 0.4 ton to 0.8 ton and a silicon dioxide content of 6% to 10% in the residue;

[0058] Based on the total weight of the SWRCH22A cold heading steel in the comparative example, Si≤0.10%, C: 0.19%-0.22%, Mn: 0.81%-0.86%, S≤0.015%, P≤0.020%, and Alt≥0.025% in the SWRCH22A cold heading steel in the comparative example.

[0059] The embodiments of the present invention have been described above, and the above description is exemplary, not exhaustive, and is not limited to the disclosed embodiments. Many modifications and changes will be apparent to those skilled in the art without departing from the scope and spirit of the described embodiments.

Claims

1. A method for controlling the silicon content in SWRCH22A cold heading steel, characterized in that: The method comprises the following steps: S1: Using SWRCH22A cold heading steel steelmaking raw material to carry out converter smelting or electric furnace smelting to obtain molten steel and using slag blocking plug, slag blocking cone, slide plate slag blocking device and slag lowering detection equipment to carry out slag blocking steel tapping, so that the molten steel flows into a ladle without residue and is deoxidized and alloyed to obtain outlet molten steel; S2: performing LF refining treatment on the outgoing molten steel to obtain LF refined molten steel.

2. The method for controlling the silicon content in SWRCH22A cold heading steel according to claim 1, wherein: The slide plate slag blocking device is installed at the molten steel outlet of the converter or electric furnace; The slag detection device is arranged on a fixed building behind the converter or electric furnace, and is interlocked with the slide slag blocking device through an automatic control system; a program for controlling the opening and closing of the slide slag blocking device is preset in the automatic control system; The slag detection device is used to detect whether there is smelting final slag in the molten steel discharged during slag blocking and steel tapping; when the slag detection device detects that smelting final slag is discharged, the slide plate slag blocking device is controlled to be closed through the automatic control system to avoid the discharge of smelting final slag.

3. The method for controlling silicon content in SWRCH22A cold heading steel according to claim 1, wherein: The method further comprises: sequentially performing continuous casting, billet cutting and rolling on the LF refined molten steel to obtain SWRCH22A cold heading steel.

4. The method for controlling the silicon content in SWRCH22A cold heading steel according to claim 3, wherein: After the LF refined steel liquid is continuously casted, the residue in the ladle containing the LF refined steel liquid is poured into a slag pot to obtain the ladle without residue; The residue content in the residue-free ladle is 0.1 ton-0.2 ton, and the silicon dioxide content in the residue is 6%-10%.

5. The method for controlling silicon content in SWRCH22A cold heading steel according to claim 1, wherein: The material used for the deoxidation alloying is at least one of aluminum ingots, calcium carbide and aluminum particles; preferably, the material used for the deoxidation alloying is: aluminum ingots 1.0-3.0 kg / t, calcium carbide 0.6-2.5 kg / t, aluminum particles 0.3-2.0 kg / t.

6. The method for controlling silicon content in SWRCH22A cold heading steel according to claim 1, wherein: The method further comprises: before the LF refining treatment, blowing argon into the outgoing molten steel until it enters the LF refining station.

7. The method for controlling silicon content in SWRCH22A cold heading steel according to claim 1, wherein: The LF refining process includes electrification, white slag refining, component tempering and calcium feeding line treatment; The time for the white slag refining treatment is 45-55 min / furnace.

8. The method for controlling silicon content in SWRCH22A cold heading steel according to claim 1, wherein: The deoxidizer used in the LF refining process is calcium carbide and / or aluminum particles; Preferably, the deoxidizer used in the LF refining treatment is: 0.6-1.0 kg / t of calcium carbide and 0.3-1.0 kg / t of aluminum particles.

9. The method for controlling silicon content in SWRCH22A cold heading steel according to claim 3, wherein: Based on the total weight of the SWRCH22A cold heading steel, Si≤0.06%, C 0.19%-0.22%, Mn 0.81%-0.85%, S≤0.010%, P≤0.020%, and Alt≥0.025% in the SWRCH22A cold heading steel.

10. The method for controlling silicon content in SWRCH22A cold heading steel according to claim 9, wherein: The size of the SWRCH22A cold heading steel is φ6-7mm.