Method for producing extreme thin and wide plate in vertical annealing furnace

By manually setting the strip offset and adjusting the tension and temperature in the annealing furnace, the problems of deflection, buckling and scratching of extremely thin and wide plates in the vertical annealing furnace are solved, improving production stability and product quality, and reducing Product downgrade due to quality defects.

CN118773431AActive Publication Date: 2024-10-15МААНЬШАНЬ АЙРОН ЭНД СТИЛ КО ЛТД
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202410813594.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-24
Publication Date
2024-10-15
Estimated Expiration
2044-06-24

AI Technical Summary

Technical Problem

The existing technology fails to effectively solve the problems of deviation, bending and scratching of extremely thin and wide plates in vertical annealing furnaces, resulting in poor production stability and reduced product quality.

Method used

By manually setting the strip offset on the HMI operation screen, adjust the tension of the heating section and cooling section of the annealing furnace, set the temperatures of the slow cooling section, flash cooling section and over-aging section, increase the tension of the flash cooling section, and adjust the stabilizing roller and The bellows are positioned to reduce strip chatter and thermal unevenness.

Benefits of technology

It significantly reduces deviations, bends and scratch defects in the furnace, improves the production stability and product quality of extremely thin and wide plates, and reduces product degradation and customer dissatisfaction caused by quality defects.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118773431A_ABST
    Figure CN118773431A_ABST
Patent Text Reader

Abstract

The invention discloses a method for producing an ultimate thin wide plate in a vertical annealing furnace, which comprises the following steps of: before wide band steel enters the furnace, manually setting the deviation of the band steel according to the actual deviation condition of the band steel; in combination with the risk that the strip steel generates heat fluttering, the tension of the first heating section and the second heating section of the easy-to-deviate area of the annealing furnace is adjusted in advance; and then the cooling rate of the wide plate in the annealing furnace is set to prevent the strip steel from cold buckling, finally the tension of the flash cooling section is increased, and meanwhile the distance between the wide plate and the stabilizing roller and the distance between the wide plate and the air bellow are adjusted to relieve scratches caused by shaking of the strip steel. According to the method, the defects of deviation, buckling, scratching and the like of the limit thin and wide plate in the furnace are greatly reduced by adjusting the tension parameters of the limit thin and wide plate process, setting the cooling rate of the limit thin and wide plate in the furnace and combining the methods of setting the offset parameters before the wide strip steel enters the furnace, setting the position parameters of the stabilizing roller and the air bellow and the like; and the stability of wide plate production in the vertical annealing furnace is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of annealing furnaces, in particular to a method for producing extreme thin and wide plates in a vertical annealing furnace. Background Art

[0002] With the rapid development of my country's automobile industry and the continuous improvement of residents' living standards, the demand for high-end automobiles has increased year by year, especially wide-gauge cold-rolled automobile plates are widely used in the production of large covering parts such as automobile side panels and roofs. Due to its thin thickness, wide product width and soft steel grade, it is very easy to have problems such as deviation in the furnace, buckling and scratching during the production process. The current technology mainly involves the method of industrial production of wide-width plates and its forming equipment, and a high-temperature precision alloy wide plate and strip and its production process. For example, Chinese patent application No. 201410652073.9 discloses a high-temperature precision alloy wide plate and strip material and its production process, which mainly involves the formula and composition of wide plate materials; another example is Chinese patent application No. 200510105788.3 discloses a method for industrial production of wide plate materials and its forming equipment, which mainly involves forming equipment for wide plate processing; Patent application No. CN104372164B discloses a production method for controlling cold buckling of thin wide soft galvanized strip steel, which mainly solves the technical problem of cold buckling of thin wide strip steel by optimizing the cooling temperature and cooling speed after annealing, and does not involve the deviation and scratching of thin wide strip steel. Based on this, the prior art does not provide a method for stable production of extreme thin wide plates in a vertical continuous annealing furnace. Summary of the invention

[0003] The purpose of the present invention is to provide a method for producing extreme thin and wide plates in a vertical annealing furnace, which is used to reduce the risks of wide plates running off track, buckling, scratching, etc. in the furnace, improve the production stability of extreme thin and wide plates, and solve the problems raised in the above-mentioned background technology.

[0004] To achieve the above object, the present invention provides the following technical solutions:

[0005] A method for producing extremely thin and wide plates in a vertical annealing furnace, comprising the following steps:

[0006] S1: Before the wide strip enters the furnace, the strip offset is manually set on the HMI operation screen, and the adjustment range is ±60mm according to the actual deviation of the strip;

[0007] S2: Adjust the tension of heating section 1 and section 2 in the annealing furnace in advance in the areas prone to deviation. Considering the risk of thermal bending of the strip, the tension of the heating section is 20-40% higher than the secondary tension, and the slow cooling section and flash cooling section are 40-60% higher than the secondary tension.

[0008] S3: Set the cooling rate of the wide plate in the annealing furnace: the slow cooling section temperature is set to 650°C, the flash cooling section temperature is set to 350°C, the first over-aging section temperature is set to 325°C, and the second over-aging section temperature is set to 300°C;

[0009] S4: Increase the tension in the flash cooling section, set it 40-60% higher than the secondary tension, and adjust the distance between the wide plate and the stabilizing roller as well as the distance between the wide plate and the bellows to reduce the scratches caused by the shaking of the strip.

[0010] Furthermore, the thickness of the extreme thin and wide plate is ≤0.7mm and the width is ≥1900mm, and the entire recrystallization annealing process is completed after preheating in the annealing furnace, heating section, slow cooling section, flash cooling section and over-aging.

[0011] Furthermore, the specific parameter adjustment method in S1 is as follows: the maximum deviation of the wide strip entering the furnace is +30mm, and the reference value of the manual adjustment correction offset is -25mm.

[0012] Furthermore, S1 is used to prevent the wide strip from running too far after entering the furnace.

[0013] Furthermore, the specific adjustment method of the parameters in S2 is: for soft steel DC04, specification 0.7*1900mm, the fixed value of the secondary tension system is 7.02KN, the tension of the heating section after adjustment is 8.554KN, which is 21% higher than the secondary tension, and the reference tension of the flash cooling section after adjustment is 9.97KN, which is 42% higher than the secondary tension.

[0014] Furthermore, in S3, the temperature of the slow cooling section, the fast cooling section and the over-aging section is adjusted to ensure uniform temperature at the edge and middle of the furnace roller to prevent cold bending of wide plates.

[0015] Compared with the prior art, the present invention has the following beneficial effects:

[0016] The method for producing extreme thin and wide plates in a vertical annealing furnace of the present invention greatly reduces defects such as deviation, warping, and scratches of the extreme thin and wide plates in the furnace by adjusting the process tension parameters of the extreme thin and wide plates and setting the cooling rate of the extreme thin and wide plates in the furnace, and combining methods such as setting bias parameters before the wide strip enters the furnace and setting parameters of the stabilizing roller and bellows positions, thereby improving the stability of the production of wide-width plates in the vertical annealing furnace, reducing losses such as product degradation caused by quality defects of the wide-width strip in the furnace, and improving product order fulfillment and customer satisfaction. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] Figure 1 The wide strip steel production flow chart of the present invention;

[0018] Figure 2 It is a schematic diagram of the structure of the flash cooling section in the production process of the present invention;

[0019] Figure 3 It is a reference diagram of the wide plate deviation correction bias value of the present invention;

[0020] Figure 4 The reference tension adjustment diagram for the wide plate of the present invention;

[0021] Figure 5 It is a schematic diagram of the wide plate scoop of the present invention. DETAILED DESCRIPTION

[0022] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0023] The thickness of the extreme thin and wide plate in the embodiment of the present invention is ≤0.7mm, the width is ≥1900mm, and the entire recrystallization annealing process is completed after preheating in the annealing furnace, heating section, slow cooling section, flash cooling section and over-aging. Figure 1 As shown; among them, the extreme thin and wide plate is an ultra-low carbon mild steel automobile plate widely used in the production of large covering parts such as automobile side panels and roofs. Due to its thin thickness, wide product and soft steel grade, it is very easy to have problems such as deviation, warping and scratching in the furnace during the production process. In order to improve the production quality stability of the extreme thin and wide plate in the vertical annealing furnace, the embodiment of the present invention provides a method for producing the extreme thin and wide plate in the vertical annealing furnace, which includes the following steps:

[0024] S1: Before the wide strip enters the furnace, the strip offset is manually set on the HMI operation screen, and the adjustment range is ±60mm according to the actual deviation of the strip; Figure 3 As shown, for example, the maximum deviation of wide strip steel entering the furnace is +30mm, and the reference value of the deviation correction is manually adjusted to -25mm, so that the wide strip steel does not deviate greatly after entering the furnace;

[0025] S2: Adjust the tension of heating section 1 and section 2 in the annealing furnace prone to deviation in advance. Considering the risk of thermal bending of the strip steel, the tension of the heating section is 20-40% higher than the secondary tension, and the slow cooling section and flash cooling section are 40-60% higher than the secondary tension. In this embodiment, IF soft steel DC04, specification 0.7*1900mm is taken as an example. The fixed value of the secondary tension system is 7.02KN. After adjustment, the reference tension of the heating section is 8.554KN, which is 21% higher than the secondary tension. The reference tension of the flash cooling section is 9.97KN, which is 42% higher than the secondary tension. Figure 4 As shown;

[0026] S3: Prevent the wide plate from buckling by reducing the cooling temperature difference in the cooling section and adjusting the cooling rate. Take IF mild steel DC04, specification 0.7*1900mm as an example, set the cooling rate of the wide plate in the annealing furnace, refer to Table 1:

[0027]

[0028] The temperature of the slow cooling section is set at 650℃, the temperature of the flash cooling section is set at 350℃, the temperature of the first over-aging section is set at 325℃, and the temperature of the second over-aging section is set at 300℃. The temperatures of the slow cooling section, the fast cooling section, and the over-aging section are adjusted by the above temperatures to make the temperature of the edge and the middle of the furnace roller gradually uniform, reducing the risk of uneven heating of the contact roller surface of the strip causing buckling along the width direction. The main reason why the temperature of the flash cooling section is higher than the over-aging temperature is that the wide plate has a slow cooling process after flash cooling and passing through the first and second aging sections, reducing the temperature difference of the strip between the furnaces, thereby achieving the purpose of preventing the strip from buckling due to cold. Figure 5 As shown;

[0029] S4: Since the wide plate is easily shaken and scratched during the cooling process, especially in the flash cooling stage of rapid cooling, the present invention needs to increase the tension of the flash cooling stage, which is set to be 40-60% higher than the secondary tension, such as Figure 4 As shown, taking IF mild steel DC04, specification 0.7*1900mm as an example, the fixed value of the secondary tension system is 7.02KN, and the reference tension of the flash cooling section after adjustment is 9.97KN, which is 42% higher than the secondary tension. At the same time, adjust the distance between the wide plate and the stable roller and the wide plate and the bellows. The reference distance between the wide plate and the stable roller is L1 (reference value 0.2-2mm), see the details Figure 2 In the flash cooling section detailed drawing, mark 1, the reference distance between the wide plate and the wind box is L2 ≥ 100mm, see Figure 2 The flash cooling section is marked with 2 in the detailed diagram, thereby alleviating the scratching caused by the shaking of the strip.

[0030] In order to further better explain the embodiments of the present invention, strip steels of different specifications are provided for testing. The specific test parameters are shown in Table 2:

[0031]

[0032]

[0033] From the above, it can be seen that the method for producing extreme thin and wide plates in a vertical annealing furnace provided by the present invention aims to solve the problems of deviation, warping and scratching in the furnace which are very likely to occur during the production of extreme thin and wide plates and ultra-low carbon soft steel. By program control and adjustment of the bias setting before the wide strip enters the furnace, combined with the adjustment and control of tension, temperature and speed parameters, the defects of deviation, warping and scratching of the extreme thin and wide plates in the furnace are greatly reduced, thereby improving the production stability of the extreme thin and wide plates.

[0034] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.

Claims

1. A method for producing extremely thin and wide plates in a vertical annealing furnace, characterized in that: The following steps are involved: S1: Before the wide strip enters the furnace, the strip offset is manually set on the HMI operation screen, and the adjustment range is ±60mm according to the actual deviation of the strip; S2: Adjust the tension of heating section 1 and section 2 in the annealing furnace in advance in the areas prone to deviation. Considering the risk of thermal bending of the strip, the tension of the heating section is 20-40% higher than the secondary tension, and the slow cooling section and flash cooling section are 40-60% higher than the secondary tension. S3: Set the cooling rate of the wide plate in the annealing furnace: the slow cooling section temperature is set to 650°C, the flash cooling section temperature is set to 350°C, the first over-aging section temperature is set to 325°C, and the second over-aging section temperature is set to 300°C; S4: Increase the tension in the flash cooling section, set it 40-60% higher than the secondary tension, and adjust the distance between the wide plate and the stabilizing roller as well as the distance between the wide plate and the bellows to reduce the scratching caused by the shaking of the strip.

2. A method for producing extremely thin and wide plates in a vertical annealing furnace according to claim 1, characterized in that: The thickness of the extreme thin and wide plate is ≤0.7mm and the width is ≥1900mm. It completes the entire recrystallization annealing process after preheating in the annealing furnace, heating section, slow cooling section, flash cooling section and over-aging.

3. A method for producing extremely thin and wide plates in a vertical annealing furnace as claimed in claim 1, characterized in that: The specific parameter adjustment method in S1 is as follows: the maximum deviation of wide strip entering the furnace is +30mm, and the reference value of the manual adjustment correction offset is -25mm.

4. A method for producing extremely thin and wide plates in a vertical annealing furnace as claimed in claim 3, characterized in that: S1 is used to prevent wide strip steel from running too far after entering the furnace.

5. The method for producing extremely thin and wide plates in a vertical annealing furnace according to claim 1, characterized in that: The specific adjustment method of parameters in S2 is: for soft steel DC04, specification 0.7*1900mm, the fixed value of the secondary tension system is 7.02KN. After adjustment, the tension of the heating section is 8.554KN, which is 21% higher than the secondary tension. After adjustment, the reference tension of the flash cooling section is 9.97KN, which is 42% higher than the secondary tension.

6. A method for producing extremely thin and wide plates in a vertical annealing furnace according to claim 1, characterized in that: In S3, the temperature of the slow cooling section, fast cooling section and over-aging section is adjusted to ensure uniform temperature at the edge and middle of the furnace roller and prevent wide-width plates from buckling due to cold.

Citation Information

Patent Citations

  • A Production Method for Controlling Cold Warpage of Thin and Wide Soft Galvanized Strip Steel

    CN104372164B

  • High-temperature precision alloy broadband strip and production process thereof

    CN104451433A

  • Method for industrial production of wide plate and its shaping equipment

    CN1743162A

  • Buckling treatment method of thin and wide specification IF steel in furnace

    CN104131152A

  • Method for preventing buckling and deviation of strip steel with thickness not larger than 0.5 mm in continuous annealing furnace

    CN111411214A