High-entropy composite ceramic material and preparation method and application thereof

Through the component ratio of high-entropy composite ceramic materials, hot isostatic pressing, and radiation heating processes, the problems of brittleness and insufficient wear resistance of ceramic artificial joint materials have been solved, and ceramic materials with high toughness and wear resistance have been prepared, improving improve the service life of artificial joints.

CN118773484APending Publication Date: 2024-10-15JIANGSU UNIV OF TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410765377.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-14
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

Existing ceramic artificial joint materials have problems such as high brittleness, low flexural strength, and poor wear resistance. Moreover, it is difficult to evenly disperse the added alumina fibers, resulting in uneven material structure and insufficient wear resistance.

Method used

Using high-entropy composite ceramic materials, by controlling the component ratio, hot isostatic pressing, and radiation heating processes, the components are fully melted and liquid nitrogen is rapidly cooled, and whiskers are synthesized by in-situ reaction to form a uniform, dense structure with high High-entropy composite ceramic materials with toughness and wear resistance.

Benefits of technology

It significantly improves the flexural strength, fracture toughness and wear resistance of ceramic materials, solves the problems of brittle fracture and uneven tissue, and extends the service life of artificial joints.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004892279680000071
    Figure BDA0004892279680000071
  • Figure BDA0004892279680000081
    Figure BDA0004892279680000081
Patent Text Reader

Abstract

The embodiment of the invention relates to a high-entropy composite ceramic material and a preparation method and application thereof, and belongs to the technical field of orthopedic materials. The high-entropy composite ceramic material disclosed by the embodiment of the invention is prepared from the following components in parts by mass: 50 to 70 parts of Al2O3, 50 to 70 parts of ZrO2, 30 to 45 parts of SiO2, 30 to 45 parts of Al, 5 to 10 parts of MgO, 5 to 10 parts of Y2O3 and 10 to 20 parts of paraffin. According to the high-entropy composite ceramic material provided by the embodiment of the invention, by controlling the proportion of all the components of the high-entropy composite ceramic material and parameters of hot isostatic pressing and radiation heating, all the components are fully melted, and after liquid nitrogen is rapidly cooled, in-situ reaction is carried out to synthesize the whisker Al2O3, so that uniform structure, high density and isotropic performance are realized; the high toughness, the strength and the wear resistance are well improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The embodiments of the present application relate to the technical field of orthopedic materials, and in particular to a high-entropy composite ceramic material and a preparation method and application thereof. Background Art

[0002] Artificial joint replacement can effectively restore joint function and improve the patient's quality of life. Artificial joints include hip, knee, shoulder, elbow, wrist, ankle and other joints, among which hip and knee joint replacement are the main ones. Artificial joints are subjected to very severe forces in the body. For example, artificial hip joints are subjected to about 3.6×10 6 The load impact and wear may be several times the body weight of the human body. At the same time, because the normal human bones constantly adjust their appearance in the complex balance between osteoblasts and osteophagocytes, the debris from the friction surface of the prosthesis accumulates near the joint, which will cause the increase of osteophagocytes in the body, break the balance between osteophagocytes and osteoblasts, and make the prosthesis loose. Therefore, if the service life of artificial joints is to be maintained for more than 20 years, the material must have excellent mechanical properties and wear resistance.

[0003] Because ceramic materials have ultra-high hardness, good biocompatibility, corrosion resistance and wear resistance, they can avoid the problem of aseptic loosening caused by wear particles of metal and polymer materials. At the same time, ceramic materials have excellent hydrophilicity and can meet the lubricity of joints. In addition, ceramics can also maintain biological inertness under physiological conditions to avoid the problem of metal ion release in the body. The ceramic artificial joint materials used in clinical practice include bio-inert ceramics, alumina ceramics (A12O3), and zirconium oxide ceramics (ZrO2); bioactive ceramics mainly include calcium-based bioceramics such as hydroxyapatite (HA), bioglass ceramics, etc., and the most widely used are A12O3 and ZrO2 ceramics. However, ceramics have the disadvantages of high hardness, high brittleness, high elastic modulus, which is 10-20 times higher than the elastic modulus of human cortical bone, and low tensile and bending strength. Brittle fracture and bone damage often occur during use. The fracture toughness of A12O3 is only about 3.5MPa·m 1 / 2 The bending strength is only about 380MPa. Impact and stress concentration will cause the A12O3 joint implant to break and produce fragments, thus causing joint damage. ZrO2 has good fracture toughness, up to 15-30MPa·m 1 / 2 , but its Vickers hardness is only 13GPa and its wear resistance is poor.

[0004] The existing Chinese patent with publication number CN110078480A discloses a ceramic composite material for artificial joints and its preparation method. The added alumina fiber has high elasticity and compression strength, which is beneficial to increase the toughness of the ceramic composite material and reduce the possibility of fragmentation of the ceramic composite material. The bending strength of the prepared ceramic material reaches 1430MPa and the fracture toughness reaches 23.8MPa·m 1 / 2 However, this patent requires that the alumina fiber be modified before being dispersed in the slurry. The process of uniformly dispersing alumina fibers in ceramic composite materials is complicated, which can easily lead to uneven structure of the ceramic composite materials. Secondly, the calcination temperature in the preparation method is relatively low at 1100-1300°C, while the melting points of alumina and zirconia are 2000°C and 2680°C, respectively. Chemical bonds cannot be completely formed between the interfaces of alumina and zirconia ceramic particles. Finally, this patent does not involve wear resistance, which is an important performance indicator of artificial joint materials. The existing Chinese patent with publication number CN108689699A discloses a high-flexibility ceramic composite material for artificial skeletal joints and a preparation method thereof, which uses 30-40% hydroxyapatite and 30-40% yttrium-stabilized zirconia toughened alumina ceramics (on the one hand, the flexural strength and fracture toughness of alumina ceramics can be improved, and on the other hand, its price is much lower than zirconia ceramics, and it has a better cost-effectiveness than zirconia ceramics) as the main material, and adds 5-10% ceramic whiskers, 5-10% nano-titanium oxide, 0-10% oyster shell powder, 0-10% magnesium oxide and 0-10% calcium oxide to prepare the high-flexibility ceramic composite material for artificial skeletal joints. Although the fracture toughness of the prepared composite material is higher than that of ordinary ceramic materials, its bending strength and compressive strength are lower than those of ordinary ceramic materials. Summary of the invention

[0005] In view of this, the embodiments of the present application provide a high-entropy composite ceramic material and a preparation method and application thereof. By controlling the ratio of the components of the high-entropy composite ceramic material and the parameters of hot isostatic pressing and radiation heating, the components are fully melted, and the whiskers Al2O3 are synthesized by in-situ reaction after rapid cooling with liquid nitrogen, thereby achieving uniform organization, high density and isotropic performance, and greatly improving high toughness, strength and wear resistance. The defects of existing ceramic composite materials for artificial joints, such as the difficulty in uniformly dispersing the added alumina fibers and the low wear resistance of the ceramic composite materials, can be effectively overcome.

[0006] A first aspect of an embodiment of the present application provides a high-entropy composite ceramic material, which includes the following components in percentage by mass: 50 to 70 parts of Al2O3, 50 to 70 parts of ZrO2, 30 to 45 parts of SiO2, 30 to 45 parts of Al, 5 to 10 parts of MgO, 5 to 10 parts of Y2O3, and 10 to 20 parts of paraffin.

[0007] In some embodiments that may include the above embodiments, the purity of the six powders of Al2O3, ZrO2, SiO2, Al, MgO and Y2O3 is 99.9%, and the average particle size of the six powders is 3-5 μm.

[0008] A second aspect of the embodiment of the present application further provides a method for preparing the above-mentioned high entropy composite ceramic material, comprising the following steps:

[0009] (1) Slurry preparation: Weigh each component in proportion, mechanically mix them by ball milling, add deionized water, and stir evenly to obtain a uniformly dispersed paste slurry;

[0010] (2) 3D printing: The 3D printer sets the printing speed and dimensional accuracy according to the artificial joint digital model, and deposits the paste slurry layer by layer through a nozzle to form an artificial joint blank;

[0011] (3) Low temperature sintering: performing low temperature sintering on the artificial joint blank by hot isostatic pressing in an inert atmosphere;

[0012] (4) Ultrafast high-temperature sintering: The artificial joint blank after low-temperature sintering is subjected to high-temperature sintering by radiation heating in an inert atmosphere, and then rapidly cooled to obtain a high-entropy composite ceramic material.

[0013] In some embodiments that may include the above embodiments, in step (1), the ball mill uses SiC grinding balls, the grinding medium is anhydrous ethanol, the ball-to-material mass ratio is 12:1, and the ball milling speed is 800 r·min -1 , the ball milling time is 6 to 10 hours.

[0014] In some embodiments that may include the above embodiments, in step (1), the mass ratio of the deionized water to the total amount of each component is 1:(1-2).

[0015] In some embodiments that may include the above embodiments, in step (1), the viscosity of the paste slurry is 0.3 to 0.8 Pa.s.

[0016] In some embodiments that may include the above embodiments, in step (2), the 3D printing speed is 3 to 5 mm / s, and the dimensional accuracy is 0.1 to 0.2 mm.

[0017] In some embodiments that may include the above embodiments, in step (3), the low temperature sintering temperature is 600-800° C., the low temperature sintering time is 10-20 min, and the low temperature sintering pressure is 150-220 MPa; or

[0018] The inert gas is high-purity argon.

[0019] In some embodiments that may include the above embodiments, in step (4), the high temperature sintering time is 5 to 10 seconds, and the high temperature sintering temperature is 2600 to 2800° C.; or

[0020] The inert gas is high-purity argon; or

[0021] The rapid cooling is performed using liquid nitrogen.

[0022] The third aspect of the embodiments of the present application also provides an application of the high entropy composite ceramic material as described above in the field of artificial joint preparation.

[0023] Compared with the prior art, the embodiments of the present application have the following beneficial effects:

[0024] (1) This application uses the characteristics of 3D printing technology that can form complex structural components to prepare ceramic artificial joints that fit human cortical bones, fundamentally solving the problem that complex ceramic artificial joint materials are difficult to machine.

[0025] (2) The present application utilizes the superposition of different mechanical properties of the ceramic components and the alloying of the components to form a dual-phase (FCC+HCP) solid solution structure, thereby improving the plastic deformation capacity of the ceramic and solving the problem of high brittleness of existing ceramic materials;

[0026] (3) The present application utilizes the high-pressure heating characteristics of the hot isostatic pressing process to form a high-density blank by high-pressure heating of the artificial joint blank, thereby reducing the porosity and internal microcracks;

[0027] (4) The present application utilizes the characteristics of fast radiation heating and rapid liquid nitrogen cooling to obtain a high-entropy composite ceramic material containing a large amount of Al2O3 whiskers through in-situ reaction, thereby overcoming the disadvantage of the prior art that the Al2O3 fibers added to the ceramic slurry are not firmly bonded to the matrix. DETAILED DESCRIPTION

[0028] In order to make the purpose, technical solutions and advantages of the embodiments of the present application clearer, the technical solutions in the embodiments of the present application are described clearly and completely below. Obviously, the described embodiments are part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present application.

[0029] Unless otherwise specified, the experimental methods used in the examples of this application are all conventional methods.

[0030] In the following examples and comparative examples, unless otherwise specified, all raw materials can be obtained by commercial purchase or conventional methods.

[0031] Example 1

[0032] The present embodiment provides a high-entropy composite ceramic material, which includes the following components in parts by mass: 50 parts of Al2O3, 50 parts of ZrO2, 30 parts of SiO2, 30 parts of Al, 5 parts of MgO, 5 parts of Y2O3, and 10 parts of paraffin; and the purity of the six powders of Al2O3, ZrO2, SiO2, Al, MgO and Y2O3 is 99.9%, and the average particle size of the six powders is 3μm.

[0033] The high entropy composite ceramic material is used to manufacture a replacement body suitable for artificial joints. The preparation method of the high entropy composite ceramic material comprises the following steps:

[0034] (1) Slurry preparation: First weigh 50 parts of Al2O3 and 50 parts of ZrO2, then weigh 30 parts of SiO2, 30 parts of Al, 5 parts of MgO, 5 parts of Y2O3, and 10 parts of paraffin wax, and use SiC grinding balls and anhydrous ethanol as grinding media (ball-to-material mass ratio 12:1) to mechanically mix them by ball milling at a speed of 800 r / min -1 , ball milling time 6h, adding deionized water, the mass ratio of deionized water to the total amount of each component is 1:1, stirring evenly to obtain a uniformly dispersed paste slurry, the viscosity of the paste slurry is 0.3Pa.s;

[0035] (2) 3D printing the prepared paste slurry: the printing speed and dimensional accuracy parameters are set to 3 mm / s and 0.1 mm respectively, and the 3D printer deposits the paste slurry layer by layer through the nozzle according to the artificial joint digital model to form an artificial joint blank;

[0036] (3) Low temperature sintering: The artificial joint blank printed above is subjected to hot isostatic pressing and low temperature sintering in an inert atmosphere. The low temperature sintering temperature is 600° C., the low temperature sintering time is 10 min, the low temperature sintering pressure is 150 MPa, and the inert gas used is high purity argon;

[0037] (4) The artificial joint blank sintered at low temperature is subjected to ultrafast high temperature sintering: the artificial joint blank is sintered at high temperature within 5 seconds by radiation heating in an inert atmosphere of high-purity argon gas, the high temperature sintering temperature is 2600°C, and then rapidly cooled by liquid nitrogen to obtain a high entropy composite ceramic material.

[0038] Example 2

[0039] The present embodiment provides a high-entropy composite ceramic material, which includes the following components in parts by mass: 60 parts of Al2O3, 60 parts of ZrO2, 40 parts of SiO2, 40 parts of Al, 7 parts of MgO, 7 parts of Y2O3, and 15 parts of paraffin; and the purity of the six powders of Al2O3, ZrO2, SiO2, Al, MgO and Y2O3 is 99.9%, and the average particle size of the six powders is 4μm.

[0040] The high entropy composite ceramic material is used to manufacture a replacement body suitable for artificial joints. The preparation method of the high entropy composite ceramic material comprises the following steps:

[0041] (1) Slurry preparation: First weigh 60 parts of Al2O3 and 60 parts of ZrO2, then weigh 40 parts of SiO2, 40 parts of Al, 7 parts of MgO, 7 parts of Y2O3, and 15 parts of paraffin wax, and use SiC grinding balls and anhydrous ethanol as grinding media (ball-to-material mass ratio 12:1) to mechanically mix them by ball milling at a speed of 800 r / min -1 , ball milling time 8h, add deionized water, the mass ratio of deionized water to the total amount of each component is 1:1.5, stir evenly to obtain a uniformly dispersed paste slurry, the viscosity of the paste slurry is 0.6Pa.s;

[0042] (2) 3D printing the prepared paste slurry: the printing speed and dimensional accuracy parameters are set to 4 mm / s and 0.15 mm respectively, and the 3D printer deposits the paste slurry layer by layer through the nozzle according to the artificial joint digital model to form an artificial joint blank;

[0043] (3) Low temperature sintering: The artificial joint blank printed above is subjected to hot isostatic pressing and low temperature sintering in an inert atmosphere. The low temperature sintering temperature is 700° C., the low temperature sintering time is 15 min, the low temperature sintering pressure is 180 MPa, and the inert gas used is high purity argon;

[0044] (4) The artificial joint blank sintered at low temperature is subjected to ultrafast high temperature sintering: the artificial joint blank is sintered at high temperature in 7 seconds by radiation heating in an inert atmosphere of high-purity argon gas, the high temperature sintering temperature is 2700°C, and then rapidly cooled by liquid nitrogen to obtain a high entropy composite ceramic material.

[0045] Example 3

[0046] The present embodiment provides a high-entropy composite ceramic material, which includes the following components in parts by mass: 70 parts of Al2O3, 70 parts of ZrO2, 45 parts of SiO2, 45 parts of Al, 10 parts of MgO, 10 parts of Y2O3, and 20 parts of paraffin; and the purity of the six powders of Al2O3, ZrO2, SiO2, Al, MgO and Y2O3 is 99.9%, and the average particle size of the six powders is 5μm.

[0047] The high entropy composite ceramic material is used to manufacture a replacement body suitable for artificial joints. The preparation method of the high entropy composite ceramic material comprises the following steps:

[0048] (1) Slurry preparation: First weigh 60 parts of Al2O3 and 60 parts of ZrO2, then weigh 40 parts of SiO2, 40 parts of Al, 7 parts of MgO, 7 parts of Y2O3, and 15 parts of paraffin wax, and use SiC grinding balls and anhydrous ethanol as grinding media (ball-to-material mass ratio 12:1) to mechanically mix them by ball milling at a speed of 800 r / min -1 , ball milling time 10h, add deionized water, the mass ratio of deionized water to the total amount of each component is 1:2, stir evenly to obtain a uniformly dispersed paste slurry, the viscosity of the paste slurry is 0.8Pa.s;

[0049] (2) 3D printing the prepared paste slurry: the printing speed and dimensional accuracy parameters are set to 5 mm / s and 0.2 mm respectively, and the 3D printer deposits the paste slurry layer by layer through the nozzle according to the artificial joint digital model to form an artificial joint blank;

[0050] (3) Low temperature sintering: The artificial joint blank printed above is subjected to hot isostatic pressing and low temperature sintering in an inert atmosphere. The low temperature sintering temperature is 800° C., the low temperature sintering time is 20 min, the low temperature sintering pressure is 220 MPa, and the inert gas used is high purity argon;

[0051] (4) The artificial joint blank sintered at low temperature is subjected to ultrafast high temperature sintering: the artificial joint blank is sintered at high temperature within 10 seconds by radiation heating in an inert atmosphere of high-purity argon gas, the high temperature sintering temperature is 2800°C, and then rapidly cooled by liquid nitrogen to obtain a high entropy composite ceramic material.

[0052] Comparative Example 1

[0053] The composite ceramic material and preparation method thereof provided in this comparative example can refer to Example 1, except that, in terms of mass percentage, it includes the following components: 49 parts of Al2O3, 49 parts of ZrO2, 29 parts of SiO2, 29 parts of Al, 4 parts of MgO, 4 parts of Y2O3, and 9 parts of paraffin.

[0054] Comparative Example 2

[0055] The composite ceramic material and preparation method thereof provided in this comparative example can refer to Example 3, except that, in terms of mass percentage, it includes the following components: 71 parts of Al2O3, 71 parts of ZrO2, 46 parts of SiO2, 46 parts of Al, 11 parts of MgO, 11 parts of Y2O3, and 21 parts of paraffin.

[0056] Comparative Example 3

[0057] This comparative example provides a composite ceramic material, which includes the following components in parts by mass: 50 parts of Al2O3, 50 parts of ZrO2, 30 parts of SiO2, 30 parts of Al, 5 parts of MgO, 5 parts of Y2O3, and 10 parts of paraffin; and the purity of the six powders of Al2O3, ZrO2, SiO2, Al, MgO and Y2O3 is 99.9%, and the average particle size of the six powders is 3μm.

[0058] The preparation method of the composite ceramic material provided in Comparative Example 3 comprises the following steps:

[0059] (1) Slurry preparation: First weigh 50 parts of Al2O3 and 50 parts of ZrO2, then weigh 30 parts of SiO2, 30 parts of Al, 5 parts of MgO, 5 parts of Y2O3, and 10 parts of paraffin wax, and use SiC grinding balls and anhydrous ethanol as grinding media (ball-to-material mass ratio 12:1) to mechanically mix them by ball milling at a speed of 750 r / min -1 , ball milling time 5h, add deionized water, the mass ratio of deionized water to the total amount of each component is 1:0.9, stir evenly to obtain a uniformly dispersed paste slurry, the viscosity of the paste slurry is 0.2Pa.s;

[0060] (2) 3D printing the prepared paste slurry: the printing speed and dimensional accuracy parameters are set to 2 mm / s and 0.09 mm respectively, and the 3D printer deposits the paste slurry layer by layer through the nozzle according to the artificial joint digital model to form an artificial joint blank;

[0061] (3) Low temperature sintering: The artificial joint blank printed above is subjected to hot isostatic pressing and low temperature sintering in an inert atmosphere. The low temperature sintering temperature is 550° C., the low temperature sintering time is 9 min, the low temperature sintering pressure is 145 MPa, and the inert gas used is high purity argon;

[0062] (4) The artificial joint blank sintered at low temperature is subjected to ultrafast high temperature sintering: the artificial joint blank is sintered at high temperature within 4 seconds by radiation heating in an inert atmosphere of high-purity argon gas, the high temperature sintering temperature is 2500°C, and then rapidly cooled by liquid nitrogen to obtain a high entropy composite ceramic material.

[0063] Comparative Example 4

[0064] This comparative example 4 provides a composite ceramic material, which includes the following components in parts by mass: 70 parts of Al2O3, 70 parts of ZrO2, 45 parts of SiO2, 45 parts of Al, 10 parts of MgO, 10 parts of Y2O3, and 20 parts of paraffin; and the purity of the six powders of Al2O3, ZrO2, SiO2, Al, MgO and Y2O3 is 99.9%, and the average particle size of the six powders is 5μm.

[0065] The preparation method of the composite ceramic material of Comparative Example 4 comprises the following steps:

[0066] (1) Slurry preparation: First weigh 60 parts of Al2O3 and 60 parts of ZrO2, then weigh 40 parts of SiO2, 40 parts of Al, 7 parts of MgO, 7 parts of Y2O3, and 15 parts of paraffin wax, and use SiC grinding balls and anhydrous ethanol as grinding media (ball-to-material mass ratio 12:1) to mechanically mix them by ball milling at a speed of 850 r / min -1 , ball milling time 11h, add deionized water, the mass ratio of deionized water to the total amount of each component is 1:3, stir evenly to obtain a uniformly dispersed paste slurry, the viscosity of the paste slurry is 0.9Pa.s;

[0067] (2) 3D printing the prepared paste slurry: the printing speed and dimensional accuracy parameters are set to 6 mm / s and 0.3 mm respectively, and the 3D printer deposits the paste slurry layer by layer through the nozzle according to the artificial joint digital model to form an artificial joint blank;

[0068] (3) Low temperature sintering: The artificial joint blank printed above is subjected to hot isostatic pressing and low temperature sintering in an inert atmosphere. The low temperature sintering temperature is 850° C., the low temperature sintering time is 21 min, the low temperature sintering pressure is 230 MPa, and the inert gas used is high purity argon;

[0069] (4) The artificial joint blank sintered at low temperature is subjected to ultrafast high temperature sintering: the high temperature sintering of the artificial joint blank is completed in 11 seconds by radiation heating in an inert atmosphere of high-purity argon, the high temperature sintering temperature is 2900°C, and then liquid nitrogen is used for rapid cooling to obtain a high entropy composite ceramic material.

[0070] Test Case

[0071] Performance test: The bending strength test adopts the GB / T4741-1999 ceramic material bending strength test method; the fracture toughness test adopts the GB / T23806-2009 ceramic material fracture toughness test method; the compression strength test adopts the GB / T8489-2006 ceramic material compression strength test method; the elastic modulus test adopts the GB / T10700-2006 ceramic elastic modulus test method; the wear rate test adopts the Chinese and foreign standard JIS T0303-2000 high-speed friction test method. The composite ceramic materials prepared in the above examples 1 to 3 and comparative examples 1 to 4 were subjected to performance tests to obtain ceramic performance parameters as shown in Table 1.

[0072] Table 1

[0073]

[0074]

[0075] It can be seen from the data in Table 1 that, compared with traditional artificial joint ceramic materials, the high entropy composite ceramic material prepared in this application contains a large amount of in-situ Al2O3 whiskers, an elastic modulus of 15-25GPa, a bending strength of 2000MPa, and a fracture toughness of 36MPa / m 2 , which has great application value in artificial joints.

[0076] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present application, rather than to limit it. Although the present application has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present application.

Claims

1. A high entropy composite ceramic material, characterized in that: The high entropy composite ceramic material comprises the following components by weight: 50-70 parts of Al2O3, 50-70 parts of ZrO2, 30-45 parts of SiO2, 30-45 parts of Al, 5-10 parts of MgO, 5-10 parts of Y2O3, and 10-20 parts of paraffin.

2. The high entropy composite ceramic material according to claim 1, characterized in that: The purity of the six powders of Al2O3, ZrO2, SiO2, Al, MgO and Y2O3 is 99.9%, and the average particle size of the six powders is 3-5 μm.

3. A method for preparing the high entropy composite ceramic material according to claim 1 or 2, characterized in that: The following steps are involved: (1) Slurry preparation: Weigh each component in proportion, mechanically mix them by ball milling, add deionized water, and stir evenly to obtain a uniformly dispersed paste slurry; (2) 3D printing: The 3D printer sets the printing speed and dimensional accuracy according to the digital model of the artificial joint, and deposits the paste slurry layer by layer through a nozzle to form an artificial joint blank; (3) Low temperature sintering: performing low temperature sintering on the artificial joint blank by hot isostatic pressing in an inert atmosphere; (4) Ultrafast high-temperature sintering: The artificial joint blank after low-temperature sintering is subjected to high-temperature sintering by radiation heating in an inert atmosphere, and then rapidly cooled to obtain a high-entropy composite ceramic material.

4. The method for preparing a high entropy composite ceramic material according to claim 3, characterized in that: In step (1), the ball mill uses SiC grinding balls, the grinding medium is anhydrous ethanol, the ball-to-material mass ratio is 12:1, and the ball mill speed is 800 r / min. -1 , the ball milling time is 6 to 10 hours.

5. The method for preparing a high entropy composite ceramic material according to claim 3, characterized in that: In step (1), the mass ratio of the deionized water to the total amount of each component is 1:(1-2).

6. The method for preparing a high entropy composite ceramic material according to claim 3, characterized in that: In step (1), the viscosity of the paste slurry is 0.3-0.8 Pa.s.

7. The method for preparing a high entropy composite ceramic material according to claim 3, characterized in that: In step (2), the 3D printing speed is 3 to 5 mm / s, and the dimensional accuracy is 0.1 to 0.2 mm.

8. The method for preparing a high entropy composite ceramic material according to claim 3, characterized in that: In step (3), the low temperature sintering temperature is 600-800° C., the low temperature sintering time is 10-20 min, and the low temperature sintering pressure is 150-220 MPa; or The inert gas is high-purity argon.

9. The method for preparing a high entropy composite ceramic material according to claim 3, characterized in that: In step (4), the high temperature sintering time is 5 to 10 seconds, and the high temperature sintering temperature is 2600 to 2800° C.; or The inert gas is high-purity argon; or The rapid cooling is performed using liquid nitrogen.

10. Use of the high entropy composite ceramic material as claimed in claim 1 or 2 in the field of artificial joint preparation.