An anti-counterfeiting label material and its preparation method
By combining an aluminum plating layer, a BOPET layer, and a rare-earth-doped modified halloysite nanotube luminescent layer into the anti-counterfeiting label material, and utilizing anti-counterfeiting label materials with specific RGB values and colorimetric parameters, the problem of easy counterfeiting of existing technologies has been solved, achieving high anti-counterfeiting security and a unique identification method, and reducing the risk of product counterfeiting.
Patent Information
- Application Number
- CN202411096456.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-12
- Publication Date
- 2026-11-10
- Estimated Expiration
- 2044-08-12
AI Technical Summary
Existing optical color-changing inks and QR code anti-counterfeiting technologies are easily counterfeited, leading to an increased risk of product counterfeiting. There is an urgent need for anti-counterfeiting label materials with high anti-counterfeiting security.
The anti-counterfeiting label material combines an aluminum-plated layer, a BOPET layer, and a rare-earth-doped modified halloysite nanotube luminescent layer. The specific RGB values and colorimetric parameters released by the rare-earth-doped modified halloysite nanotube luminescent layer serve as anti-counterfeiting information, which is then combined with the cut-edge marking area for identification.
It improves the security of anti-counterfeiting label materials, reduces the risk of product counterfeiting, ensures the legitimate rights and interests of merchants, and enhances the recognition effect through unique colorimetric inspection parameters and RGB values.
Smart Images

Figure CN118781906B_ABST
Abstract
Description
Technical Field
[0001] This application relates to the field of anti-counterfeiting label materials technology, and in particular to an anti-counterfeiting label material and its preparation method. Background Technology
[0002] With the rapid development of technology, traditional anti-counterfeiting technologies are no longer sufficient to meet the needs of social development. In order to reduce the risk of product counterfeiting and minimize the adverse impact on economic production and life, it is necessary to actively explore efficient anti-counterfeiting technologies.
[0003] Traditional counterfeiting techniques such as watermarking and embossing have been gradually replaced by modern anti-counterfeiting technologies such as optically variable inks and QR codes. With technological advancements, counterfeiting techniques have also developed rapidly. For example, anti-counterfeiting labels printed with optically variable ink rely on the ink itself as their core anti-counterfeiting technology. Since optically variable inks can be analyzed using modern analytical instruments, they are easily reverse-engineered to produce similar finished products, increasing the risk of counterfeiting.
[0004] QR code anti-counterfeiting technology generates QR codes on existing systems or platforms. Scanning the QR code leads to the system or platform's information entry interface, where product production and material information is entered. When consumers scan the QR code on the label, they can obtain corresponding product information (production and material information, etc.). Through this information, consumers can verify the product's authenticity via phone or the manufacturer's official website, thus reducing the risk of counterfeiting. However, this QR code anti-counterfeiting technology is also easily cracked. Counterfeiters can replicate the anti-counterfeiting methods of legitimate merchants, increasing the risk of product counterfeiting. Therefore, there is an urgent need for a highly secure anti-counterfeiting label material to reduce the risk of product counterfeiting and protect the legitimate rights and interests of merchants. Summary of the Invention
[0005] To address the aforementioned anti-counterfeiting and security technical issues, this application provides an anti-counterfeiting label material and its preparation method.
[0006] The anti-counterfeiting label material provided in this application is achieved through the following technical solution:
[0007] An anti-counterfeiting label material includes an aluminum-plated layer, a first BOPET layer, a second BOPET layer, a rare-earth-doped modified halloysite nanotube luminescent layer, a third BOPET layer, and a coating layer. The aluminum-plated layer is laminated to one surface of the first BOPET layer, and the other surface of the first BOPET layer is laminated and connected to the second BOPET layer. The rare-earth-doped modified halloysite nanotube luminescent layer is formed on the surface of the second BOPET layer facing away from the first BOPET layer. The coating layer is laminated to the surface of the third BOPET layer facing away from the second BOPET layer. A cutting and attaching marking area is formed at the bottom edge of the third BOPET layer. In use, the cutting and attaching marking area of the finished anti-counterfeiting label is cut off, and the cut-off label is attached to the surface of the product or product packaging material. The cutting and attaching marking area at the bottom edge of the third BOPET layer is marked with anti-counterfeiting information. The anti-counterfeiting information includes the RGB value of the color of light emitted by the rare-earth-doped modified halloysite nanotube luminescent layer through the coating layer.
[0008] The anti-counterfeiting identification method is as follows: the product producer or seller measures the RGB value of the light emitted by the rare earth-doped modified halloysite nanotube light-emitting layer through the coating layer, and marks the measured RGB value as anti-counterfeiting information on the cutting and pasting marking area of the third BOPET layer; the consumer reads the RGB value of the anti-counterfeiting label material through the cutting and pasting marking sub-label on the surface of the product or product packaging material, and detects the RGB value of the light emitted by the rare earth-doped modified halloysite nanotube light-emitting layer on the coating layer of the anti-counterfeiting label material by visual colorimetry, spectrophotometry or photoelectric integration method, and compares the detected RGB value with the read RGB value of the anti-counterfeiting label material to determine the authenticity of the product.
[0009] Preferably, the anti-counterfeiting information includes the RGB value of the light emitted by the rare earth-doped modified halloysite nanotube light-emitting layer through the coating layer and the colorimetric test parameters of the light emitted by the rare earth-doped modified halloysite nanotube light-emitting layer through the coating layer, wherein the colorimetric test parameters are L*, a*, b*.
[0010] The anti-counterfeiting identification method is as follows: the product producer or seller measures the RGB value of the light emitted by the rare earth-doped modified halloysite nanotube light-emitting layer through the coating layer and the colorimetric test parameters of the light emitted by the rare earth-doped modified halloysite nanotube light-emitting layer through the coating layer, wherein the colorimetric test parameters are L*, a*, b*, and marks the measured RGB value and colorimetric test parameters as anti-counterfeiting information on the cutting and pasting edge marking area of the third BOPET layer;
[0011] Consumers can read the RGB values and colorimetric parameters of the anti-counterfeiting label material by examining the cut-edge markings on the surface of the product or its packaging. They can then use visual colorimetry, spectrophotometry, or photoelectric integration to detect the RGB values of the light emitted by the rare-earth-doped modified halloysite nanotube luminescent layer on the anti-counterfeiting label material's coating layer. The detected RGB values are compared with the RGB values read from the anti-counterfeiting label material to determine the product's authenticity. Finally, a spectrophotometer is used to test the colorimetric parameters of the light emitted by the rare-earth-doped modified halloysite nanotube luminescent layer on the anti-counterfeiting label material's coating layer. The detected colorimetric parameters are then compared with the colorimetric parameters read from the anti-counterfeiting label material to determine the product's authenticity.
[0012] The anti-counterfeiting label material prepared in this application uses a combination of a rare earth-doped modified halloysite nanotube luminescent layer and a coating layer to form specific colorimetric inspection parameters L*, a*, b* and RGB values. By using unique colorimetric inspection parameters and RGB values as anti-counterfeiting information, the high anti-counterfeiting security of the anti-counterfeiting label material is effectively guaranteed, the risk of product counterfeiting is reduced, and the legitimate rights and interests of merchants are protected.
[0013] Preferably, the anti-counterfeiting information further includes a color mark, the RGB value of which is equal to the RGB value of the light emitted by the rare earth-doped modified halloysite nanotube light-emitting layer through the coating layer as measured.
[0014] The method for identifying anti-counterfeiting information of the anti-counterfeiting label material is as follows: The product producer or seller measures the RGB value of the light emitted by the rare earth-doped modified halloysite nanotube luminescent layer through the coating layer, determines the color of the light by the RGB value, and marks the color of the light determined by the RGB value as anti-counterfeiting information on the surface of the product packaging material; Consumers obtain the color information of the mark on the surface of the product packaging material, and compare the color of the light emitted by the rare earth-doped modified halloysite nanotube luminescent layer on the coating layer of the anti-counterfeiting label material with the color of the mark on the surface of the product packaging material by visual colorimetry to determine the authenticity of the product.
[0015] Preferably, the product producer or seller measures the RGB value of the light emitted by the rare earth-doped modified halloysite nanotube luminescent layer through the coating layer, determines the color of the light by the RGB value, prepares ink with the corresponding RGB value, and imprints the ink with the corresponding RGB value onto the cutting and attaching marking area of the third BOPET layer; the consumer obtains the color information on the cutting and attaching marking sub-label, and compares the color of the light emitted by the rare earth-doped modified halloysite nanotube luminescent layer on the coating layer of the anti-counterfeiting label material with the color on the cutting and attaching marking sub-label by visual colorimetry to determine the authenticity of the product.
[0016] By adopting the above technical solutions, the anti-counterfeiting security of anti-counterfeiting label materials can be improved, and the risk of product counterfeiting can be reduced.
[0017] Preferably, the coating layer includes a circular coating color area and several ring-shaped coating color areas. The diameter of the circular coating color area is 0.4-0.6 times the length of the rare-earth-doped modified halloysite nanotube light-emitting layer. The inner diameter of the ring-shaped coating color areas is equal to the diameter of the circular coating color area. The outer diameter of the ring-shaped coating color areas is 2-4 times the diameter of the circular coating color area. The circular coating color area is one of green, pink, blue, yellow, and purple. The ring-shaped coating color areas are one of green, pink, blue, yellow, and purple. The circular coating color areas and the ring-shaped coating color areas reflect different colors of light.
[0018] Preferably, the coating layer includes a circular coating color area and four annular coating color areas, namely, the east annular coating color area, the west annular coating color area, the south annular coating color area, and the north annular coating color area; the diameter of the circular coating color area is 0.5 times the length of the rare earth-doped modified halloysite nanotube light-emitting layer; the inner diameter of the annular coating color area is equal to the diameter of the circular coating color area; and the outer diameter of the annular coating color area is equal to three times the diameter of the circular coating color area.
[0019] The RGB values of the light emitted by the rare-earth-doped modified halloysite nanotube luminescent layer passing through the circular coated color area and the colorimetric parameters of the light emitted by the rare-earth-doped modified halloysite nanotube luminescent layer passing through the circular coated color area were measured. The colorimetric parameters were L1*, a1*, and b1*. The measured RGB values and colorimetric parameters were marked as anti-counterfeiting information on the cutting edge marking area at the bottom edge of the third BOPET layer. The colorimetric parameters in the anti-counterfeiting information marked on the cutting edge marking area were denoted as C:L1*, a1*, b1**.
[0020] The RGB values of the light emitted by the rare-earth-doped modified halloysite nanotube luminescent layer passing through the north-side ring-shaped coating color area and the colorimetric test parameters of the light emitted by the rare-earth-doped modified halloysite nanotube luminescent layer passing through the north-side ring-shaped coating color area were measured. The colorimetric test parameters were L2*, a2*, and b2*. The measured RGB values and colorimetric test parameters were marked as anti-counterfeiting information on the cutting and attaching marking area at the bottom edge of the third BOPET layer. The colorimetric test parameters in the anti-counterfeiting information marked on the cutting and attaching marking area were denoted as N:L2*, a2*, b2*.
[0021] The RGB values of the light emitted by the rare-earth-doped modified halloysite nanotube luminescent layer passing through the ring-shaped coating color region on the south side and the colorimetric test parameters of the light emitted by the rare-earth-doped modified halloysite nanotube luminescent layer passing through the ring-shaped coating color region on the south side were measured. The colorimetric test parameters are L3*, a3*, and b3*. The measured RGB values and colorimetric test parameters are marked as anti-counterfeiting information on the cutting edge marking area at the bottom edge of the third BOPET layer. The colorimetric test parameters in the anti-counterfeiting information marked on the cutting edge marking area are denoted as S:L3*, a3*, b3*.
[0022] The RGB values of the light emitted by the rare-earth-doped modified halloysite nanotube luminescent layer passing through the western ring-shaped coating color area and the colorimetric test parameters of the light emitted by the rare-earth-doped modified halloysite nanotube luminescent layer passing through the western ring-shaped coating color area were measured. The colorimetric test parameters were L4*, a4*, and b4*. The measured RGB values and colorimetric test parameters were marked as anti-counterfeiting information on the cutting and attaching marking area at the bottom edge of the third BOPET layer. The colorimetric test parameters in the anti-counterfeiting information marked on the cutting and attaching marking area were denoted as W:L4*, a4*, b4*.
[0023] The RGB values of the light emitted by the rare-earth-doped modified halloysite nanotube luminescent layer passing through the east-side ring-shaped coating color area and the colorimetric parameters of the light emitted by the rare-earth-doped modified halloysite nanotube luminescent layer passing through the east-side ring-shaped coating color area were measured. The colorimetric parameters were L5*, a5*, and b5*. The measured RGB values and colorimetric parameters were marked as anti-counterfeiting information on the cutting edge marking area at the bottom edge of the third BOPET layer. The colorimetric parameters in the anti-counterfeiting information marked on the cutting edge marking area were denoted as E:L5*, a5*, b5*.
[0024] By adopting the above technical solutions, the anti-counterfeiting security of anti-counterfeiting label materials can be improved, and the risk of product counterfeiting can be reduced.
[0025] Preferably, the product producer or seller respectively measures the RGB values of the light emitted by the rare earth-doped modified halloysite nanotube light-emitting layer in the circular coated color area, the rare earth-doped modified halloysite nanotube light-emitting layer in the eastern ring-shaped coated color area, the rare earth-doped modified halloysite nanotube light-emitting layer in the southern ring-shaped coated color area, the rare earth-doped modified halloysite nanotube light-emitting layer in the western ring-shaped coated color area, and the rare earth-doped modified halloysite nanotube light-emitting layer in the northern ring-shaped coated color area. The color of the light is determined by the RGB values and recorded as color C, color E, color S, color W, and color N, respectively. Color C, color E, color S, color W, and color N are marked as anti-counterfeiting information on the surface of the product or product packaging material.
[0026] When marking the surface of a product or its packaging material with color C, color E, color S, color W, or color N, the corresponding orientation information of each color should be marked on the surface of the product or its packaging material.
[0027] Consumers can determine the authenticity of a product by visually comparing the color of the light emitted by the rare earth-doped modified halloysite nanotube luminescent layer on the circular coated color area of the anti-counterfeiting label material with the color C of the marking on the surface of the product or its packaging material through a colorimetric method.
[0028] The authenticity of a product is determined by visually comparing the color of the light emitted by the rare earth-doped modified halloysite nanotube luminescent layer on the eastern ring-shaped coating color area of the anti-counterfeiting label material with the color E of the marking on the surface of the product or its packaging material.
[0029] The authenticity of a product is determined by visually comparing the color of the light emitted by the rare earth-doped modified halloysite nanotube luminescent layer on the ring-shaped coating color area of the anti-counterfeiting label material with the color S of the marking on the surface of the product or its packaging material.
[0030] The authenticity of a product is determined by visually comparing the color of the light emitted by the rare earth-doped modified halloysite nanotube luminescent layer on the western ring-shaped coating color area of the anti-counterfeiting label material with the color W of the marking on the surface of the product or its packaging material.
[0031] The authenticity of a product is determined by visually comparing the color of the light emitted by the rare earth-doped modified halloysite nanotube luminescent layer on the north-side ring-shaped coating color area of the anti-counterfeiting label material with the color N of the marking on the surface of the product or its packaging material.
[0032] Preferably, when the reflected light of the circular coating color area is green, the circular coating color area includes a 105nm nano-silica coating and a 153nm nano-titanium dioxide coating; when the reflected light of the circular coating color area is pink, the circular coating color area includes an 82nm nano-silica coating and a 103nm nano-titanium dioxide coating; when the reflected light of the circular coating color area is blue, the circular coating color area includes a 46nm nano-silica coating and a 48nm nano-titanium dioxide coating; when the reflected light of the circular coating color area is yellow, the circular coating color area includes a 65nm nano-silica coating and an 83nm nano-titanium dioxide coating; and when the reflected light of the circular coating color area is purple, the circular coating color area includes an 88nm nano-silica coating and a 110nm nano-titanium dioxide coating.
[0033] Preferably, the thickness of the aluminum plating layer is 0.5-5 μm, the thickness of the first BOPET layer is 10-25 μm, the thickness of the second BOPET layer is 50-80 μm, the thickness of the rare earth-doped modified halloysite nanotube luminescent layer is 0.5-20 μm, and the thickness of the third BOPET layer is 50-200 μm.
[0034] By adopting the above technical solutions, the anti-counterfeiting security of anti-counterfeiting label materials can be improved, and the risk of product counterfeiting can be reduced.
[0035] Preferably, the preparation method of the rare earth-doped modified halloysite nanotube luminescent layer / third BOPET layer includes the following steps:
[0036] S1, Preparation of rare earth-doped modified halloysite nanotube luminescent liquid:
[0037] S1.1, Preparation of rare earth-doped modified halloysite nanotubes;
[0038] Luminescent rare earth complexes are adsorbed inside and between the shells of the obtained rare earth-doped modified halloysite nanotubes.
[0039] The luminescent rare earth complex is Ln·L3, where Ln is a rare earth element, specifically La. 3+ Ce 3+ Lu 3+ Y 3+ Eu 3 + 、Tb 3+ 、Sm 3+ Dy 3+ One of them; wherein L is a ligand, specifically one of o-phenanthroline, triphenylphosphine oxide, salicylic acid, phthalic acid, phthalocyanine compounds, 4-phenylpyridine-2,6-dicarboxylic acid, and 4-hydroxypyridine-2,6-dicarboxylic acid;
[0040] S1.2, Preparation of magnetic iron oxide@rare earth doped modified halloysite nanotubes;
[0041] The resulting magnetic iron(III) oxide@rare earth doped modified halloysite nanotubes include rare earth doped modified halloysite nanotubes and magnetic iron(III) oxide grafted onto the outer wall of the rare earth doped modified halloysite nanotubes.
[0042] S1.3, 1 part of surface magnetic iron oxide@rare earth doped modified halloysite nanotubes is dispersed and mixed evenly with 49-199 parts of water-based polyurethane latex to prepare rare earth doped modified halloysite nanotube luminescent liquid.
[0043] Step 2: Coat the surface of the BOPET film with rare earth-doped modified halloysite nanotube luminescent liquid, and apply an irregular magnetic field at 65-80℃. The directional action time in the irregular magnetic field is 2-24 hours, and the direction of the magnetic field is perpendicular to the horizontal plane. This will give you the rare earth-doped modified halloysite nanotube luminescent layer / third BOPET layer.
[0044] Preferably, the preparation method of the magnetic iron(III) oxide@rare earth doped modified halloysite nanotubes in step S1.2 is as follows:
[0045] Rare earth-doped halloysite nanotubes were obtained by ultrasonic dispersion of rare earth-doped halloysite nanotubes with methacryloyloxysilane aqueous solution.
[0046] Simultaneously, vinylsilane-modified magnetic iron oxide nanoparticles were obtained by ultrasonic dispersion of magnetic iron oxide nanoparticles and vinylsilane aqueous solution.
[0047] The diameter of the magnetic iron oxide nanoparticles is larger than the diameter of the halloysite nanotubes;
[0048] The prepared methacryloxysilane-grafted rare earth-doped halloysite nanotubes were dissolved in an organic solvent and dispersed evenly to obtain dispersion A, wherein the solid content of dispersion A was 0.5-5.0 wt%.
[0049] Vinylsilane-modified magnetic iron oxide nanoparticles and accelerator BPO were dissolved in an organic solvent and dispersed uniformly to obtain dispersion B. The solid content of dispersion B was 0.01-2.0 wt%, and the mass ratio of accelerator BPO to vinylsilane-modified magnetic iron oxide nanoparticles was 1:(100-200). The mass ratio of methacryloyloxysilane-grafted modified rare earth doped halloysite nanotubes to vinylsilane-modified magnetic iron oxide nanoparticles was 10:(0.5-2).
[0050] After heating dispersion A to 45-85℃, dispersion B is added dropwise to dispersion A at 0.5-2.0 ml / 1 min under magnetic stirring at 400-800 rpm. After the addition is complete, the reaction continues until the supernatant becomes transparent. Then, centrifugation, water washing, and vacuum drying are performed to obtain magnetic iron tetroxide@rare earth doped modified halloysite nanotubes.
[0051] By adopting the above technical solutions, the anti-counterfeiting security of anti-counterfeiting label materials can be improved, and the risk of product counterfeiting can be reduced.
[0052] The method for preparing an anti-counterfeiting label material provided in this application is achieved through the following technical solution:
[0053] A method for preparing an anti-counterfeiting label material includes the following steps:
[0054] Step 1: An aluminum-plated BOPET film is formed on the first BOPET layer by vacuum deposition onto the aluminum-plated layer.
[0055] Simultaneously, a colored BOPET film is formed on the third BOPET layer by vacuum deposition;
[0056] Step 2: Preparation of rare earth-doped modified halloysite nanotube luminescent layer / third BOPET layer;
[0057] Step 3: The aluminum-plated BOPET film, the rare earth-doped modified halloysite nanotube luminescent layer / third BOPET layer, and the colored BOPET film of the third BOPET layer are bonded together by a hot-pressing composite process to form a semi-finished anti-counterfeiting label.
[0058] Step four: Heat-treat the semi-finished anti-counterfeiting label to obtain the finished anti-counterfeiting label. At least RGB value detection is performed on the light emitted by the finished anti-counterfeiting label. The measured RGB value parameters are laser-printed on the bottom edge of the third BOPET layer to form a cutting and attaching marking area. When in use, the cutting and attaching marking area of the finished anti-counterfeiting label is cut off and the cut-off marking sub-label is attached to the surface of the product packaging material.
[0059] In summary, this application has the following advantages:
[0060] 1. This application has a specific RGB value. By using the unique RGB value as anti-counterfeiting information, the high anti-counterfeiting security of the anti-counterfeiting label material can be effectively guaranteed, the risk of product counterfeiting can be reduced, and the legitimate rights and interests of merchants can be guaranteed.
[0061] 2. This application has specific colorimetric inspection parameters L*, a*, b* and RGB values. By using unique colorimetric inspection parameters and RGB values as anti-counterfeiting information, it can effectively ensure the high anti-counterfeiting security of anti-counterfeiting label materials, reduce the risk of product counterfeiting, and protect the legitimate rights and interests of merchants.
[0062] 3. This application has specific colorimetric inspection parameters L*, a*, b* and RGB values and their corresponding RGB values ink marking colors. By using unique colorimetric inspection parameters and RGB values, as well as the corresponding RGB values ink marking colors as anti-counterfeiting information, it can effectively ensure the high anti-counterfeiting security of anti-counterfeiting label materials, reduce the risk of product counterfeiting, and ensure the legitimate rights and interests of merchants.
[0063] 4. This application can classify product grades by the number of ring-shaped coating color areas, such as 1 ring-shaped coating color area for entry-level, 2 ring-shaped coating color areas for mid-range, 3 ring-shaped coating color areas for high-end, and 4-6 ring-shaped coating color areas for flagship, which facilitates consumer identification of products and enhances product recognition and brand awareness.
[0064] 5. The cutting and attaching label area designed in this application can avoid the problem of reusing the label after tearing it off, which helps to improve anti-counterfeiting security.
[0065] 6. In the rare earth-doped modified halloysite nanotube luminescent layer of this application, the rare earth-doped modified halloysite nanotubes are arranged in a near-vertical or vertical manner. That is, the light intensity observed is the greatest when the observer's line of sight is perpendicular to the surface of the anti-counterfeiting label. As the observer's line of sight switches from 90° to 30°, it will be found that the smaller the observation angle, the smaller the light intensity observed, or even the light disappears. This anti-counterfeiting identification method facilitates consumers' identification of products and enhances product recognition and brand awareness. Attached Figure Description
[0066] Figure 1 This is a schematic diagram of the overall structure of the anti-counterfeiting label material in the embodiments of this application.
[0067] Figure 2 This is a planar schematic diagram of the anti-counterfeiting label material in Embodiment 1 of this application, with one ring-shaped coated color area.
[0068] Figure 3 This is a planar schematic diagram of the anti-counterfeiting label material in Embodiment 2 of this application, with two annular coated color areas.
[0069] Figure 4 This is a planar schematic diagram of the anti-counterfeiting label material in Embodiment 3 of this application, with three annular coated color areas.
[0070] Figure 5 This is a planar schematic diagram of the anti-counterfeiting label material in Embodiment 4 of this application, with four annular coated color zones.
[0071] In the figure, 1 is the aluminum plating layer; 2 is the first BOPET layer; 3 is the second BOPET layer; 4 is the rare earth-doped modified halloysite nanotube light-emitting layer; 5 is the third BOPET layer; 6 is the coating layer; 60 is the cutting and marking area; 61 is the circular coating color area; and 62 is the ring-shaped coating color area. Detailed Implementation
[0072] To further understand the present invention, preferred embodiments of the present invention are described below in conjunction with examples and comparative examples.
[0073] Example
[0074] refer to Figure 1An anti-counterfeiting label material comprises an aluminized BOPET film, a rare-earth-doped modified halloysite nanotube luminescent layer 4 / a third BOPET layer 5, and a colored BOPET film, manufactured through a hot-pressing composite process and heat treatment. The aluminized BOPET film consists of an aluminized layer 1 and a first BOPET layer 2; the colored BOPET film consists of a third BOPET layer 5 and a coating layer 6. Specifically, the aluminized layer 1 is vacuum-deposited onto one surface of the first BOPET layer 2, and the other surface of the first BOPET layer 2 is hot-pressed to connect with the second BOPET layer 3. The rare-earth-doped modified halloysite nanotube luminescent layer 4 is formed on the surface of the second BOPET layer 3 facing away from the first BOPET layer 2. The coating layer 6 is vacuum-deposited onto the surface of the third BOPET layer 5 facing away from the second BOPET layer 3. A cutting and attaching marking area 60 is formed at the bottom edge of the third BOPET layer 5. In use, the cutting and attaching marking area 60 of the finished anti-counterfeiting label is cut off, and the cut-off label is attached to the surface of the product or its packaging material. The cutting and attaching marking area 60 at the bottom edge of the third BOPET layer 5 is marked with anti-counterfeiting information, which includes the RGB value of the color of the light emitted by the rare earth-doped modified halloysite nanotube light-emitting layer 4 through the coating layer 6.
[0075] refer to Figure 1 The thickness of the aluminum plating layer 1 is 0.5-5 μm, the thickness of the first BOPET layer 2 is 10-25 μm, the thickness of the second BOPET layer 3 is 50-80 μm, the thickness of the rare earth-doped modified halloysite nanotube luminescent layer 4 is 0.5-20 μm, and the thickness of the third BOPET layer 5 is 50-200 μm. In the actual anti-counterfeiting label test production process, the thickness of the aluminum plating layer 1 (vacuum magnetron sputtering coating) is 2 μm, the thickness of the first BOPET layer 2 (BOPET film) is 25 μm, the thickness of the second BOPET layer 3 (BOPET film) is 50 μm, the thickness of the rare earth-doped modified halloysite nanotube luminescent layer 4 is in the range of 5-8 μm, and the measured thickness is 6.34 μm; the thickness of the third BOPET layer 5 (BOPET film) is 100 μm.
[0076] refer to Figure 1 and Figure 2 The coating layer 6 includes circular coating color areas 61 and several ring-shaped coating color areas 62. The number of ring-shaped coating color areas 62 can be used to classify product grades. Product grades are classified by the number of ring-shaped coating color areas, such as 1 ring-shaped coating color area for entry-level, 2 ring-shaped coating color areas for mid-range, 3 ring-shaped coating color areas for high-end, and 4-6 ring-shaped coating color areas for flagship, which facilitates product identification by consumers and enhances product recognition and brand awareness.
[0077] refer to Figure 1 and Figure 2The diameter of the circular coated color area 61 is 0.4-0.6 times the length of the rare-earth-doped modified halloysite nanotube light-emitting layer 4. Preferably, the diameter of the circular coated color area 61 is 0.5 times the length of the rare-earth-doped modified halloysite nanotube light-emitting layer 4. The pattern information formed by the rare-earth-doped modified halloysite nanotube light-emitting layer 4 is designed according to the different product series requirements of the customer. However, a design concept needs to be introduced: the length of the rare-earth-doped modified halloysite nanotube light-emitting layer 4 directly forms a circular observation area. The center of the circular coated color area 61 and the center of the formed circular observation area are located on the same vertical line.
[0078] refer to Figure 1 and Figure 2 The inner diameter of the annular coating color area 62 is equal to the diameter of the circular coating color area 61, and the outer diameter of the annular coating color area 62 is 2-4 times the diameter of the circular coating color area 61. Preferably, the outer diameter of the annular coating color area 62 is 3 times the diameter of the circular coating color area 61. The annular coating color area 62 can then be divided into a test area and an observation area. The inner diameter of the test area is equal to the diameter of the circular coating color area 61, and its outer diameter is equal to the outer diameter of the formed circular observation area. The inner diameter of the observation area is equal to the diameter of the formed circular observation area, and the outer diameter of the observation area is 3 times the diameter of the circular coating color area 61. The test area is used for RGB value and colorimetric parameter testing. The purpose of the observation area is to allow product holders to visually compare the light intensity of the rare earth-doped modified halloysite nanotube luminescent layer 4 observed here. In qualified anti-counterfeiting label materials, the light intensity of the rare earth-doped modified halloysite nanotube luminescent layer 4 observed in the observation area is relatively weak, which can improve the high anti-counterfeiting security of the anti-counterfeiting label material and reduce the risk of product counterfeiting.
[0079] The circular coating color area 61 is one of green, pink, blue, yellow, or purple.
[0080] The ring-shaped coating color area 62 is one of green, pink, blue, yellow, or purple.
[0081] Specifically, when the reflected light of the circular coating color area 61 is green, the circular coating color area 61 includes, but is not limited to, a 105nm nano-silica coating, a 153nm nano-titanium dioxide coating, or a multi-layer coating to form a green film.
[0082] When the reflected light of the circular coating color area 61 is pink, the circular coating color area 61 includes, but is not limited to, an 82nm nano-silica coating and a 103nm nano-titanium dioxide coating. It can also be a pink coating formed by a special target material, such as the pink gold target material composition of Shenyang Dongchuang Precious Metals Materials Co., Ltd., which contains Au 85.0%, Pd 6.5%, Fe 3.0%, Cu 2.5%, Cr 2.5%, and In 0.5% by weight, and the color value range is: a* = 2.7, b* = 12.9.
[0083] When the reflected light of the circular coating color area 61 is blue, the circular coating color area 61 includes, but is not limited to, a 46nm nano-silica coating, a 48nm nano-titanium dioxide coating, or a multi-layer coating to form a blue film, such as the blue film prepared by the blue vacuum coating method of Shenzhen Xinjingyuan Technology Co., Ltd.: Cr base film / Cr-Ti transition film / TinO2 blue film / AF film.
[0084] When the reflected light of the circular coating color area 61 is yellow, the circular coating color area 61 includes, but is not limited to, a 65nm nano-silica coating and an 83nm nano-titanium dioxide coating. It can also be a yellow coating formed by a special target material, such as the lemon yellow gold target material of Shenyang Dongchuang Precious Metals Materials Co., Ltd., whose composition is: Au 95.0%, Ag 4.0%, Zn 0.5%, Cr 0.2%, In 0.2%, Y 0.1%, colorimetric values: a*=4.5, b*=36.2, and hardness value 158HV.
[0085] When the reflected light of the circular coating color area 61 is purple, the circular coating color area 61 includes, but is not limited to, an 88nm nano-silica coating and a 110nm nano-titanium dioxide coating. It can also be a purple coating formed by a special target material, such as the purple gold target material of Shenyang Dongchuang Precious Metals Materials Co., Ltd., whose composition is: 85.0wt.%Au, 10.0wt.%Al, 3.0wt.%Ag, 1.6wt.%Cu, 0.3wt.%In, 0.1wt.%Nd, with color values of: L=72.2, a*=3.1, b*=8.2, and hardness value of 238Hv.
[0086] Similarly, when the reflected light of the annular coating color area 62 is green, the circular coating color area 61 includes, but is not limited to, a 105nm nano-silica coating, a 153nm nano-titanium dioxide coating, or a multi-layer coating to form a green film.
[0087] When the reflected light of the annular coating color area 62 is pink, the circular coating color area 61 includes, but is not limited to, an 82nm nano-silica coating and a 103nm nano-titanium dioxide coating. It can also be a pink coating formed by a special target material, such as the pink gold target material composition of Shenyang Dongchuang Precious Metals Materials Co., Ltd., which contains Au 85.0%, Pd 6.5%, Fe 3.0%, Cu 2.5%, Cr 2.5%, and In 0.5% by weight, and the color value range is: a* = 2.7, b* = 12.9.
[0088] When the reflected light of the annular coating color area 62 is blue, the circular coating color area 61 includes, but is not limited to, a 46nm nano-silica coating and a 48nm nano-titanium dioxide coating. Alternatively, a multi-layer coating can be used to form the blue film, such as the blue film prepared by Shenzhen Xinjingyuan Technology Co., Ltd.'s blue vacuum coating method: Cr base film / Cr-Ti transition film / TinO2 blue film / AF film.
[0089] When the reflected light of the annular coating color area 62 is yellow, the circular coating color area 61 includes, but is not limited to, a 65nm nano-silica coating and an 83nm nano-titanium dioxide coating. It can also be a yellow coating formed by a special target material, such as the lemon yellow gold target material of Shenyang Dongchuang Precious Metals Materials Co., Ltd., whose composition is: Au 95.0%, Ag 4.0%, Zn 0.5%, Cr 0.2%, In 0.2%, Y 0.1%, colorimetric values: a*=4.5, b*=36.2, and hardness value 158HV.
[0090] When the reflected light of the annular coating color area 62 is purple, the circular coating color area 61 includes, but is not limited to, an 88nm nano-silica coating and a 110nm nano-titanium dioxide coating. It can also be a purple coating formed by a special target material, such as the purple gold target material of Shenyang Dongchuang Precious Metals Materials Co., Ltd., with the following composition: 85.0wt.% Au, 10.0wt.% Al, 3.0wt.% Ag, 1.6wt.% Cu, 0.3wt.% In, 0.1wt.% Nd, and chromaticity values: L=72.2, a*=3.1, b*=8.2, and hardness value: 238Hv.
[0091] It should be noted that the reflected light colors of the circular coating color area 61 and the annular coating color area 62 are different.
[0092] refer to Figure 1Anti-counterfeiting information collection and recording: The light emitted by the finished anti-counterfeiting label is tested for at least RGB value. The measured RGB value is laser-printed on the bottom edge of the third BOPET layer 5 to form a cutting and attaching marking area 60, that is, the cutting and attaching marking area 60 is marked with anti-counterfeiting information; Alternatively, a QR code can be laser-printed on the cutting and attaching marking area 60 formed on the bottom edge of the third BOPET layer 5. The QR code contains the RGB value information of the color of the light emitted by the finished anti-counterfeiting label.
[0093] When using the finished anti-counterfeiting label, cut off the 60mm trimming and affixing area of the label and attach the cut-off sub-label to the surface of the product packaging material. To further enhance anti-counterfeiting security, mark the RGB value information of the light color emitted by the finished anti-counterfeiting label on the surface of the product or product guarantee material.
[0094] The anti-counterfeiting information includes the RGB values of the light emitted by the rare-earth-doped modified halloysite nanotube luminescent layer 4 through the coating layer 6, and the colorimetric parameters of the light emitted by the rare-earth-doped modified halloysite nanotube luminescent layer 4 through the coating layer 6. The colorimetric parameters are L*, a*, and b*. The anti-counterfeiting information is collected and recorded as follows: At least the RGB values and colorimetric parameters of the light emitted by the finished anti-counterfeiting label are detected. The measured RGB values and colorimetric parameters are laser-printed on the bottom edge of the third BOPET layer 5 to form a cutting and attaching marking area 60, where the anti-counterfeiting information is marked. Alternatively, a QR code can be laser-printed on the cutting and attaching marking area 60 at the bottom edge of the third BOPET layer 5. The QR code contains the RGB values and colorimetric parameters of the light emitted by the finished anti-counterfeiting label. To further enhance anti-counterfeiting security, the RGB values and colorimetric parameters of the light emitted by the finished anti-counterfeiting label are marked on the surface of the product or product guarantee material.
[0095] The anti-counterfeiting identification method of the finished product anti-counterfeiting label is as follows: The product producer or seller measures the RGB value of the light emitted by the rare earth-doped modified halloysite nanotube light-emitting layer 4 through the coating layer 6 and the colorimetric test parameters of the light emitted by the rare earth-doped modified halloysite nanotube light-emitting layer 4 through the coating layer 6. The colorimetric test parameters are L*, a*, b*. The measured RGB value and colorimetric test parameters are marked as anti-counterfeiting information on the cutting and attaching marking area 60 of the third BOPET layer 5.
[0096] When the anti-counterfeiting information is the RGB value of the light emitted by the rare earth-doped modified halloysite nanotube light-emitting layer 4 through the coating layer 6, consumers can read the RGB value of the anti-counterfeiting label material through the cut-edge label on the surface of the product or product packaging material. The RGB value of the light emitted by the rare earth-doped modified halloysite nanotube light-emitting layer 4 on the coating layer 6 of the anti-counterfeiting label material is detected by visual colorimetry, spectrophotometry, or photoelectric integration. The detected RGB value is compared with the RGB value read from the anti-counterfeiting label material to determine the authenticity of the product.
[0097] When the anti-counterfeiting information is the RGB value and colorimetric test parameters of the light emitted by the rare earth-doped modified halloysite nanotube luminescent layer 4 through the coating layer 6, consumers can read the RGB value and colorimetric test parameters of the anti-counterfeiting label material through the cut-edge label on the surface of the product or its packaging material. They can then use visual colorimetry, spectrophotometry, or photoelectric integration to detect the RGB value of the light emitted by the rare earth-doped modified halloysite nanotube luminescent layer 4 on the coating layer 6 of the anti-counterfeiting label material, and compare the obtained RGB value with the RGB value read from the anti-counterfeiting label material to determine the authenticity of the product. Finally, they can use a spectrophotometer to test the colorimetric test parameters of the light emitted by the rare earth-doped modified halloysite nanotube luminescent layer 4 on the coating layer 6 of the anti-counterfeiting label material, and compare the obtained colorimetric test parameters with the colorimetric test parameters read from the anti-counterfeiting label material to determine the authenticity of the product.
[0098] In addition, preferred anti-counterfeiting encryption methods also include the following: the anti-counterfeiting information also includes color markings, where the RGB value of the color markings is equal to the measured RGB value of the light emitted by the rare-earth-doped modified halloysite nanotube luminescent layer 4 through the coating layer 6. The anti-counterfeiting identification method for the finished product's anti-counterfeiting label is as follows:
[0099] Product producers or sellers measure the RGB values of the light emitted by the rare-earth-doped modified halloysite nanotube light-emitting layer 4 through the coating layer 6, determine the color parameters of the light through the RGB values, configure inks with corresponding RGB values, and mark the specific color as anti-counterfeiting information on the surface of the product or product packaging material through ink printing.
[0100] Consumers can determine the authenticity of a product by visually comparing the color of the light emitted by the rare earth-doped modified halloysite nanotube luminescent layer 4 on the coating layer 6 of the anti-counterfeiting label material with the color RGB value information of the product or packaging material surface.
[0101] A method for preparing an anti-counterfeiting label material includes the following steps:
[0102] Step 1: An aluminum-plated BOPET film is formed on the first BOPET layer 2 by vacuum deposition on the aluminum-plated layer 1.
[0103] Simultaneously, a colored BOPET film is formed on the third BOPET layer 5 by vacuum deposition to form a coating layer 6.
[0104] Step 2, Preparation of rare earth-doped modified halloysite nanotube luminescent layer 4 / third BOPET layer 5:
[0105] S2.1, Preparation of rare earth-doped modified halloysite nanotube luminescent liquid:
[0106] S2.1.1, Preparation of rare earth-doped modified halloysite nanotubes;
[0107] Luminescent rare earth complexes are adsorbed inside and between the shells of the obtained rare earth-doped modified halloysite nanotubes.
[0108] The luminescent rare earth complex is Ln·L3, where Ln is a rare earth element, specifically La. 3+ Ce 3+ Lu 3+ Y 3+ Eu 3 + 、Tb 3+ 、Sm 3+ Dy 3+ One of them; wherein L is a ligand, specifically one of o-phenanthroline, triphenylphosphine oxide, salicylic acid, phthalic acid, phthalocyanine compounds, 4-phenylpyridine-2,6-dicarboxylic acid, and 4-hydroxypyridine-2,6-dicarboxylic acid;
[0109] S2.1.2, Preparation of magnetic iron oxide@rare earth doped modified halloysite nanotubes;
[0110] The resulting magnetic iron(III) oxide@rare earth doped modified halloysite nanotubes include rare earth doped modified halloysite nanotubes and magnetic iron(III) oxide grafted onto the outer wall of the rare earth doped modified halloysite nanotubes.
[0111] Specifically, rare earth-doped halloysite nanotubes are first ultrasonically dispersed with an aqueous solution of methacryloyloxysilane to obtain methacryloyloxysilane-grafted and modified rare earth-doped halloysite nanotubes; simultaneously, magnetic iron oxide nanoparticles are ultrasonically dispersed with an aqueous solution of vinyl silane to obtain vinyl silane-modified magnetic iron oxide nanoparticles; it should be noted that the diameter of the magnetic iron oxide nanoparticles is larger than the diameter of the halloysite nanotubes; then, the prepared methacryloyloxysilane-grafted and modified rare earth-doped halloysite nanotubes are dissolved in an organic solvent and dispersed evenly to obtain dispersion A, the solid content of dispersion A being 0.5-5.0 wt%; then, vinyl silane-modified magnetic iron oxide nanoparticles and the accelerator BPO are dissolved in an organic solvent... Dispersion B is uniformly dispersed in an organic solvent to obtain dispersion B, with a solid content of 0.01-2.0 wt%. The mass ratio of the promoter BPO to the vinylsilane-modified magnetic iron oxide nanoparticles is 1:9-50; and the mass ratio of the methacryloyloxysilane-grafted modified rare earth doped halloysite nanotubes to the vinylsilane-modified magnetic iron oxide nanoparticles is 10:0.5-2. Finally, after dispersing A is heated to 45-85℃, dispersing B is added dropwise to dispersing A at 0.5-2.0 ml / 1 min under magnetic stirring at 400-800 rpm. After the addition is completed, the reaction continues until the supernatant becomes transparent. Then, centrifugation, water washing, and vacuum drying are performed to obtain magnetic iron oxide@rare earth doped halloysite nanotubes.
[0112] S2.1.3, 1 part of surface magnetic iron oxide@rare earth doped modified halloysite nanotubes is dispersed and mixed evenly with 49-199 parts of water-based polyurethane latex to prepare rare earth doped modified halloysite nanotube luminescent liquid.
[0113] S2.2, the rare earth-doped modified halloysite nanotube luminescent liquid is coated on the surface of the BOPET film, and an irregular magnetic field is applied in an environment of 65-80℃. The directional action time in the irregular magnetic field is 2-24h, and the direction of the magnetic field is relatively perpendicular to the horizontal plane, so as to obtain the rare earth-doped modified halloysite nanotube luminescent layer 4 / third BOPET layer 5.
[0114] Step 3: The aluminum-plated BOPET film, the rare earth-doped modified halloysite nanotube luminescent layer 4 / third BOPET layer 5, and the colored BOPET film of the third BOPET layer 5 are bonded together by a hot-pressing composite process to form a semi-finished anti-counterfeiting label.
[0115] Step four: Heat-treat the semi-finished anti-counterfeiting label to obtain the finished anti-counterfeiting label. At least RGB value detection is performed on the light emitted by the finished anti-counterfeiting label. The measured RGB value parameters are laser-printed on the bottom edge of the third BOPET layer 5 to form a cutting and attaching marking area 60. When in use, the cutting and attaching marking area of the finished anti-counterfeiting label is cut off and the cut-off marking sub-label is attached to the surface of the product packaging material.
[0116] Example 1: Reference Figure 1 An anti-counterfeiting label material includes an aluminum-plated layer 1, a first BOPET layer 2, a second BOPET layer 3, a rare earth-doped modified halloysite nanotube luminescent layer 4, a third BOPET layer 5, and a coating layer 6, wherein the pattern formed by the rare earth-doped modified halloysite nanotube luminescent layer 4 is a circle with a diameter R.
[0117] refer to Figure 1 A cutting and marking area 60 is formed at the bottom edge of the third BOPET layer 5. The thickness of the aluminum plating layer 1 (vacuum magnetron sputtering coating) is 2μm, the thickness of the first BOPET layer 2 (BOPET film) is 25μm, the thickness of the second BOPET layer 3 (BOPET film) is 50μm; the thickness of the rare earth-doped modified halloysite nanotube luminescent layer 4 is 6.34μm; and the thickness of the third BOPET layer 5 (BOPET film) is 100μm.
[0118] refer to Figure 1 and Figure 2 The coating layer 6 includes a circular coating color area 61 and a ring-shaped coating color area 62, where the ring-shaped coating color area 62 is an annular shape. The diameter of the circular coating color area 61 is 0.5 times the diameter of the circular pattern formed by the rare-earth-doped modified halloysite nanotube light-emitting layer 4, and the center of the circular coating color area 61 is on the same vertical line as the center of the circular pattern formed by the rare-earth-doped modified halloysite nanotube light-emitting layer 4. The inner diameter of the ring-shaped coating color area 62 is equal to the diameter of the circular coating color area 61, and the outer diameter of the ring-shaped coating color area 62 is equal to 3 times the diameter of the circular coating color area 61.
[0119] The circular coating color area 61 is a 65nm nano-silica yellow coating formed by vacuum magnetron sputtering.
[0120] The ring-shaped coating color area 62 is a 153nm nano-titanium dioxide green coating formed by vacuum magnetron sputtering.
[0121] To improve the corrosion resistance of the third BOPET layer 5, a 200nm AF transparent film can be optionally deposited on the outside of the coating layer 6.
[0122] refer to Figure 1 and Figure 2The annular coating color area 62 can be divided into a test area and an observation area. The inner diameter of the test area is equal to the diameter of the circular coating color area 61, and its outer diameter is equal to the outer diameter of the formed circular observation area. The inner diameter of the observation area is equal to the diameter of the formed circular observation area, and the outer diameter of the observation area is three times the diameter of the circular coating color area 61.
[0123] In the testing area, RGB values and colorimetric parameters are measured, and the corresponding RGB values of the color ink used for cutting the edge marking area 60 are tested. The purpose of the observation area: Product holders can use visual colorimetry to determine the intensity of the light emitted by the rare-earth-doped modified halloysite nanotube luminescent layer 4 observed here. In qualified anti-counterfeiting label materials, the intensity of the light emitted by the rare-earth-doped modified halloysite nanotube luminescent layer 4 observed from a vertical viewing angle within the observation area is significantly weaker, thereby improving the high anti-counterfeiting security of the anti-counterfeiting label material and reducing the risk of product counterfeiting.
[0124] Therefore, the rare earth-doped modified halloysite nanotubes in the rare earth-doped modified halloysite nanotube luminescent layer are arranged in a near-vertical or vertical manner. That is, when the observer's line of sight is perpendicular to the surface of the anti-counterfeiting label, the light intensity observed vertically is the greatest in the circular coated color area 61 and some annular coated color areas 62 (the diameter of which is less than or equal to the diameter of the circular pattern formed by the rare earth-doped modified halloysite nanotube luminescent layer 4). In some annular coated color areas 62 (the diameter of which is greater than the diameter of the circular pattern formed by the rare earth-doped modified halloysite nanotube luminescent layer 4) and the uncoated area of the third BOPET layer 5, as the observer's line of sight switches from 90° to 30°, it will be found that the smaller the line of sight, the smaller the observed light intensity, and even the light disappears. This anti-counterfeiting identification method facilitates consumer identification of products and enhances product recognition and brand awareness.
[0125] refer to Figure 1 and Figure 2 The cutting and attaching marking area 60 at the bottom edge of the third BOPET layer 5 is marked with anti-counterfeiting information. This information includes the RGB value N of the light emitted by the rare-earth-doped modified halloysite nanotube luminescent layer 4 through the circular coated color area 61, along with colorimetric test parameters (L1*, a1*, b1*) and the RGB value W of the light emitted by the rare-earth-doped modified halloysite nanotube luminescent layer 4 through the annular coated color area 62, along with colorimetric test parameters (L2*, a2*, b2*). The anti-counterfeiting information parameters are laser-printed onto the bottom edge of the third BOPET layer 5 to form the cutting and attaching marking area 60. Corresponding colored inks are prepared based on the measured RGB value N and RGB value W of the emitted light color, and two different inks are printed onto the cutting and attaching marking area 60 of the third BOPET layer 5.
[0126] A method for preparing an anti-counterfeiting label material includes the following steps:
[0127] Step 1: A 2μm thick aluminum layer is formed on the surface of a 25μm thick BOPET film by vacuum deposition, thus obtaining an aluminum-plated BOPET film (aluminum layer 1 / first BOPET layer 2).
[0128] Meanwhile, the yellow coating with a diameter of 5 mm and a thickness of 65 nm nano-silica coating formed by vacuum deposition on the 50 μm thick BOPET film is the circular coating color area 61, and the green coating with an inner diameter of 5 mm, an outer diameter of 15 mm and a thickness of 153 nm nano-titanium dioxide coating formed by vacuum deposition is the ring-shaped coating color area 62, thus obtaining the colored BOPET film.
[0129] Step 2, Preparation of rare earth-doped modified halloysite nanotube luminescent layer 4 / third BOPET layer 5:
[0130] S2.1, Preparation of rare earth-doped modified halloysite nanotube luminescent liquid:
[0131] S2.1.1, Preparation of rare earth-doped modified halloysite nanotubes;
[0132] Luminescent rare earth complexes are adsorbed inside and between the shells of the obtained rare earth-doped modified halloysite nanotubes.
[0133] The luminescent rare earth complex is Ln·L3, where Ln is the rare earth element La. 3+ L represents 4-phenylpyridine-2,6-dicarboxylic acid;
[0134] The specific preparation method is as follows: 5g of halloysite nanotubes are dissolved in 100mL of N,N-dimethylformamide solvent to obtain mixture A; 0.8g of luminescent rare earth complex (Ln·L3, where Ln is the rare earth element La) is added. 3+ L is 4-phenylpyridine-2,6-dicarboxylic acid) dissolved in 100 mL of N,N-dimethylformamide solvent to obtain mixture B; at room temperature, mixture B is added dropwise to dispersion A at 1 mL / 1 min under magnetic stirring at 500 rpm. After the addition is completed, the reaction continues for 24 h until the supernatant becomes transparent. Then, centrifugation, water washing, and vacuum drying are performed for 4 h to obtain 5.56 g of self-luminescent rare earth-doped modified halloysite nanotubes.
[0135] S2.1.2, Preparation of magnetic iron oxide@rare earth doped modified halloysite nanotubes;
[0136] The resulting magnetic iron(III) oxide@rare earth doped modified halloysite nanotubes include rare earth doped modified halloysite nanotubes and magnetic iron(III) oxide grafted onto the outer wall of the rare earth doped modified halloysite nanotubes.
[0137] Specifically, 5.56g of rare earth-doped modified halloysite nanotubes were first mixed with 250mL of KH570 aqueous solution (KH570 mass percentage is 5wt.%) and then subjected to ultrasonic dispersion treatment for 0.5h. The ultrasonic dispersion frequency was 44kHz and the ultrasonic frequency was 800W. After filtration, water washing and vacuum drying, 5.34g of KH570 grafted modified rare earth-doped modified halloysite nanotubes were obtained.
[0138] Meanwhile, 1g of magnetic iron oxide nanoparticles with a particle size of 20-30nm were mixed with 100mL of KH151 aqueous solution (KH151 mass percentage of 5wt.%) and then subjected to ultrasonic dispersion treatment for 0.5h at an ultrasonic dispersion frequency of 44kHz and an ultrasonic frequency of 800W. After filtration, water washing and vacuum drying, 0.92g of KH151 modified magnetic iron oxide nanoparticles were obtained.
[0139] It should be noted that the diameter of halloysite nanotubes is 10-15nm, while the diameter of magnetic iron oxide nanoparticles is larger than that of halloysite nanotubes, that is, the particle size of magnetic iron oxide nanoparticles is 20-30nm. Magnetic iron oxide nanoparticles with a particle size of 20-30nm can be customized by Jiangsu Xianfeng Nanomaterials Technology Co., Ltd.
[0140] Then, 5.34 g of the prepared KH570 grafted and modified rare earth doped halloysite nanotubes were dissolved in 500 mL of organic solvent DMF and dispersed evenly to obtain dispersion A;
[0141] Then, 0.92 g of KH151 modified magnetic iron oxide nanoparticles and 0.08 g of accelerator BPO were dissolved in 100 mL of organic solvent DMF and dispersed evenly to obtain dispersion B;
[0142] Finally, after the dispersion A is heated to 60℃, the dispersion B is added dropwise to the dispersion A at 2mL / 1min under magnetic stirring at 400rpm. After the addition is completed, the reaction continues for 24h until the supernatant becomes transparent. Then, centrifugation, water washing, and vacuum drying are performed for 4h to obtain 6.45g of magnetic iron tetroxide@rare earth doped modified halloysite nanotubes.
[0143] S2.1.3, Preparation of aqueous polyurethane latex: 8.4g of aqueous polyurethane solution with a solid content of 35%, 0.1g of xanthan gum, and 91.5g of deionized water are mixed evenly to obtain aqueous polyurethane latex; 1g of the above-prepared magnetic iron tetroxide@rare earth doped modified halloysite nanotubes are dispersed and mixed evenly with 99g of the above-prepared aqueous polyurethane latex to prepare rare earth doped modified halloysite nanotube luminescent liquid.
[0144] S2.2, a PP material locating ring is fixed on a 100μm thick BOPET film. The inner diameter of the locating ring is 10mm. The rare earth-doped modified halloysite nanotube luminescent liquid prepared in S2.1.3 is dropped into the locating ring. Then, it is placed in a 65℃ environment and an irregular magnetic field is applied (the magnetic field range is a circle with a diameter of 12mm, and the center of the circular magnetic field is on the same vertical line as the center of the locating ring). The parameters for forming the irregular magnetic field are: voltage of 110V, current of 14A, magnetic field strength of 300mT, directional action time in the irregular magnetic field of 12h, and magnetic field direction is perpendicular to the horizontal plane. Thus, a rare earth-doped modified halloysite nanotube luminescent layer 4 with a thickness of 6.34μm is formed on the 100μm thick BOPET film, which is the rare earth-doped modified halloysite nanotube luminescent layer 4 / third BOPET layer 5.
[0145] Step 3: The aluminum-plated BOPET film, the rare earth-doped modified halloysite nanotube luminescent layer 4 / third BOPET layer 5, and the colored BOPET film of the third BOPET layer 5 are bonded together by hot pressing at 135℃ to obtain a semi-finished anti-counterfeiting label.
[0146] Step four: Heat-treat the semi-finished anti-counterfeiting label at 75℃ for 0.5 hours to obtain the finished anti-counterfeiting label.
[0147] The colorimetric parameters L1*, a1*, and b1* of the finished anti-counterfeiting labels were tested using a DS60 colorimeter.
[0148] The RGB values of the emitted light color of the finished anti-counterfeiting label were tested using a CZ-V20 series RGB digital fiber optic sensor.
[0149] The RGB values N and colorimetric parameters (L1*, a1*, b1*) of the light emitted by the rare-earth-doped modified halloysite nanotube luminescent layer 4 through the circular coated color area 61 and the RGB values W and colorimetric parameters (L2*, a2*, b2*) of the light emitted by the rare-earth-doped modified halloysite nanotube luminescent layer 4 through the annular coated color area 62 were measured. The anti-counterfeiting information parameters were laser-printed onto the bottom edge of the third BOPET layer 5 to form a cutting and attaching marking area 60. Corresponding colored inks were prepared based on the measured RGB values N and W of the emitted light color, and the two inks were printed onto the cutting and attaching marking area 60 of the third BOPET layer 5.
[0150] The difference between Example 2 and Example 1 is as follows: (Refer to...) Figure 1 and Figure 3The coating layer 6 includes one circular coating color area 61 and two annular coating color areas 62, each annularly shaped. The diameter of the circular coating color area 61 is 0.5 times the diameter of the circular pattern formed by the rare-earth-doped modified halloysite nanotube light-emitting layer 4, and the center of the circular coating color area 61 is on the same vertical line as the center of the circular pattern formed by the rare-earth-doped modified halloysite nanotube light-emitting layer 4. The inner diameter of the annular coating color area 62 is equal to the diameter of the circular coating color area 61, and the outer diameter of the annular coating color area 62 is equal to three times the diameter of the circular coating color area 61.
[0151] The circular coating color area 61 is a 65nm nano-silica yellow coating formed by vacuum magnetron sputtering.
[0152] One annular coating color area 62 is a 153nm nano-titanium dioxide coating, i.e., a green coating, formed by vacuum magnetron sputtering; the other annular coating color area 62 is a 103nm nano-titanium dioxide coating, i.e., a pink coating, formed by vacuum magnetron sputtering. To improve the corrosion resistance of the third BOPET layer 5, a 200nm AF transparent film can be optionally deposited on the outside of the coating layer 6.
[0153] The RGB values and colorimetric parameters (L1*, a1*, b1*) of the light emitted by the rare earth-doped modified halloysite nanotube luminescent layer 4 through the circular coated color area 61 were measured. The RGB values and colorimetric parameters (L2*, a2*, b2*) of the light emitted by the rare earth-doped modified halloysite nanotube luminescent layer 4 through one of the annular coated color areas 62 and the other annular coated color area 62 were also measured. The anti-counterfeiting information parameters are laser-printed onto the bottom edge of the third BOPET layer 5 to form a cutting and attaching marking area 60. Based on the RGB values of the emitted light color measured by the circular coating color area 61, the RGB values of the emitted light color measured by the one ring-shaped coating color area 62, and the RGB values of the emitted light color measured by the other ring-shaped coating color area 62, corresponding colored inks are prepared, and the three inks are printed onto the cutting and attaching marking area 60 of the third BOPET layer 5 respectively.
[0154] The difference between Example 3 and Example 1 is as follows: (Refer to...) Figure 1 and Figure 4The coating layer 6 includes one circular coating color area 61 and three annular coating color areas 62, each annular coating color area 62 being one-third of a circle. The diameter of the circular coating color area 61 is 0.5 times the diameter of the circular pattern formed by the rare-earth-doped modified halloysite nanotube light-emitting layer 4, and the center of the circular coating color area 61 is on the same vertical line as the center of the circular pattern formed by the rare-earth-doped modified halloysite nanotube light-emitting layer 4. The inner diameter of the annular coating color area 62 is equal to the diameter of the circular coating color area 61, and the outer diameter of the annular coating color area 62 is equal to three times the diameter of the circular coating color area 61.
[0155] The circular coating color area 61 is a 65nm nano-silica yellow coating formed by vacuum magnetron sputtering.
[0156] One annular coating color area 62 is a 153nm nano-titanium dioxide coating, i.e., a green coating, formed by vacuum magnetron sputtering; another annular coating color area 62 is a 103nm nano-titanium dioxide coating, i.e., a pink coating, formed by vacuum magnetron sputtering; and yet another annular coating color area 62 is a 110nm nano-titanium dioxide coating, i.e., a purple coating, formed by vacuum magnetron sputtering. To improve the corrosion resistance of the third BOPET layer 5, a 200nm AF transparent film can be optionally deposited on the outside of the coating layer 6.
[0157] The RGB values and colorimetric parameters (L1*, a1*, b1*) of the light emitted by the rare earth-doped modified halloysite nanotube luminescent layer 4 through the circular coated color area 61 were measured. The RGB values and colorimetric parameters (L2*, a2*, b2*) of the light emitted by the rare earth-doped modified halloysite nanotube luminescent layer 4 through one of the annular coated color areas 62, the other annular coated color areas 62, and the third annular coated color areas 62 were also measured. The anti-counterfeiting information parameters are laser-printed onto the bottom edge of the third BOPET layer 5 to form a cutting and attaching marking area 60. Based on the RGB values of the emitted light color measured by the circular coating color area 61, the RGB values of the emitted light color measured by the one ring-shaped coating color area 62, the RGB values of the emitted light color measured by the other ring-shaped coating color area 62, and the RGB values of the emitted light color measured by the other ring-shaped coating color area 62, corresponding colored inks are prepared, and the four inks are printed onto the cutting and attaching marking area 60 of the third BOPET layer 5.
[0158] The difference between Example 4 and Example 1 is as follows: (Refer to...) Figure 1 and Figure 5 The coating layer 6 includes one circular coating color area 61 and four annular coating color areas 62, each annularly shaped like a quarter circle. The diameter of the circular coating color area 61 is 0.5 times the diameter of the circular pattern formed by the rare-earth-doped modified halloysite nanotube light-emitting layer 4, and the center of the circular coating color area 61 is on the same vertical line as the center of the circular pattern formed by the rare-earth-doped modified halloysite nanotube light-emitting layer 4. The inner diameter of the annular coating color area 62 is equal to the diameter of the circular coating color area 61, and the outer diameter of the annular coating color area 62 is equal to three times the diameter of the circular coating color area 61.
[0159] The circular coating color area 61 is a 65nm nano-silica yellow coating formed by vacuum magnetron sputtering.
[0160] Among them, one annular coating color area 62 is a 153nm nano-titanium dioxide coating, i.e., a green coating, formed by vacuum magnetron sputtering; another annular coating color area 62 is a 103nm nano-titanium dioxide coating, i.e., a pink coating, formed by vacuum magnetron sputtering; another annular coating color area 62 is a 110nm nano-titanium dioxide coating, i.e., a purple coating, formed by vacuum magnetron sputtering; and another annular coating color area 62 is an 83nm nano-titanium dioxide coating, i.e., a yellow coating, formed by vacuum magnetron sputtering. To improve the corrosion resistance of the third BOPET layer 5, a 200nm AF transparent film can be optionally deposited on the outside of the coating layer 6.
[0161] The RGB values of the light emitted by the rare earth-doped modified halloysite nanotube light-emitting layer 4 through the circular coated color area 61 and the colorimetric test parameters of the light emitted by the rare earth-doped modified halloysite nanotube light-emitting layer 4 through the circular coated color area 61 are measured. The colorimetric test parameters are L1*, a1*, and b1*. The measured RGB values and colorimetric test parameters are marked as anti-counterfeiting information on the cutting and pasting edge marking area 60 at the bottom edge of the third BOPET layer 5. The colorimetric test parameters in the anti-counterfeiting information marked on the cutting and pasting edge marking area 60 are recorded as C:L1*, a1*, b1*.
[0162] The RGB values of the light emitted by the rare earth-doped modified halloysite nanotube luminescent layer 4 passing through the north-side ring-shaped coating color area and the colorimetric test parameters of the light emitted by the rare earth-doped modified halloysite nanotube luminescent layer 4 passing through the north-side ring-shaped coating color area are measured. The colorimetric test parameters are L2*, a2*, b2*. The measured RGB values and colorimetric test parameters are marked as anti-counterfeiting information on the cutting and pasting edge marking area 60 at the bottom edge of the third BOPET layer 5. The colorimetric test parameters in the anti-counterfeiting information marked on the cutting and pasting edge marking area 60 are recorded as N:L2*, a2*, b2*.
[0163] The RGB values of the light emitted by the rare earth-doped modified halloysite nanotube luminescent layer 4 passing through the south-side ring-shaped coating color area and the colorimetric test parameters of the light emitted by the rare earth-doped modified halloysite nanotube luminescent layer 4 passing through the south-side ring-shaped coating color area are measured. The colorimetric test parameters are L3*, a3*, and b3*. The measured RGB values and colorimetric test parameters are marked as anti-counterfeiting information on the cutting and pasting edge marking area 60 at the bottom edge of the third BOPET layer 5. The colorimetric test parameters in the anti-counterfeiting information marked on the cutting and pasting edge marking area 60 are recorded as S:L3*, a3*, b3*.
[0164] The RGB values of the light emitted by the rare earth-doped modified halloysite nanotube luminescent layer 4 passing through the western ring-shaped coating color area and the colorimetric test parameters of the light emitted by the rare earth-doped modified halloysite nanotube luminescent layer 4 passing through the western ring-shaped coating color area are measured. The colorimetric test parameters are L4*, a4*, b4*. The measured RGB values and colorimetric test parameters are marked as anti-counterfeiting information on the cutting and pasting edge marking area 60 at the bottom edge of the third BOPET layer 5. The colorimetric test parameters in the anti-counterfeiting information marked on the cutting and pasting edge marking area 60 are recorded as W:L4*, a4*, b4*.
[0165] The RGB values of the light emitted by the rare earth-doped modified halloysite nanotube luminescent layer 4 passing through the east-side ring-shaped coating color area and the colorimetric test parameters of the light emitted by the rare earth-doped modified halloysite nanotube luminescent layer 4 passing through the east-side ring-shaped coating color area are measured. The colorimetric test parameters are L5*, a5*, b5*. The measured RGB values and colorimetric test parameters are marked as anti-counterfeiting information on the cutting and pasting edge marking area 60 at the bottom edge of the third BOPET layer 5. The colorimetric test parameters in the anti-counterfeiting information marked on the cutting and pasting edge marking area 60 are recorded as E:L5*, a5*, b5*.
[0166] In addition, the RGB values of the light emitted by the rare earth-doped modified halloysite nanotube luminescent layer 4 through the circular coated color region 61, the rare earth-doped modified halloysite nanotube luminescent layer 4 in the eastern ring-shaped coated color region, the rare earth-doped modified halloysite nanotube luminescent layer 4 in the southern ring-shaped coated color region, the rare earth-doped modified halloysite nanotube luminescent layer 4 in the western ring-shaped coated color region, and the rare earth-doped modified halloysite nanotube luminescent layer 4 in the northern ring-shaped coated color region were measured respectively. The RGB values of the light emitted by layer 4 are used to determine the color of the light emitted by the anti-counterfeiting label, which are denoted as color C, color E, color S, color W, and color N respectively. Inks corresponding to colors C, E, S, W, and N are prepared respectively. Colors C, E, S, W, and N are printed as anti-counterfeiting information marks on the cutting and pasting marking area 60 at the bottom edge of the third BOPET layer 5 by printing with the corresponding colored inks. They can also be used as anti-counterfeiting information marks on the surface of the product or product packaging material.
[0167] It should be noted that when marking the cutting and attaching area 60 at the bottom edge of the third BOPET layer 5 or marking the product or product packaging material with color C, color E, color S, color W, or color N, the corresponding orientation information should be marked on the cutting and attaching area 60 at the bottom edge of the third BOPET layer 5 or on the product or product packaging material.
[0168] Consumers can determine the authenticity of a product by visually comparing the color of the light emitted by the rare earth-doped modified halloysite nanotube luminescent layer 4 on the circular coated color area 61 of the anti-counterfeiting label material with the color C of the mark on the bottom edge of the third BOPET layer 5, the cut edge marking area 60, or the mark on the surface of the product or its packaging material.
[0169] The authenticity of a product is determined by visually comparing the color of the light emitted by the rare earth-doped modified halloysite nanotube luminescent layer 4 on the eastern ring-shaped coating color area of the anti-counterfeiting label material with the color E of the marking on the surface of the product or its packaging material.
[0170] The authenticity of a product is determined by visually comparing the color of the light emitted by the rare earth-doped modified halloysite nanotube luminescent layer 4 on the south side ring-shaped coated color area of the anti-counterfeiting label material with the color S of the cut and pasted marking area 60 at the bottom edge of the third BOPET layer 5 or the marking on the surface of the product or its packaging material.
[0171] The authenticity of a product is determined by visually comparing the color of the light emitted by the rare earth-doped modified halloysite nanotube luminescent layer 4 on the western ring-shaped coated color area of the anti-counterfeiting label material with the color W of the cut and pasted marking area 60 at the bottom edge of the third BOPET layer 5 or the marking on the surface of the product or its packaging material.
[0172] The authenticity of a product is determined by visually comparing the color of the light emitted by the rare earth-doped modified halloysite nanotube luminescent layer 4 on the north-side ring-shaped coated color area of the anti-counterfeiting label material with the color N of the cut and pasted marking area 60 at the bottom edge of the third BOPET layer 5 or the marking on the surface of the product or its packaging material.
[0173] The difference between Comparative Example 1 and Example 1 is as follows: In step two, in the preparation of the rare earth-doped modified halloysite nanotube luminescent layer 4 / third BOPET layer 5, in S2.2, a PP material limiting ring is fixed in a BOPET film with a thickness of 100 μm. The inner diameter of the limiting ring is 10 mm. The rare earth-doped modified halloysite nanotube luminescent liquid prepared in S2.1.3 is dropped into the limiting ring. Then, it is placed in a 65°C environment for curing for 12 h to obtain the rare earth-doped modified halloysite nanotube luminescent layer 4, thus obtaining the rare earth-doped modified halloysite nanotube luminescent layer 4 / third BOPET layer 5.
[0174] In Comparative Example 1, the difference in light intensity observed by consumers in the test and observation areas for the finished anti-counterfeiting label is not significant. Furthermore, as the observer's viewing angle shifts from 90° to 30°, it is observed that the smaller the viewing angle, the lower the observed light intensity. However, the difference in light intensity observed at 90° and 30° is significantly smaller than the difference in light intensity observed at 90° and 30° in Example 1. This indicates that the rare-earth-doped modified halloysite nanotubes in the rare-earth-doped modified halloysite nanotube luminescent layer are arranged nearly vertically or vertically, effectively ensuring high anti-counterfeiting security of the anti-counterfeiting label material and reducing the risk of product counterfeiting.
[0175] In summary, this application has specific colorimetric inspection parameters and RGB values. By using unique colorimetric inspection parameters and RGB values as anti-counterfeiting information, the high anti-counterfeiting security of the anti-counterfeiting label material can be effectively guaranteed, and the risk of product counterfeiting can be reduced.
[0176] This specific embodiment is merely an explanation of this application and is not intended to limit it. After reading this specification, those skilled in the art can make modifications to this embodiment without contributing any inventive step, but such modifications are protected by patent law as long as they fall within the scope of the claims of this application.
Claims
1. An anti-counterfeiting label material, characterized in that: The product comprises an aluminum-plated layer (1), a first BOPET layer (2), a second BOPET layer (3), a rare-earth-doped modified halloysite nanotube luminescent layer (4), a third BOPET layer (5), and a coating layer (6). The aluminum-plated layer (1) is laminated to one surface of the first BOPET layer (2), and the other surface of the first BOPET layer (2) is laminated to the second BOPET layer (3). The rare-earth-doped modified halloysite nanotube luminescent layer (4) is formed on the surface of the second BOPET layer (3) facing away from the first BOPET layer (2). The coating layer (6) is laminated to the surface of the third BOPET layer (5) facing away from the second BOPET layer (3). A cutting and attaching marking area (60) is formed at the bottom edge of the third BOPET layer (5). When in use, the cutting and attaching marking area (60) of the finished anti-counterfeiting label is cut off, and the cut-off cutting and attaching marking sub-label is attached to the surface of the product or product packaging material. The third BOPET layer (5) The bottom edge of the cut-and-attach marking area (60) is marked with anti-counterfeiting information; the anti-counterfeiting information includes the RGB value of the light color emitted by the rare earth-doped modified halloysite nanotube luminescent layer (4) through the coating layer (6); the coating layer (6) includes a circular coating color area (61) and several ring-shaped coating color areas (62), the diameter of the circular coating color area (61) is 0.4-0.6 times the length of the rare earth-doped modified halloysite nanotube luminescent layer (4); the ring-shaped coating color areas The inner diameter of (62) is equal to the diameter of the circular coating color area (61); the outer diameter of the annular coating color area (62) is 2-4 times the diameter of the circular coating color area (61); the circular coating color area (61) is one of green, pink, blue, yellow, and purple; the annular coating color area (62) is one of green, pink, blue, yellow, and purple; the circular coating color area (61) and the annular coating color area (62) reflect different colors of light; The length of the rare earth-doped modified halloysite nanotube luminescent layer (4) is directly formed into a circular observation area; the center of the circular coating color area (61) and the center of the formed circular observation area are located on the same vertical line; the rare earth-doped modified halloysite nanotubes in the rare earth-doped modified halloysite nanotube luminescent layer (4) are arranged in a near-vertical or vertical manner, that is, the light intensity observed is the greatest when the observer's line of sight is perpendicular to the surface of the anti-counterfeiting label. As the observer's line of sight switches from 90° to 30°, it will be found that the smaller the line of sight, the smaller the light intensity observed. The colorimetric parameters of the light emitted by the rare earth-doped modified halloysite nanotube luminescent layer (4) on the coating layer (6) of the anti-counterfeiting label material are tested by a spectrophotometer. The obtained colorimetric parameters are compared with the colorimetric parameters of the anti-counterfeiting label material to determine the authenticity of the product. When the anti-counterfeiting information is the RGB value of the light emitted by the rare earth-doped modified halloysite nanotube light-emitting layer (4) through the coating layer (6), the consumer reads the RGB value of the anti-counterfeiting label material through the cut edge label on the surface of the product or product packaging material, and performs RGB value detection on the light emitted by the rare earth-doped modified halloysite nanotube light-emitting layer (4) on the coating layer (6) of the anti-counterfeiting label material by visual colorimetry, spectrophotometry or photoelectric integration method, and compares the detected RGB value with the read RGB value of the anti-counterfeiting label material to determine the authenticity of the product; The anti-counterfeiting information also includes the colorimetric test parameters of the light emitted by the rare earth-doped modified halloysite nanotube light-emitting layer (4) of the coating layer (6), wherein the colorimetric test parameters are L*, a*, b*; When the anti-counterfeiting information is the RGB value and colorimetric test parameters of the light emitted by the rare earth-doped modified halloysite nanotube luminescent layer (4) through the coating layer (6), consumers can read the RGB value and colorimetric test parameters of the anti-counterfeiting label material through the cut-edge label on the surface of the product or product packaging material. They can also use visual colorimetry, spectrophotometry, or photoelectric integration to detect the RGB value of the light emitted by the rare earth-doped modified halloysite nanotube luminescent layer (4) on the coating layer (6) of the anti-counterfeiting label material. The obtained RGB value is compared with the RGB value of the anti-counterfeiting label material to determine the authenticity of the product. Furthermore, the colorimetric test parameters of the light emitted by the rare earth-doped modified halloysite nanotube luminescent layer (4) on the coating layer (6) of the anti-counterfeiting label material are tested using a spectrophotometer. The obtained colorimetric test parameters are compared with the colorimetric test parameters of the anti-counterfeiting label material to determine the authenticity of the product. The anti-counterfeiting information also includes color markings, the RGB values of which are equal to the RGB values of the light emitted by the rare earth-doped modified halloysite nanotube light-emitting layer (4) through the coating layer (6). The anti-counterfeiting information identification method of the anti-counterfeiting label material is as follows: the product producer or seller measures the RGB value of the light emitted by the rare earth-doped modified halloysite nanotube light-emitting layer (4) through the coating layer (6), determines the color parameters of the light by the RGB value, configures the ink with the corresponding RGB value, and marks the specific color as anti-counterfeiting information on the surface of the product or product packaging material by ink printing; the consumer obtains the color RGB value information marked on the surface of the product or product packaging material, and compares the color of the light emitted by the rare earth-doped modified halloysite nanotube light-emitting layer (4) on the coating layer (6) of the anti-counterfeiting label material with the color RGB value information on the surface of the product or product packaging material by visual colorimetry to judge the authenticity of the product.
2. The anti-counterfeiting label material according to claim 1, characterized in that: The thickness of the aluminum plating layer (1) is 0.5-5 μm, the thickness of the first BOPET layer (2) is 10-25 μm, the thickness of the second BOPET layer (3) is 50-80 μm, the thickness of the rare earth doped modified halloysite nanotube luminescent layer (4) is 0.5-20 μm, and the thickness of the third BOPET layer (5) is 50-200 μm.
3. The anti-counterfeiting label material according to claim 1, characterized in that: The coating layer (6) includes a circular coating color area (61) and four annular coating color areas (62), the four annular coating color areas (62) being the east annular coating color area, the west annular coating color area, the south annular coating color area, and the north annular coating color area, respectively; the diameter of the circular coating color area (61) is 0.5 times the length of the rare earth doped modified halloysite nanotube light-emitting layer (4); the inner diameter of the annular coating color area (62) is equal to the diameter of the circular coating color area (61); the outer diameter of the annular coating color area (62) is equal to 3 times the diameter of the circular coating color area (61); The RGB values of the light emitted by the rare earth-doped modified halloysite nanotube light-emitting layer (4) through the circular coated color area (61) and the colorimetric test parameters of the light emitted by the rare earth-doped modified halloysite nanotube light-emitting layer (4) through the circular coated color area (61) are measured. The colorimetric test parameters are L1*, a1*, b1*. The measured RGB values and colorimetric test parameters are marked as anti-counterfeiting information in the cutting and pasting edge marking area (60) at the bottom edge of the third BOPET layer (5). The colorimetric test parameters in the anti-counterfeiting information marked in the cutting and pasting edge marking area (60) are recorded as C:L1*, a1*, b1*. The RGB values of the light emitted by the rare earth-doped modified halloysite nanotube luminescent layer (4) through the north-side ring-shaped coating color area and the colorimetric test parameters of the light emitted by the rare earth-doped modified halloysite nanotube luminescent layer (4) through the north-side ring-shaped coating color area are measured. The colorimetric test parameters are L2*, a2*, b2*. The measured RGB values and colorimetric test parameters are marked as anti-counterfeiting information in the cutting and pasting edge marking area (60) at the bottom edge of the third BOPET layer (5). The colorimetric test parameters in the anti-counterfeiting information marked in the cutting and pasting edge marking area (60) are recorded as N: L2*, a2*, b2*. The RGB values of the light emitted by the rare earth-doped modified halloysite nanotube luminescent layer (4) through the south-side ring-shaped coating color area and the colorimetric test parameters of the light emitted by the rare earth-doped modified halloysite nanotube luminescent layer (4) through the south-side ring-shaped coating color area were measured. The colorimetric test parameters were L3*, a3*, b3*. The measured RGB values and colorimetric test parameters were marked as anti-counterfeiting information in the cutting and pasting edge marking area (60) at the bottom edge of the third BOPET layer (5). The colorimetric test parameters in the anti-counterfeiting information marked in the cutting and pasting edge marking area (60) were recorded as S:L3*, a3*, b3*. The RGB values of the light emitted by the rare earth-doped modified halloysite nanotube luminescent layer (4) through the western ring-shaped coating color area and the colorimetric test parameters of the light emitted by the rare earth-doped modified halloysite nanotube luminescent layer (4) through the western ring-shaped coating color area are measured. The colorimetric test parameters are L4*, a4*, b4*. The measured RGB values and colorimetric test parameters are marked as anti-counterfeiting information in the cutting and pasting edge marking area (60) at the bottom edge of the third BOPET layer (5). The colorimetric test parameters in the anti-counterfeiting information marked in the cutting and pasting edge marking area (60) are recorded as W:L4*, a4*, b4*. The RGB values of the light emitted by the rare earth-doped modified halloysite nanotube light-emitting layer (4) through the east-side ring-shaped coating color area and the colorimetric test parameters of the light emitted by the rare earth-doped modified halloysite nanotube light-emitting layer (4) through the east-side ring-shaped coating color area are measured. The colorimetric test parameters are L5*, a5*, b5*. The measured RGB values and colorimetric test parameters are marked as anti-counterfeiting information in the cutting and pasting edge marking area (60) at the bottom edge of the third BOPET layer (5). The colorimetric test parameters in the anti-counterfeiting information marked in the cutting and pasting edge marking area (60) are recorded as E:L5*, a5*, b5*.
4. The anti-counterfeiting label material according to claim 2, characterized in that: The producers or sellers of the goods shall respectively measure the RGB values of the light emitted by the rare earth-doped modified halloysite nanotube light-emitting layer (4) in the circular coated color area (61), the rare earth-doped modified halloysite nanotube light-emitting layer (4) in the east ring-shaped coated color area, the rare earth-doped modified halloysite nanotube light-emitting layer (4) in the south ring-shaped coated color area, the rare earth-doped modified halloysite nanotube light-emitting layer (4) in the west ring-shaped coated color area, and the rare earth-doped modified halloysite nanotube light-emitting layer (4) in the north ring-shaped coated color area. The color of the light shall be determined by the RGB values and recorded as color C, color E, color S, color W, and color N respectively. Color C, color E, color S, color W, and color N shall be marked as anti-counterfeiting information on the surface of the goods or the packaging materials. When marking the surface of a product or its packaging material with color C, color E, color S, color W, or color N, the corresponding orientation information of each color should be marked on the surface of the product or its packaging material. Consumers can obtain color information from the markings on the surface of goods or packaging materials, and compare the color of the light emitted by the rare earth-doped modified halloysite nanotube luminescent layer (4) on the circular coated color area (61) of the anti-counterfeiting label material with the color C of the markings on the surface of goods or packaging materials by visual colorimetry to determine the authenticity of the goods. The color of the light emitted by the rare earth-doped modified halloysite nanotube luminescent layer (4) on the east side ring-shaped coating color area of the anti-counterfeiting label material is compared with the color E of the mark on the surface of the product or product packaging material by visual colorimetry to determine the authenticity of the product. The color of the light emitted by the rare earth-doped modified halloysite nanotube luminescent layer (4) on the south side ring-shaped coating color area of the anti-counterfeiting label material is compared with the color S of the mark on the surface of the product or product packaging material by visual colorimetry to determine the authenticity of the product. The color of the light emitted by the rare earth-doped modified halloysite nanotube luminescent layer (4) on the western ring-shaped coating color area of the anti-counterfeiting label material is compared with the color W of the mark on the surface of the product or product packaging material by visual colorimetry to determine the authenticity of the product. The color of the light emitted by the rare earth-doped modified halloysite nanotube luminescent layer (4) on the north side ring-shaped coating color area of the anti-counterfeiting label material is compared with the color N of the mark on the surface of the product or product packaging material by visual colorimetry to determine the authenticity of the product.
5. The anti-counterfeiting label material according to claim 3, characterized in that: When the reflected light of the circular coating color area (61) is green, the circular coating color area (61) includes a 105nm nano-silica coating and a 153nm nano-titanium dioxide coating; when the reflected light of the circular coating color area (61) is pink, the circular coating color area (61) includes an 82nm nano-silica coating and a 103nm nano-titanium dioxide coating; when the reflected light of the circular coating color area (61) is blue, the circular coating color area (61)... The circular coating area (61) includes a 46nm nano-silica coating and a 48nm nano-titanium dioxide coating. When the reflected light of the circular coating area (61) is yellow, the circular coating area (61) includes a 65nm nano-silica coating and an 83nm nano-titanium dioxide coating. When the reflected light of the circular coating area (61) is purple, the circular coating area (61) includes an 88nm nano-silica coating and a 110nm nano-titanium dioxide coating.
6. The anti-counterfeiting label material according to claim 1 or 5, characterized in that: The preparation method of the rare earth-doped modified halloysite nanotube luminescent layer (4) / third BOPET layer (5) includes the following steps: S1, Preparation of rare earth-doped modified halloysite nanotube luminescent liquid: S1.1, Preparation of rare earth-doped modified halloysite nanotubes; Luminescent rare earth complexes are adsorbed inside and between the shells of the obtained rare earth-doped modified halloysite nanotubes. The luminescent rare earth complex is Ln•L3, where Ln is a rare earth element, specifically La. 3+ Ce 3+ Lu 3+ Y 3+ Eu 3+ 、Tb 3+ 、Sm 3+ Dy 3+ One of them; wherein L is a ligand, specifically one of o-phenanthroline, triphenylphosphine oxide, salicylic acid, phthalic acid, phthalocyanine compounds, 4-phenylpyridine-2,6-dicarboxylic acid, and 4-hydroxypyridine-2,6-dicarboxylic acid; S1.2, Preparation of magnetic iron oxide@rare earth doped modified halloysite nanotubes; The resulting magnetic iron(III) oxide@rare earth doped modified halloysite nanotubes include rare earth doped modified halloysite nanotubes and magnetic iron(III) oxide grafted onto the outer wall of the rare earth doped modified halloysite nanotubes. S1.3, 1 part of surface magnetic iron oxide@rare earth doped modified halloysite nanotubes is dispersed and mixed evenly with 49-199 parts of water-based polyurethane latex to prepare rare earth doped modified halloysite nanotube luminescent liquid. Step 2: Coat the rare earth-doped modified halloysite nanotube luminescent liquid onto the surface of the BOPET film, place it in an environment of 65-80℃ and apply an irregular magnetic field. The directional action time in the irregular magnetic field is 2-24h, and the direction of the magnetic field is relatively perpendicular to the horizontal plane. The rare earth-doped modified halloysite nanotube luminescent layer (4) / third BOPET layer (5) can be obtained.
7. The anti-counterfeiting label material according to claim 6, characterized in that: The preparation method of S1.2, magnetic iron oxide@rare earth doped modified halloysite nanotubes is as follows: Rare earth-doped halloysite nanotubes were obtained by ultrasonic dispersion of rare earth-doped halloysite nanotubes with methacryloyloxysilane aqueous solution. Simultaneously, vinylsilane-modified magnetic iron oxide nanoparticles were obtained by ultrasonic dispersion of magnetic iron oxide nanoparticles and vinylsilane aqueous solution. The diameter of the magnetic iron oxide nanoparticles is larger than the diameter of the halloysite nanotubes; The prepared methacryloxysilane-grafted rare earth-doped halloysite nanotubes were dissolved in an organic solvent and dispersed uniformly to obtain dispersion A, wherein the solid content of dispersion A was 0.5-5.0 wt%. Vinylsilane-modified magnetic iron oxide nanoparticles and accelerator BPO were dissolved in an organic solvent and dispersed uniformly to obtain dispersion B. The solid content of dispersion B was 0.01-2.0 wt%, and the mass ratio of accelerator BPO to vinylsilane-modified magnetic iron oxide nanoparticles was 1:(100-200). The mass ratio of methacryloyloxysilane-grafted rare earth-doped halloysite nanotubes to vinylsilane-modified magnetic iron oxide nanoparticles was 10:(0.5-2). After heating dispersion A to 45-85℃, dispersion B is added dropwise to dispersion A at 0.5-2.0 ml / 1 min under magnetic stirring at 400-800 rpm. After the addition is complete, the reaction continues until the supernatant becomes transparent. Then, centrifugation, water washing, and vacuum drying are performed to obtain magnetic iron tetroxide@rare earth doped modified halloysite nanotubes.
8. A method for preparing an anti-counterfeiting label material according to any one of claims 1-7, characterized in that: Includes the following steps: Step 1: An aluminum-plated BOPET film is formed on the first BOPET layer (2) by vacuum deposition on the aluminum-plated layer (1); Meanwhile, a coating layer (6) is formed on the third BOPET layer (5) by vacuum deposition to obtain a colored BOPET film; Step 2, preparation of rare earth-doped modified halloysite nanotube luminescent layer (4) / third BOPET layer (5); Step 3: The aluminum-plated BOPET film, the rare earth-doped modified halloysite nanotube luminescent layer (4) / the third BOPET layer (5), and the third BOPET layer (5) are bonded together by a hot-pressing composite process to form a semi-finished anti-counterfeiting label. Step 4: Heat treatment of the semi-finished anti-counterfeiting label to obtain the finished anti-counterfeiting label. At least RGB value detection is performed on the light emitted by the finished anti-counterfeiting label. The measured RGB value parameters are laser printed on the bottom edge of the third BOPET layer (5) to form a cutting and attaching mark area. When using, the cutting and attaching mark area of the finished anti-counterfeiting label is cut off and the cut-off cutting and attaching mark sub-label is attached to the surface of the product packaging material.
Citation Information
Patent Citations
Rare-earth luminous fibre anti-counterfeit mark
CN101140716A
Volume hologram transfer foil, volume hologram laminate, and production method thereof
CN101329546A