Radioactive graphite volume reduction treatment method capable of easily recovering radionuclides

By using molybdate oxide to enrich radionuclides during the graphite combustion process and recycling them through acid-base treatment, the problems of aerosol diffusion and equipment corrosion in radioactive graphite processing are solved, and safe and efficient radionuclide recovery and graphite are achieved. Volume reduction.

CN118782284APending Publication Date: 2024-10-15MATERIAL INST OF CHINA ACADEMY OF ENG PHYSICS
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202410914568.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-09
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

When dealing with radioactive graphite, it is difficult to effectively control the distribution and recovery of radioactive aerosols with existing technology, leading to safety risks and equipment corrosion problems, which limits engineering applications.

Method used

Molybdate oxide is used as an additive and mixed with graphite to enrich radionuclides through the combustion process, and recover radionuclides through subsequent acid and alkali treatment, avoiding aerosol diffusion and equipment corrosion.

Benefits of technology

It effectively eliminates the problem of radioactive aerosols, simplifies the recovery process of radionuclides, reduces the risk of corrosion of equipment materials, and improves the safety of graphite volume reduction processing and the recycling efficiency of strategic metals.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118782284A_ABST
    Figure CN118782284A_ABST
Patent Text Reader

Abstract

The invention discloses a radioactive graphite volume reduction treatment method capable of easily recovering radionuclides, which realizes graphite gasification volume reduction and radionuclide recovery through additive and graphite mixing, powder granulation, combustion after granulation and nuclide separation. According to the method, molybdic acid oxide is used as an additive, the molybdic acid oxide and graphite are mixed and combusted together, and the molybdic acid oxide can enrich radionuclides in the graphite combustion process by utilizing the bonding effect of molybdic acid radicals of the molybdic acid oxide and the radionuclides, so that the problem of radioactive aerosol is eliminated, and the radionuclides can be easily separated from the graphite subsequently.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of graphite volume reduction treatment, in particular to a radioactive graphite volume reduction treatment method which is easy to recover radioactive nuclides. Background Art

[0002] The application of nuclear technology has produced a large amount of radioactive contaminated graphite, such as graphite mainly contaminated by radioactive metal elements. Since graphite waste is large in volume and not compressible, direct geological disposal of it is obviously unreasonable and impractical. Therefore, a large number of technical explorations have been carried out internationally for the volume reduction treatment of radioactive graphite, mainly including fixed bed incineration, fluidized bed incineration, steam reforming, etc., but they have not been able to achieve engineering application due to many problems that cannot be solved at this stage.

[0003] For example, the aforementioned graphite, which is mainly contaminated by radioactive metal elements, has a certain amount of metal nuclides attached to it. In the high-temperature and high-speed airflow coexistence environment of graphite burning or similar (such as steam reforming), the aerosols generated by these metals will diffuse with the airflow and deposit in certain parts between the incineration chamber and the exhaust gas outlet, with a discrete distribution. The control and protection of dangerous nuclides are extremely difficult. If the distribution of radioactive nuclides can be controlled during the graphite gasification process so that they are enriched in a specific area, it will be of great significance to eliminate the radioactive aerosol problem in the graphite volume reduction process, improve the safety of the graphite volume reduction process, and for the recycling of strategic metals.

[0004] The molten salt oxidation technology invented by Russia (RU2390862 C2) uses molten alkali metal carbonate to embed graphite blocks and set up two-stage series molten salt pools. The oxidation temperature of the first molten salt pool is controlled between 750-900℃, where graphite is converted into gas, and then the gas is introduced into the second molten salt pool by bubbling. The radioactive nuclides attached to the graphite are eluted by the molten salt in the molten salt pool, which greatly reduces the pressure of tail gas treatment and reduces the frequency of filter replacement. However, molten alkali metal salts are extremely permeable and corrosive. Germany used similar technology to treat radioactive metal contaminated waste in the 1970s and 1980s, and built a pre-test device with a processing capacity of 1-2kg / h. However, the corrosion problem of equipment materials that followed the further increase in the amount of molten alkali became one of the main factors limiting the engineering of this technology. Summary of the invention

[0005] The technical purpose of the present invention is to provide a radioactive graphite volume reduction treatment method which is easy to recover radioactive nuclides.

[0006] In order to achieve the above technical objectives, the technical solution provided by the present invention is:

[0007] A method for reducing the volume of radioactive graphite for easy recovery of radioactive nuclides comprises the following steps:

[0008] Step 1: crushing radioactive graphite to obtain granular radioactive graphite, adding an initial batch of additives enriched with radionuclides, and grinding to obtain a mixture;

[0009] Step 2: Granulate the mixture obtained in step 1 to obtain granulated graphite;

[0010] Step 3: burning granulated graphite to obtain incineration ash;

[0011] Step 4: Recover the radionuclides.

[0012] Furthermore, the initial batch of additives for enriching radionuclides includes oxides containing molybdate.

[0013] Furthermore, the cations in the molybdate oxide include Ca 2+ , Fe 2+ , Fe 3+ 、Co 2+ 、Ni 2+ 、Zn 2+ , Mn 2+ , Ba 2+ 、Bi 3+ 、Cd 2+ , Sr 2+ , Pb 2+ Mg 2+ 、Ag + At least one of .

[0014] Furthermore, the mass of the radioactive nuclides in the radioactive graphite is 0.01-1%.

[0015] Furthermore, in step 1, the grinding ratio of the granular radioactive graphite and the additive for enriching radionuclides is 1:0.25-4 in parts by weight.

[0016] Furthermore, in step 2, a granulation binder needs to be added, and the mass percentage of the granulation binder is 2-25%; the granulation binder includes any one of water and an organic binder.

[0017] Furthermore, in step 2, the particle size of the granulated graphite is 2-10 mm.

[0018] Furthermore, in step 3, the incineration ash is used as an additive for subsequent batches, and the specific steps of burning granulated graphite include:

[0019] Step 3.1: Add granulated graphite into the combustion furnace and control the temperature of the constant temperature section to 500-800℃;

[0020] Step 3.2: Introduce the reaction gas preheated to 500-800° C. into the combustion furnace and keep it warm for 5-10 hours. The reaction gas is either an oxygen-containing inert gas or air; the oxygen content is 21-100 vol%.

[0021] Furthermore, in step 4, the specific steps of recovering the radioactive nuclides include:

[0022] Step 4.1: Soak the incineration ash from step 3 in liquid acid for a period of time, and filter to obtain a first filtrate; the liquid acid is any one of hydrochloric acid, sulfuric acid, and nitric acid;

[0023] Step 4.2: continuously adding soluble carbonate to the first filtrate obtained in step 4.1 until no more precipitation occurs, and filtering to obtain a second filtrate;

[0024] Step 4.3: Add alkali to the second filtrate obtained in step 4.2, let stand and filter to obtain a solid oxide precipitate containing radioactive nuclides.

[0025] Furthermore, in step 4.3, the base is any one of ammonia water, sodium hydroxide and potassium hydroxide.

[0026] The present invention has the following beneficial effects:

[0027] The present invention uses molybdate oxide as an additive, which is mixed with graphite and burned together. Molybdate oxide can enrich radionuclides in itself during the graphite combustion process by utilizing the bonding effect between its own molybdate radical and radioactive nuclides, thereby eliminating the radioactive aerosol problem, and the radioactive nuclides can be easily separated therefrom later. In addition, the additive used remains solid during the graphite combustion process, has no flow permeability, and has no corrosive effect on equipment materials. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 It is a process flow chart of the present invention;

[0029] Figure 2 This is a picture of the granulated material and after combustion. DETAILED DESCRIPTION

[0030] The technical solution of the present invention is described clearly and completely below in conjunction with the accompanying drawings. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0031] In the description of the present invention, it should be noted that the directions or positional relationships indicated by "center", "up", "down", "left", "right", "vertical", "horizontal", "inside", "outside", etc. are directions or positional relationships based on the drawings, which are only for the convenience of describing the present invention and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as limiting the present invention. In addition, "first" and "second" are only used for descriptive purposes and cannot be understood as indicating or implying relative importance.

[0032] In addition, the technical features involved in the different embodiments of the present invention described below can be combined with each other as long as they do not conflict with each other.

[0033] like Figure 1 As shown, a method for reducing the volume of radioactive graphite that is easy to recover radioactive nuclides is applicable to carbon-based materials contaminated by radioactive metal nuclides, including but not limited to graphite and resin. Specifically, the method comprises the following steps:

[0034] Step 1: crushing radioactive graphite to obtain granular radioactive graphite, adding an initial batch of additives enriched with radionuclides, and grinding to obtain a mixture.

[0035] Specifically, the crushing treatment steps include coarse crushing, fine grinding, and screening to obtain granular radioactive graphite with a particle size of less than 2 mm, wherein the mass proportion of radioactive nuclides in the graphite is between 0.01% and 1%. The initial additive for enriching radioactive nuclides includes an oxide containing molybdate, and the cations in the oxide of molybdate include Ca 2+ , Fe 2+ , Fe 3+ 、Co 2+ 、Ni 2 + 、Zn 2+ , Mn 2+ , Ba 2+ 、Bi 3+ 、Cd 2+ , Sr 2+ , Pb 2+ Mg 2+ 、Ag +At least one of the following, wherein representative molybdate oxides include CaMoO4, FeMoO4, Fe2(MoO4)3, CoMoO4, NiMoO4, ZnMoO4, MnMoO4, BaMoO4, Bi2MoO6, CdMoO4, SrMoO4, PbMoO4, MgMoO4, and Ag2MoO4; wherein the grinding ratio of the granular radioactive graphite and the initial batch of additives enriched with radionuclides is 1:0.25-4 in parts by weight, and the use of this weight ratio can not only effectively suppress graphite dust during the combustion process, but also ensure low-temperature, static combustion of the graphite under the catalytic action of the additive.

[0036] Step 2: Granulate the mixture obtained in step 1 to obtain granulated graphite.

[0037] Specifically, in step 2, a granulation binder is further added, the granulation binder includes any one of water and an organic binder, the organic binder can be polyvinyl alcohol commonly used in industry, and the weight proportion of the granulation binder is between 2-25%; the particle size of the granulated graphite is 2-10 mm.

[0038] Step 3: Burning the granulated graphite to obtain incineration ash.

[0039] Specifically, the incineration ash is used as an additive for subsequent batches. In step 3, the specific steps of burning granulated graphite include:

[0040] Step 3.1: Add granulated graphite into the combustion furnace and control the temperature of the constant temperature section to 500-800℃;

[0041] Step 3.2: introducing the reaction gas preheated to 500-800°C into the combustion furnace and keeping it warm for 5-10 hours, wherein the reaction gas is either an oxygen-containing inert gas or air, wherein the oxygen content in the oxygen-containing inert gas is between 21-100 vol%; Figure 2 Shown are the granulated materials and the products after combustion. Figure 2 Left - Gray-black granulated particles containing graphite. Figure 2 Right - White particles without graphite after graphite is completely vaporized.

[0042] Step 4: Recover the radionuclides.

[0043] Specifically, in step 4, the specific steps of recovering the radioactive nuclides include:

[0044] Step 4.1: Soak the incineration ash in liquid acid for a period of time, and filter to obtain a first filtrate; wherein the number of times the incineration ash is reused depends on the content of radionuclides in the incineration ash, generally 5-400 times; wherein the liquid acid is one of hydrochloric acid, nitric acid, and sulfuric acid;

[0045] Step 4.2: continuously adding soluble carbonate to the first filtrate obtained in step 4.1 until no more precipitation occurs, and filtering to obtain a second filtrate;

[0046] Step 4.3: Add a base to the second filtrate obtained in step 4.2, let it stand and filter to obtain a solid oxide precipitate containing radioactive nuclides; specifically, the base is any one of ammonia water, sodium hydroxide and potassium hydroxide.

[0047] Example 1

[0048] Step 1: crushing radioactive graphite to obtain granular radioactive graphite, adding an initial batch of additives enriched with radionuclides, and grinding to obtain a mixture.

[0049] Specifically, the crushing process includes coarse crushing, fine grinding, and screening to obtain granular radioactive graphite with a particle size of less than 2 mm, wherein the mass proportion of radioactive nuclides in the graphite is between 0.01%; the initial additive for enriching radioactive nuclides is CaMoO4; and the grinding weight ratio of granular radioactive graphite and CaMoO4 is 1:1.

[0050] Step 2: Granulate the mixture obtained in step 1 to obtain granulated graphite.

[0051] Specifically, in step 2, water is added as a granulation binder, and the weight proportion of water is 25%; the particle size of the granulated graphite is 5 mm.

[0052] Step 3: Burning the granulated graphite to obtain incineration ash, which can be used as an additive for subsequent batches.

[0053] Specifically, in step 3, the specific steps of burning granulated graphite include:

[0054] Step 3.1: Add granulated graphite into the combustion furnace and control the temperature of the constant temperature section to 600°C;

[0055] Step 3.2: Introduce the reaction gas preheated to 600° C. into the combustion furnace and keep it warm for 5 hours. The reaction gas is air.

[0056] Step 4: Recover the radionuclides.

[0057] Specifically, in step 4, the specific steps of recovering the radioactive nuclides include:

[0058] Step 4.1: Soak the incineration ash in liquid acid for a period of time, and filter to obtain a first filtrate; wherein the incineration ash is reused 400 times; wherein the liquid acid is hydrochloric acid;

[0059] Step 4.2: continuously adding sodium carbonate to the first filtrate obtained in step 4.1 until no more precipitation occurs, and filtering to obtain a second filtrate;

[0060] Step 4.3: adding a base to the second filtrate obtained in step 4.2, standing and filtering to obtain a solid oxide precipitate containing radioactive nuclides; specifically, the base is aqueous ammonia.

[0061] Example 2

[0062] Step 1: crushing radioactive graphite to obtain granular radioactive graphite, adding an initial batch of additives enriched with radionuclides, and grinding to obtain a mixture.

[0063] Specifically, the crushing process includes coarse crushing, fine grinding, and screening to obtain granular radioactive graphite with a particle size of less than 2 mm, wherein the mass proportion of radioactive nuclides in the graphite is 0.1%; the initial additive for enriching radioactive nuclides is CoMoO4; and the grinding weight ratio of granular radioactive graphite and CoMoO4 is 1:4.

[0064] Step 2: Granulate the mixture obtained in step 1 to obtain granulated graphite.

[0065] Specifically, in step 2, polyvinyl alcohol is further added as a granulation binder, and the weight proportion of polyvinyl alcohol is 10%; the particle size of the granulated graphite is 10 mm.

[0066] Step 3: Burning the granulated graphite to obtain incineration ash, which can be used as an additive for subsequent batches.

[0067] Specifically, in step 3, the specific steps of burning granulated graphite include:

[0068] Step 3.1: Add granulated graphite into the combustion furnace and control the temperature of the constant temperature section to 800°C;

[0069] Step 3.2: Introduce the reaction gas preheated to 800° C. into the combustion furnace and keep it warm for 10 hours. The reaction gas is an oxygen-containing inert gas; wherein the oxygen content in the oxygen-containing inert gas is 21 vol%.

[0070] Step 4: Recover the radionuclides.

[0071] Specifically, in step 4, the specific steps of recovering the radioactive nuclides include:

[0072] Step 4.1: Soak the incineration ash in liquid acid for a period of time, and filter to obtain a first filtrate; wherein the incineration ash is reused 50 times; wherein the liquid acid is nitric acid;

[0073] Step 4.2: continuously adding potassium carbonate to the first filtrate obtained in step 4.1 until no more precipitation occurs, and filtering to obtain a second filtrate;

[0074] Step 4.3: adding a base to the second filtrate obtained in step 4.2, standing and filtering to obtain a solid oxide precipitate containing radioactive nuclides; specifically, the base is sodium hydroxide.

[0075] Example 3

[0076] Step 1: crushing radioactive graphite to obtain granular radioactive graphite, adding an initial batch of additives enriched with radionuclides, and grinding to obtain a mixture.

[0077] Specifically, the crushing process includes coarse crushing, fine grinding, and screening to obtain granular radioactive graphite with a particle size of less than 2 mm, wherein the mass proportion of radioactive nuclides in the graphite is 1%; the initial additive for enriching radioactive nuclides is FeMoO4; the grinding weight ratio of granular radioactive graphite and FeMoO4 is 1:2.

[0078] Step 2: Granulate the mixture obtained in step 1 to obtain granulated graphite.

[0079] Specifically, in step 2, polyvinyl alcohol is further added as a granulation binder, and the weight proportion of polyvinyl alcohol is 15%; the particle size of the granulated graphite is 8 mm.

[0080] Step 3: Burning the granulated graphite to obtain incineration ash, which can be used as an additive for subsequent batches.

[0081] Specifically, in step 3, the specific steps of burning granulated graphite include:

[0082] Step 3.1: Add granulated graphite into the combustion furnace and control the temperature of the constant temperature section to 500°C;

[0083] Step 3.2: Introduce the reaction gas preheated to 500° C. into the combustion furnace and keep it warm for 8 hours. The reaction gas is an oxygen-containing inert gas; wherein the oxygen content in the oxygen-containing inert gas is 60 vol%.

[0084] Step 4: Recover the radionuclides.

[0085] Specifically, in step 4, the specific steps of recovering the radioactive nuclides include:

[0086] Step 4.1: Soak the incineration ash in liquid acid for a period of time, and filter to obtain a first filtrate; wherein the incineration ash is reused 5 times; wherein the liquid acid is sulfuric acid;

[0087] Step 4.2: continuously adding sodium carbonate to the first filtrate obtained in step 4.1 until no more precipitation occurs, and filtering to obtain a second filtrate;

[0088] Step 4.3: adding a base to the second filtrate obtained in step 4.2, standing and filtering to obtain a solid oxide precipitate containing radioactive nuclides; specifically, the base is potassium hydroxide.

[0089] Example 4

[0090] Step 1: crushing radioactive graphite to obtain granular radioactive graphite, adding an initial batch of additives enriched with radionuclides, and grinding to obtain a mixture.

[0091] Specifically, the crushing process includes coarse crushing, fine grinding, and screening to obtain granular radioactive graphite with a particle size of less than 2 mm, wherein the mass proportion of radioactive nuclides in the graphite is 0.01%; the initial additive for enriching radioactive nuclides is BaMoO4; and the grinding weight ratio of granular radioactive graphite and BaMoO4 is 1:0.25.

[0092] Step 2: Granulate the mixture obtained in step 1 to obtain granulated graphite.

[0093] Specifically, in step 2, water is added as a granulation binder, and the weight of water accounts for 2%; the particle size of the granulated graphite is 2 mm.

[0094] Step 3: Burning the granulated graphite to obtain incineration ash, which can be used as an additive for subsequent batches.

[0095] Specifically, in step 3, the specific steps of burning granulated graphite include:

[0096] Step 3.1: Add granulated graphite into the combustion furnace and control the temperature of the constant temperature section to 500°C;

[0097] Step 3.2: Introduce the reaction gas preheated to 500° C. into the combustion furnace and keep it warm for 8 hours. The reaction gas is an oxygen-containing inert gas; wherein the oxygen content in the oxygen-containing inert gas is 100 vol%.

[0098] Step 4: Recover the radionuclides.

[0099] Specifically, in step 4, the specific steps of recovering the radioactive nuclides include:

[0100] Step 4.1: Soak the incineration ash in liquid acid for a period of time, and filter to obtain a first filtrate; wherein the incineration ash is reused 400 times; wherein the liquid acid is hydrochloric acid;

[0101] Step 4.2: continuously adding sodium carbonate to the first filtrate obtained in step 4.1 until no more precipitation occurs, and filtering to obtain a second filtrate;

[0102] Step 4.3: adding ammonia water to the second filtrate obtained in step 4.2, standing and filtering to obtain a solid oxide precipitate containing radioactive nuclides; specifically, the base is potassium hydroxide.

[0103] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

[0104] The above specific implementation methods are detailed descriptions of the present invention. It cannot be determined that the specific implementation methods of the present invention are limited to these descriptions. For ordinary technicians in the technical field to which the present invention belongs, several simple deductions and substitutions can be made without departing from the concept of the present invention, which should be regarded as belonging to the protection scope of the present invention.

Claims

1. A method for reducing the volume of radioactive graphite for easy recovery of radioactive nuclides, It is characterized in that The steps include: Step 1: crushing radioactive graphite to obtain granular radioactive graphite, adding an initial batch of additives enriched with radionuclides, and grinding to obtain a mixture; Step 2: Granulate the mixture obtained in step 1 to obtain granulated graphite; Step 3: burning granulated graphite to obtain incineration ash; Step 4: Recover the radionuclides.

2. A method for reducing the volume of radioactive graphite for easy recovery of radioactive nuclides according to claim 1, It is characterized in that The initial batch of additives for enriching radionuclides includes an oxide containing molybdate.

3. The method for reducing the volume of radioactive graphite of the radioactive nuclide according to claim 2, It is characterized in that The cations in the molybdate oxide include Ca 2+ , Fe 2+ , Fe 3+ 、Co 2+ 、Ni 2+ 、Zn 2+ , Mn 2+ , Ba 2+ 、Bi 3+ 、Cd 2+ , Sr 2+ , Pb 2+ Mg 2+ 、Ag + At least one of .

4. The method for reducing the volume of radioactive graphite of a radionuclide according to claim 1, It is characterized in that The mass proportion of radioactive nuclides in the radioactive graphite is 0.01-1%.

5. The method for reducing the volume of radioactive graphite of a radionuclide according to claim 1, It is characterized in that In the step 1, the grinding ratio of the granular radioactive graphite and the additive for enriching radionuclides is 1:0.25-4 in parts by weight.

6. The method for reducing the volume of radioactive graphite of a radionuclide according to claim 1, It is characterized in that In the step 2, a granulation binder is also added, and the mass percentage of the granulation binder is 2-25%; the granulation binder includes any one of water and an organic binder.

7. The method for reducing the volume of radioactive graphite of a radioactive nuclide according to claim 1, It is characterized in that In the step 2, the particle size of the granulated graphite is 2-10 mm.

8. The method for reducing the volume of radioactive graphite of a radioactive nuclide according to claim 1, It is characterized in that In step 3, the incineration ash is used as an additive for subsequent batches, and the specific steps of burning granulated graphite include: Step 3.1: Add granulated graphite into the combustion furnace and control the temperature of the constant temperature section to 500-800℃; Step 3.2: Introduce the reaction gas preheated to 500-800° C. into the combustion furnace and keep it warm for 5-10 hours. The reaction gas is either an oxygen-containing inert gas or air; the oxygen content is 21-100 vol%.

9. The method for reducing the volume of radioactive graphite of a radionuclide according to claim 1, It is characterized in that In step 4, the specific steps of recovering the radioactive nuclides include: Step 4.1: Soak the incineration ash from step 3 in liquid acid for a period of time, and filter to obtain a first filtrate; the liquid acid is any one of hydrochloric acid, sulfuric acid, and nitric acid; Step 4.2: continuously adding soluble carbonate to the first filtrate obtained in step 4.1 until no more precipitation occurs, and filtering to obtain a second filtrate; Step 4.3: Add alkali to the second filtrate obtained in step 4.2, let stand and filter to obtain a solid oxide precipitate containing radioactive nuclides.

10. The method for reducing the volume of radioactive graphite of a radioactive nuclide according to claim 9, It is characterized in that In step 4.3, the base is any one of ammonia water, sodium hydroxide and potassium hydroxide.

Citation Information

Cited By

  • Treatment method of graphite waste containing radioactive elements

    CN120356716A

  • A method and system for extracting carbon-14 from radioactive waste graphite

    CN122889471A