Preparation method of co-fired inductor
Through the secondary pressing and multi-stage annealing process combined with magnetic powder coating technology, the problem of insufficient molding density and insulation of co-fired inductors is solved, the high-frequency efficiency and electrical performance are improved, and it is suitable for the inductor needs of modern electronic products.
Patent Information
- Application Number
- CN202410997296.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-24
- Publication Date
- 2024-10-15
AI Technical Summary
Due to the mismatch between the pressing strength and annealing temperature during the molding process of existing co-fired inductors, the inductor density is uneven, the insulation effect is poor, and the high-frequency efficiency is low, which cannot meet the needs of high-frequency small-volume inductors.
Using a secondary press molding and multi-stage annealing process, the first press pressure is lower than the second press, and the second press pressure is higher than the first press. Combining inorganic and organic coating processes, low-temperature annealing releases internal stress, and high-temperature annealing improves magnetic permeability and insulation performance. , and improve the surface insulation performance through phosphating treatment.
It significantly improves the molding density, insulation resistance and high-frequency efficiency of the inductor, avoids product cracking, improves the overall performance and insulation characteristics of the inductor, and is suitable for high-frequency applications.
Smart Images

Figure CN118782371A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of magnetic component manufacturing, and in particular relates to a method for preparing a co-fired inductor. Background Art
[0002] With the rapid development of electronic products, the continuous improvement of computer computing power, the emergence and application of artificial intelligence, the packaging space is becoming increasingly limited, the number of components is increasing rapidly, and the size of the inductor used is also greatly reduced. The inductance performance of traditional one-piece molded inductors is difficult to reach the level of ferrites, but ferrites are resistant to high temperatures, have poor high current tolerance, and occupy a large space, which cannot meet the current demand for high-frequency, low-loss, and small-volume inductors. The emergence of soft magnetic metal powder core inductors has perfectly replaced traditional ferrites. The existing co-fired inductors have poor molding effects and poor insulation effects after high-temperature annealing, resulting in low inductor Q values, high losses, and low high-frequency efficiency.
[0003] The patent with publication number CN112735752A discloses a co-fired inductor formed under high pressure, which is coated with phosphoric acid insulation and adhesive. If the pressure of a single molding is too high, it is easy to make the internal density of the product uneven. If an air gap is generated, it will cause a large internal stress. A single annealing will produce dark cracks, and the annealing temperature is high. The phosphoric acid insulation of the iron-nickel material is reduced during high-temperature annealing. The eddy current loss of the resulting inductor is large and it is difficult to exceed the level of ferrite. The patent with publication number CN114743785A discloses an inductor production process using two moldings, which is characterized in that the first stamping molding pressure is high, and the density of the iron core after molding is large, but the second molding pressure is small, which will cause the conductor and the joint surface to have insufficient bonding strength during the second pressing, causing the product to crack. The patent with publication number CN116313460A discloses a new inductor production process, which aims to improve the efficiency of inductor processes such as powder filling, molding and winding. Although the first molding pressure is smaller than the second, the pressing process of this invention does not involve coordination with the annealing process and the magnetic powder coating process, and does not consider the close relationship between the pressing strength and the annealing temperature and the magnetic powder coating.
[0004] Therefore, the prior art lacks a method for preparing a co-fired inductor, and it is necessary to simultaneously consider the close relationship between the pressing strength, annealing temperature and magnetic powder coating in the inductor manufacturing process, so as to effectively improve the molding density, insulation resistance, moldability and high-frequency efficiency of the inductor. Summary of the invention
[0005] The present invention provides a method for preparing a co-fired inductor. Through the coating method, molding and annealing process of the present invention, the molding density, insulation resistance, molding property and high-frequency efficiency of the inductor can be effectively improved.
[0006] A method for preparing a co-fired inductor, wherein the inductor is formed by pressing, annealing and phosphating a conductor and magnetic powder, and both ends of the conductor extend outside the magnet. The preparation method comprises the following steps: The magnetic powder needs to be pressed twice to form an inductor. First, the magnetic powder is filled into the mold cavity and pressed into the matrix for the first time. Cold pressing or warm pressing with a pressing temperature below 100°C is used. The pressure of the first pressing is 15%~30% of the pressure of the second pressing. The conductor is placed on the surface of the matrix, and then the magnetic powder is filled into the cavity. The semi-finished product is formed by the second pressing. The pressure of the second pressing is 800~1600MPa, and it is pressed at room temperature or hot pressing not higher than 200°C. Wherein, a double annealing method is adopted, and the first annealing temperature is lower than the second annealing temperature; The magnetic powder is obtained after batching, insulation coating and granulation processes, wherein a double coating process is adopted, namely, inorganic coating first and then organic coating.
[0007] Preferably, the density of the matrix is 3-4.5 g / cm 3 The density of the semi-finished product is 5.8~7.2g / cm 3 ; Preferably, the conductor is a straight copper sheet without enameled wire or a U-shaped, "X"-shaped, "G"-shaped or other special-shaped copper sheet.
[0008] Preferably, if the selected conductor is a special-shaped copper sheet, on the contact surface between the copper sheet and the substrate, when the contact area accounts for more than 40% of the total area of the substrate on that surface, an organic coating agent with an epoxy structure is preferably selected during the organic coating treatment. Due to the presence of modified epoxy bonds, it has better bonding strength and a certain high-temperature stability. At the same time, the molding pressure and annealing temperature need to be appropriately reduced to improve the insulation resistance (IR) and strength of the product.
[0009] Preferably, the first molding condition is warm pressing at a temperature not exceeding 80° C., with no pressure holding treatment or a pressure holding time of less than 3 seconds.
[0010] Preferably, the second molding pressure is 1000-1400 MPa, the second molding condition is hot pressing at no higher than 180° C., and the holding time is 0.5-5 s; Preferably, during the second molding, the molding pressure of the iron-nickel material is 800-1400 MPa, and the molding pressure of the iron-silicon-aluminum material is 1000-1600 MPa.
[0011] Among them, the inductor adopts a secondary annealing method, the annealing atmosphere is one or more of hydrogen, nitrogen, and argon, the oxygen content is less than 100ppm, the first annealing temperature is 80~300℃, the insulation time is 30~150min, the preferred first annealing temperature is 150-220℃, the insulation time is 60-80min, and the temperature is naturally reduced; the second annealing temperature is 500~800℃, the annealing time is 30~120min, the cooling rate is greater than 30℃ / min, the preferred second annealing temperature is 550-750℃, and the insulation time is 60-100min. The first low-temperature annealing is performed to release the residual stress of the product and solidify the coating layer to reduce the cracking of the product. The second high-temperature annealing is performed to improve the magnetic permeability of the material and improve the strength of the product.
[0012] Among them, the second coating of magnetic powder is organic coating, and the organic coating agent will be carbonized and discharged during the high-temperature annealing process. In order to improve the insulation performance of the product, the annealed product needs to be phosphated to improve the surface insulation performance of the product; Preferably, the phosphating treatment is: placing the annealed inductor product in 2-7wt% dilute phosphoric acid, and heating it in an oil bath or water bath at 60-120°C; Preferably, the phosphating treatment is: placing the annealed inductor product in 3-6wt% dilute phosphoric acid, and heating it in an oil bath or water bath at 80-100°C.
[0013] Among them, the magnetic powder is obtained after batching, insulation coating and granulation processes.
[0014] The raw materials used in the formulation are a mixture of one or more of iron-nickel alloy powder, iron-silicon-aluminum alloy powder, iron-silicon-chromium alloy powder, molybdenum-permalloy powder, iron-silicon alloy powder and carbonyl iron powder.
[0015] Among them, the insulation coating is first carried out by inorganic coating, and then organic coating is carried out after baking.
[0016] Preferably, the inorganic coating is coated by oxidation method, and the coating step is to place the magnetic powder and the inorganic coating agent in a solvent and then mix and stir, the mass ratio of the inorganic coating agent to the solvent is 0.05-0.15:1, the mass ratio of the inorganic coating agent to the magnetic powder is 0.001-0.01:1, the mixing and stirring time is 20-60 minutes, the standing time after adding the solvent is 30-60 minutes, and the temperature condition of the coating treatment is 25-100°C; Preferably, the inorganic coating agent is a magnesium salt or silicate solution with a mass fraction of 2 to 8 wt%, preferably a magnesium carbonate solution; Preferably, the solvent is selected from acetone, ethanol, water or an ammonium salt solution with a mass fraction of 1-10wt%.
[0017] Preferably, during the magnetic powder baking process, the baking temperature is 60-120° C., the baking insulation time is 30-200 min, and the baking is carried out under an inert gas such as argon, helium or nitrogen.
[0018] Preferably, the step of organic coating is: mixing magnetic powder, solvent and organic coating agent, drying the coated magnetic powder at 100-200°C for 30-120min, and the mass ratio of organic coating agent, solvent and magnetic powder is 0.005-0.05:0.01-0.1:1; preferably, the organic coating agent is one or more of silicone resin, modified epoxy resin, modified epoxy silicone resin or phenolic resin; Preferably, the organic coating solvent is selected from one of xylene, acetone or ethanol.
[0019] Since the magnetic powder used in the present invention has been inorganically coated and organically coated, considering that too much organic coating agent will increase the bonding effect of the magnetic powder but is not conducive to improving the magnetic permeability and the inductance value, the coating agent content used in the organic coating is relatively low; considering that the organic coating agent has relatively good viscosity, the product can have a certain strength and formability under low-pressure one-time molding conditions, so the first molding pressure is designed to be lower, the purpose is to avoid the matrix density being too high during the first pressing, and the insufficient bonding strength of the contact surface during the second pressing causing the product to crack. Compared with the one-time molding process, the two-pressing process makes the copper sheet better centered, the overall density more uniform, and the density near the product winding higher, so the obtained product has more advantages in terms of initial inductance, saturation characteristics and conversion efficiency.
[0020] The coated powder is granulated, a granulating agent and a solvent are added to the powder, and after granulation, the magnetic powder is obtained by screening; Preferably, the screen is selected to be -80~250 mesh; Preferably, the granulating agent is one or more of silicone resin, modified epoxy resin, modified epoxy silicone resin or phenolic resin, and the solvent is selected from one of xylene solution, acetone solution or ethanol, and the mass ratio of the granulating agent, solvent and magnetic powder is 0.01~0.08:0.1:2.
[0021] Preferably, the specification and amount of the granulating agent used for granulation are the same as those of the organic coating agent for secondary coating.
[0022] The invention provides a method for preparing magnetic powder for co-fired inductor, which is a method for preparing magnetic powder in the process of preparing the co-fired inductor.
[0023] Compared with the prior art, the present invention has the following beneficial effects: The present invention provides a method for preparing a co-fired inductor. Through the coating method, molding and annealing process of the present invention, the molding density, insulation resistance, molding property and high-frequency efficiency of the inductor can be effectively improved; The existing co-fired inductors often have the problem of internal cracking due to insufficient bonding strength of powder materials. The magnetic powder secondary coating system proposed in the present invention can make the inductor product have better strength. On this basis, the second pressure is much higher than the first molding pressure, the purpose is to avoid the matrix density of the first pressing being too high, and the insufficient bonding strength of the contact surface during the second pressing causing the product to crack, so that the internal density of the product can be more uniform, with higher electrical performance and insulation characteristics; considering that the organic coating agent will be carbonized and discharged during the high temperature process, which will lead to an increase in the amount of inductor debinding, a multi-stage annealing is proposed, firstly through a low-temperature annealing, the temperature of this low-temperature annealing does not reach the debinding temperature and the winding softening temperature, only the internal stress generated by pressing is released in advance, and then through a high-temperature annealing, the debinding and softening of the winding simultaneously stimulate the material properties, effectively release the product internal stress, reduce power consumption, and effectively avoid product cracking. After annealing, phosphating treatment can be performed to improve the pressure resistance and insulation performance of the product, and the obtained inductor has better high-frequency characteristics; The co-fired inductor of the present invention is mainly used to power chips, including but not limited to servers, communication power supplies, GPUs, FPGAs, power modules, laptop computers and other fields. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 A schematic diagram of the matrix formed by the first pressing; Figure 2 Schematic diagram of the position of the substrate and the copper sheet; Figure 3 It is a schematic diagram of the semi-finished product structure; In the figure, 1-contact surface between copper sheet and substrate, 2-substrate, 3-copper sheet, 4-electrode groove, 5-semi-finished product. DETAILED DESCRIPTION
[0025] Example 1 is as follows: A method for preparing a co-fired inductor comprises the following steps: 1. The iron-nickel raw powders with particle sizes of -400 mesh, -600 mesh and -800 mesh are uniformly mixed in a mass ratio of 7:2:1 to obtain iron-nickel raw powders with D50 of 15um, D10 of 9um and D90 of 25um; 2. First, the oxidation method is used for coating. The original powder and the magnesium salt solution are placed in water and then mixed and stirred. The mass of the magnesium salt solution used is 5wt% magnesium carbonate solution, the mass ratio of magnesium carbonate content to magnetic powder is 0.001:1, and the mass ratio of magnesium carbonate content to water is 0.05:1. After the magnesium salt and magnetic powder are mixed and evenly stirred for 40 minutes, they are allowed to stand for 60 minutes; then, they are baked under nitrogen conditions, the baking temperature is 120°C, and the insulation time is 30-60 minutes. The baked powder is then subjected to secondary coating treatment. The secondary coating material is silicone resin, the solvent is acetone, and the mass ratio of silicone resin, solvent, and magnetic powder is 0.04:0.05:1. The powder after the secondary coating is dried in an oven at 150°C for 100 minutes. After 10 min, granulation treatment is carried out. The granulating agent is modified epoxy silicone resin, and the addition ratio is consistent with the organic coating agent. The magnetic powder required for the inductor is obtained by passing through a -80~250 mesh sieve. The magnetic permeability of the magnetic powder is 100, and the magnetic ring loss is 180kW / m under the test conditions of 1MHz and 20mT. 3 , and has good bulk density; 3. Fill the magnetic powder into the mold cavity and perform the first pressing at 400MPa pressure at room temperature to form the matrix 2 (see Figure 1 ), the holding time is 2s, there are electrode grooves 4 at both ends of the substrate, a copper sheet 3 is placed on the surface of the substrate, and the contact surface 1 between the copper sheet and the substrate is Figure 2 As shown, after the magnetic powder is filled again, it is pressed for the second time to form a semi-finished product 5 (see Figure 3 ), the second pressing pressure is 1200MPa, the holding time is 3s, and the pressing temperature is room temperature. The copper sheet has a length, width and height of 1.8mm×18mm×0.3mm, and there is no insulating paint film on the surface of the copper sheet. After the magnetic powder is buried, the two ends are exposed to the outside of the magnet; 4. The semi-finished product is subjected to the first annealing treatment in an air atmosphere at a temperature of 250°C for 2 hours. After annealing, the product is naturally cooled. After natural cooling, the second annealing treatment is carried out at a temperature of 700°C for 50 minutes. This process is carried out in a nitrogen atmosphere with an oxygen content of 80ppm. After annealing, the product is water-cooled at a cooling rate of 35°C / min. After annealing, the product is subjected to phosphating treatment, that is, the product is placed in 5wt% dilute phosphoric acid, water-bathed at 80°C for 5 minutes, and naturally dried to obtain the inductor product.
[0026] Comparative Example 1 is as follows: A method for preparing a co-fired inductor comprises the following steps: 1. The iron-nickel raw powder used is the same as that in Example 1; 2. The original powder was treated with phosphoric acid and then coated with epoxy resin. The original powder was mixed with phosphoric acid solution. The phosphoric acid concentration in the solution was 0.01 g / mL, and the mass ratio of phosphoric acid solution to original powder was 1:3. Stirring was performed at 80°C for 30-40 minutes. After standing for 30 minutes, the powder was washed with acetone solution and dried at 60°C for 40 minutes. After granulation in the granulator, the magnetic powder was passed through a -80~250 mesh screen to obtain a magnetic powder with a magnetic permeability of 100. The magnetic ring loss at 1MHz and 20mT was 237kw / m 3 ; 3. The magnetic powder pressing process is the same as that in Example 1; 4. After pressing, the semi-finished product was annealed at 700℃ nitrogen for 50min, the cooling rate was 35℃ / min, the oxygen content was 80ppm, and the nitrogen flow rate was 9m 3 / h, and get the inductance product.
[0027] Comparative Example 2 is as follows: The iron-nickel raw powder used in Comparative Example 2 is the same as that in Example 1, the preparation method of the magnetic powder is the same as that in Example 1, and the pressing process of the magnetic powder is the same as that in Example 1, except that the semi-finished product is annealed once, the annealing temperature is 720°C, the holding time is 60min, the atmosphere is nitrogen, and the nitrogen flow rate is 10m 3 / h, oxygen content is 80ppm, and cooling rate is 35℃ / min.
[0028] Compared with Example 1, Comparative Example 1 and Comparative Example 2, it can be seen from Table 1 that, under the same level of product density, initial inductance and DC bias, the Q value of Example 1 is significantly improved, and the loss under 1MHz, 20mT conditions is reduced, indicating that the coating process proposed in the present invention has a significant effect on improving the insulation of the product, and the corresponding product has lower eddy current loss and has a certain efficiency advantage under heavy load conditions.
[0029] Table 1 Comparison of inductance performance of Example 1, Comparative Example 1, and Comparative Example 2
[0030] Example 2 is as follows: A method for preparing a co-fired inductor comprises the following steps: 1. Use raw powders of different particle sizes for batching, and select -300 mesh and -700 mesh sendust raw powders with a weight ratio of 1:3.5 for mixing; 2. The coating conditions of the original powder are the same as those in Example 1. After granulation and screening (consistent with Example 1), the finished magnetic powder with a magnetic permeability of 80 is obtained. Under the test conditions of 1MHz and 20mT, the magnetic ring loss is 176kw / m 3 ; 3. Fill the magnetic powder into the mold cavity, press it for the first time at 300MPa pressure to form the matrix, hold the pressure for 2s, press at 80℃, have electrode grooves at both ends of the matrix, place copper sheets on the surface of the matrix, and fill the magnetic powder again for the second pressing, press at 80℃, press at 1300MPa pressure, hold the pressure for 2s, and obtain a density of not less than 6.2g / cm 3 The semi-finished product, wherein the length, width and height of the copper sheet are 2.7 mm×20 mm×0.55 mm, the surface of the copper sheet has no insulating paint film, and both ends are exposed outside the magnet after the magnetic powder is buried; 4. The semi-finished product is subjected to the first annealing treatment in an air atmosphere at a temperature of 200°C and a holding time of 2h. After annealing, the product is naturally cooled and subjected to the second annealing treatment at a temperature of 750°C and a holding time of 50min. This process is carried out in a nitrogen atmosphere. After annealing, the product is water-cooled at a cooling rate of 35°C / min. After annealing, the semi-finished product is placed in 5wt% dilute phosphoric acid and placed in a water bath at 80°C for 5 minutes. After natural drying, the inductor product is obtained. The product has a good appearance without cracking, and the solder is heat-resistant without cracking.
[0031] Comparative Example 3 is as follows: The raw materials used in Comparative Example 3 are the same as those in Example 2, and the preparation process of the magnetic powder is the same as that in Example 2, except that the molding process is one-time molding, the molding pressure is 1200 MPa, the holding time is 50 s, the annealing method of the semi-finished product is one-time annealing, the first annealing temperature is 200°C, the annealing temperature is 750°C, the holding time is 50°C, and the annealing heating rate is 6°C / min. It is found that dark cracks are generated in the middle part of the electrode surface of the inductor product in the solder heat resistance test, and the cracking ratio is 1 / 3. This is mainly due to the fact that during the annealing pressure release process of the product, the internal air gap expands due to heat, the stress is concentrated, and the high-density magnetic core and the copper sheet have a large difference in springback, which leads to product cracking.
[0032] Comparative analysis of Example 2 and Comparative Example 3 shows that the multi-stage pressing process and multiple annealing processes have certain advantages in product appearance and strength.
[0033] Example 3 is as follows: A method for preparing a co-fired inductor comprises the following steps: 1. Select the original powder of sendustine and iron-nickel in a weight ratio of 2:8, wherein the D50 of iron-nickel is 10um and the D50 of sendustine is 12um; 2. The preparation process of magnetic powder is the same as that of Example 1. The magnetic permeability of the obtained magnetic powder is 90. The magnetic ring loss is measured at 1MHz and 20mT to be 177kw / m 3 ; 1MHz, 50mT magnetic powder loss is 1300kW / m 3 ; 3. Place the magnetic powder in the mold cavity and use 300Mpa molding pressure for the first compression molding, hold the pressure for 2s, and the molding temperature is room temperature. The matrix density obtained is 3.45g / cm 3 There are electrode grooves at both ends of the substrate, copper sheets are placed on the surface of the substrate, and magnetic powder is filled again for the second pressing. The molding pressure of the second pressing is 1500MPa, the holding time is 1s, and the pressing is performed at room temperature. The density of the pressed product is 6.7~7g / cm 3 , where the length and width of the copper sheet are 20 mm×2.7 mm×0.35 mm, there is no insulating paint film on the surface of the copper sheet, and after the magnetic powder is buried, both ends are exposed outside the magnet; 4. The semi-finished product is annealed multiple times. The first annealing temperature is 300°C, the holding time is 60 minutes, and the atmosphere is nitrogen atmosphere. The second annealing temperature is 700°C, the holding time is 60 minutes, the heating rate is 5°C / min, the atmosphere is hydrogen and nitrogen, and the gas flow ratio is 1:3. After annealing, the semi-finished product is water-cooled at a cooling rate of 35°C / min. After annealing, the semi-finished product is placed in 5wt% dilute phosphoric acid, water bathed at 80°C for 5 minutes, and naturally dried to obtain the inductor product.
[0034] Comparative Example 4 is as follows: The same material ratio as in Example 3 was adopted, and the coating method adopted phosphoric acid insulation treatment and modified epoxy silicone resin coating, as follows: a phosphoric acid solution with a pH of 3 was selected and mixed with the magnetic powder in a ratio of 1:1, and a water bath was placed at 80°C for 15 minutes. After washing, the powder was dried at 90°C for 45 minutes to obtain a primary coated powder, and then 1wt% of modified epoxy silicone resin was added as a secondary coating agent, and the powder was dissolved in acetone for secondary coating. The mass ratio of modified epoxy silicone resin, solvent and magnetic powder was 0.03:0.07:1. After sufficient stirring, the powder was dried in the shade for 3 hours. The finished magnetic powder was obtained by granulation and screening. The copper sheet conditions were consistent with those in Example 3, the molding pressure was 1500MPa, the holding time was 2s, the annealing method was single annealing, the annealing atmosphere was hydrogen and nitrogen, the gas flow ratio was 1:3, the annealing temperature was 700°C, the holding time was 60min, the heating rate was 5°C / min, and the cooling rate was 35°C / min.
[0035] Table 2 Comparison of inductance performance of Example 3 and Comparative Example 4
[0036] Example 3 is a powder coating system of the present invention with multiple pressing and annealing processes, and the resonant frequency of the product is 70~80MHz. Comparative Example 4 uses the traditional coating and manufacturing process of the current co-fired inductor, and the resonant frequency of the product is 30~40MHz, indicating that both products can be used normally, and the resonant frequency of Example 3 is higher. When the product characteristic parameters and size parameters are close, the board test is carried out, and the test conditions are 700kHz, 12V to 1.1V. It can be seen from Table 2 that the coating and molding annealing process of the present invention has a greater advantage in both light load conversion efficiency and heavy load conversion efficiency compared with the prior art, mainly due to the coating method and multiple annealing process used, which fully releases the internal stress, and the second pressing and holding time is short, the die wind direction of the product demolding is low, and it has good insulation properties, low product magnetic loss, excellent light load performance, and under heavy load conditions, the conversion efficiency of Example 3 is greater than that of Comparative Example 4.
[0037] The above content is a further explanation of the present invention in combination with specific or preferred implementation methods. It cannot be considered that the implementation of the present invention is limited to the above embodiments. For ordinary practitioners in the field of the present invention, simple modifications or changes made within the conceptual framework of this invention are within the protection scope and disclosure scope of the present invention.
Claims
1. A method for preparing a co-fired inductor, characterized in that: The inductor is formed by pressing, annealing and phosphating a conductor and magnetic powder, and both ends of the conductor extend outside the magnet. The preparation method includes the following steps: The magnetic powder needs to be pressed twice to form an inductor. First, the magnetic powder is filled into the mold cavity and pressed into the matrix for the first time. Cold pressing or warm pressing with a pressing temperature below 100°C is used. The pressure of the first pressing is 15%~30% of the pressure of the second pressing. The conductor is placed on the surface of the matrix, and then the magnetic powder is filled into the cavity. The semi-finished product is formed by the second pressing. The pressure of the second pressing is 800~1600MPa, and it is pressed at room temperature or hot pressing not higher than 200°C. Wherein, a double annealing method is adopted, and the first annealing temperature is lower than the second annealing temperature; The magnetic powder is obtained after batching, insulation coating and granulation processes, wherein a double coating process is adopted, namely, inorganic coating first and then organic coating.
2. The method for preparing a co-fired inductor according to claim 1, characterized in that: The conductor is a straight copper sheet or a special copper sheet without enameled wire, and the density of the matrix is 3-4.5g / cm 3 The density of the semi-finished product is 5.8~7.2g / cm 3 .
3. The method for preparing a co-fired inductor according to claim 2, characterized in that: The conductor is a special-shaped copper sheet. On the contact surface between the copper sheet and the substrate, when the contact area accounts for more than 40% of the total area of the substrate, an organic coating agent with an epoxy structure is selected during organic coating treatment.
4. The method for preparing a co-fired inductor according to claim 1, characterized in that: The first molding condition is hot pressing at no more than 80°C, with no pressure holding treatment or a pressure holding time of less than 3s; the second molding pressure is 1000~1400MPa, the second molding condition is hot pressing at no more than 180°C, and the pressure holding time is 0.5~5s.
5. The method for preparing a co-fired inductor according to claim 1, characterized in that: A secondary annealing method is adopted, the annealing atmosphere is one or more of hydrogen, nitrogen, and argon, the oxygen content is less than 100ppm, the first annealing temperature is 80~300℃, the insulation time is 30~150min, and the temperature is naturally reduced; the second annealing temperature is 500~800℃, the annealing time is 30~120min, and the cooling rate is greater than 30℃ / min.
6. The method for preparing a co-fired inductor according to claim 1, characterized in that: The phosphating treatment is as follows: placing the annealed inductor product in 2-7wt% dilute phosphoric acid and performing oil bath or water bath heating treatment at 60-120°C.
7. The method for preparing a co-fired inductor according to claim 1, characterized in that: The raw materials used in the ingredients of the magnetic powder are a mixture of one or more of iron-nickel alloy powder, iron-silicon-aluminum alloy powder, iron-silicon-chromium alloy powder, molybdenum-permalloy powder, iron-silicon alloy powder and carbonyl iron powder.
8. The method for preparing a co-fired inductor according to claim 1, characterized in that: The inorganic coating adopts oxidation coating, and the coating steps are: placing the magnetic powder and the inorganic coating agent in a solvent and mixing and stirring, the mass ratio of the inorganic coating agent to the solvent is 0.05-0.15:1, the mass ratio of the inorganic coating agent content to the magnetic powder is 0.01-0.1:1, the mixing and stirring time is 20-60 minutes, the standing time after adding the solvent is 30-60 minutes, and the temperature condition of the coating treatment is 25-100°C; the inorganic coating agent is a magnesium salt or silicate solution with a mass fraction of 2-8wt%, and the solvent is selected from acetone, ethanol, water or an ammonium salt solution with a mass fraction of 1-10wt%; The inorganic coating treatment needs to be followed by baking, the baking temperature is 60-120° C., the baking insulation time is 30-200 min, and the baking is carried out under argon, helium or nitrogen gas.
9. The method for preparing a co-fired inductor according to claim 1, characterized in that: The organic coating step comprises: mixing magnetic powder, an organic coating agent and a solvent; drying the coated magnetic powder at 100-200° C. for 30-120 min; the mass ratio of the organic coating agent, the solvent and the magnetic powder is 0.005-0.05:0.01-0.1:1; the organic coating agent is one or more of silicone resin, modified epoxy resin, modified epoxy silicone resin or phenolic resin; and the solvent is one of xylene solution, acetone solution or ethanol.
10. A method for preparing magnetic powder for co-fired inductor, characterized in that: The preparation method is a method for preparing magnetic powder in the preparation process of the co-fired inductor as described in any one of claims 1-9.
Citation Information
Patent Citations
Integrally formed co-fired inductor and preparation method and application thereof
CN112735752A
Inductor production process adopting two-time forming
CN114743785A
Novel inductor production process and inductor device thereof
CN116313460A
Cited By
Preparation method of copper-magnetic co-fired inductor and copper-magnetic co-fired inductor
CN119993720A
Chip inductance element and preparation method and application thereof
CN120581331A