Power battery and preparation method thereof
The semi-solid electrode material layer of power batteries is prepared by extrusion, which solves the problems of complex battery production process, high cost and environmental pollution in traditional battery production, and achieves a high energy density, low-carbon and environmentally friendly production process.
Patent Information
- Application Number
- CN202410872970.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-01
- Publication Date
- 2024-10-15
AI Technical Summary
The traditional battery production process is complex, the production cost is high, the production cycle is long, and the solvent NMP used is toxic and can easily cause environmental pollution.
The extrusion method is used to prepare power batteries. The positive and negative electrode mixtures are uniformly extruded to form a semi-solid material layer, which is stacked to form a battery core. The electrodes are coated without solvent, simplifying the process and reducing energy consumption. Avoid fluid channeling problems.
It improves the energy density of the battery, simplifies the production process, reduces the manufacturing cost and production cycle, avoids the use of toxic solvents, and achieves a low-carbon and environmentally friendly production process.
Smart Images

Figure CN118782718A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of batteries, and in particular relates to a power battery and a preparation method thereof. Background Art
[0002] With the rapid development of new energy technologies in my country, electrochemical energy storage has been widely used due to its environmental protection, energy saving, high efficiency, and flexibility. At present, under the dual influence of product technology improvement and rapid service response, the demand for domestic power batteries continues to grow. In the traditional battery production process, the production process is complicated, the fixed asset investment of production equipment is large, the production cost is high, the production cycle is long, and the solvent NMP used is highly toxic and easily pollutes the environment. Summary of the invention
[0003] The embodiments of the present invention provide a power battery and a method for preparing the same, aiming to solve the problems of complex production process of traditional batteries, high production cost, long production cycle, and easy pollution to the environment.
[0004] To achieve the above object, on the one hand, an embodiment of the present invention provides a method for preparing a power battery, comprising the following steps:
[0005] S01, uniformly extruding the positive electrode mixture onto both sides of the first current collector to obtain a positive electrode sheet having a positive electrode material layer extruded on the side;
[0006] S02, uniformly extruding the negative electrode mixture onto both sides of the second current collector to obtain a negative electrode sheet having a negative electrode material layer extruded on the side;
[0007] S03, stacking the positive electrode sheets of step S01 and the negative electrode sheets of step S02, with the positive electrode sheets and the negative electrode sheets arranged alternately, to obtain a battery core; placing the battery core in a battery casing to obtain a power battery.
[0008] As a preferred embodiment, in step S01,
[0009] Taking the mass of the positive electrode mixture as 100%, the positive electrode mixture includes the following components in mass percentage: 20% to 25% of a first carbonate solvent, 65% to 75% of a positive electrode active mixture and 5% to 10% of a first additive.
[0010] The preparation method of the positive electrode mixture comprises the following steps: 20% to 25% of a first carbonate solvent, 65% to 75% of a positive electrode active mixture and 5% to 10% of a first additive are uniformly mixed to obtain a positive electrode mixture; the solid content of the positive electrode mixture is 75% to 80%.
[0011] The mixing is achieved by a double planetary vacuum mixer, comprising the following steps: stirring at 15 Hz±5 Hz for 10 min, and then stirring at 800 rpm±50 rpm and 40 Hz±5 Hz for 2 h.
[0012] Taking the mass of the positive electrode active mixture as 100%, the positive electrode active mixture includes the following components in mass percentage: 0.1% to 3% of a first binder, 81% to 96.9% of a first metal compound, 1% to 10% of a first conductive agent, and 2% to 6% of a first electrolyte.
[0013] The preparation method of the positive electrode active mixture comprises the following steps: uniformly mixing 0.1% to 3% of a first binder, 81% to 96.9% of a first metal compound, 1% to 10% of a first conductive agent and 2% to 6% of a first electrolyte to obtain a positive electrode active mixture.
[0014] The mixing is achieved by a double planetary vacuum mixer, comprising the following steps: stirring at a rotation speed of 500 rpm±50 rpm and a revolution speed of 15 Hz±5 Hz for 10 min, and then stirring at a rotation speed of 1000 rpm±50 rpm and a revolution speed of 40 Hz±5 Hz for 1 h.
[0015] The first binder is a fiber binder, one of PEO (polyethylene oxide) or PTFE (polytetrafluoroethylene), or a mixture of at least two of them; the first metal compound is at least one of lithium iron phosphate, lithium manganese oxide, lithium nickel cobalt manganese oxide or a sodium-containing compound; the first conductive agent is one of carbon black, graphene, carbon nanotubes and conductive graphite, or a mixture of at least two of them; the first electrolyte is lithium hexafluorophosphate (LIPF6), lithium bis(fluorosulfonyl)imide (LiFSI) or sodium hexafluorophosphate (NaPF6).
[0016] The first carbonate solvent is at least one of ethylene carbonate, dimethyl carbonate, diethyl carbonate or ethyl methyl carbonate; the first additive is lithium lanthanum zirconium oxide (LLZO / LiLaZrO), lithium aluminum titanium phosphate (LATP / LiAITi(PO 4 )) or lithium lanthanum titanium oxide (LLTO / LiLaTiO). Using the first electrolyte as a liquid electrolyte and the first additive as a solid electrolyte can well ensure the transmission of lithium ions.
[0017] The positive electrode material layer is a semi-solid material layer; the thickness of the positive electrode material layer is 0.010 mm to 2 mm; and the first current collector is an aluminum foil current collector.
[0018] In the present application, by adding a liquid first electrolyte to the positive electrode material layer and controlling the dosage ratio of each component of the positive electrode material layer, the positive electrode material layer forms a semi-solid coating, and the coating of the electrode material of the positive electrode sheet can be achieved by extrusion, so that the thickness of the electrode using the positive electrode sheet of the present application can be more than 1.2 times the thickness of the electrode using the traditional coating process, that is, the preparation of thick electrodes can be achieved by extrusion, which can effectively improve the energy density of the battery.
[0019] As a preferred embodiment, in step S02,
[0020] Taking the mass of the negative electrode mixture as 100%, the negative electrode mixture includes the following components in percentage by mass: 20% to 25% of a second carbonate solvent, 65% to 75% of a negative electrode active mixture and 5% to 10% of a second additive.
[0021] The method for preparing the negative electrode mixture comprises the following steps: uniformly mixing 20% to 25% of a second carbonate solvent, 65% to 75% of a negative electrode active mixture and 5% to 10% of a second additive to obtain a negative electrode mixture.
[0022] The mixing is achieved by a double planetary vacuum mixer, comprising the following steps: stirring at a rotation of 1800 rpm±50 rpm and a revolution of 40 Hz±5 Hz for 1 hour, and then stirring at a rotation of 1500 rpm±50 rpm and a revolution of 40 Hz±5 Hz for 2 hours.
[0023] Taking the mass of the negative electrode active mixture as 100%, the negative electrode active mixture includes the following components in mass percentage: 0.1% to 3% of a second binder, 86% to 96.9% of a second metal compound, 1% to 5% of a second conductive agent and 2% to 6% of a second electrolyte.
[0024] The preparation method of the negative electrode active mixture comprises the following steps: uniformly mixing 0.1% to 3% of a second binder, 86% to 96.9% of a second metal compound, 1% to 5% of a second conductive agent and 2% to 6% of a second electrolyte to obtain a negative electrode active mixture.
[0025] The mixing is achieved by a double planetary vacuum mixer, comprising the following steps: stirring at a rotation of 500 rpm ± 50 rpm and a revolution of 15 Hz ± 5 Hz for 10 min, and then stirring at a rotation of 1800 rpm ± 50 rpm and a revolution of 40 Hz ± 5 Hz for 1.5 h.
[0026] The second binder is a fiber binder, PEO (polyethylene oxide) or PTFE (polytetrafluoroethylene); the second metal compound is at least one of lithium titanate, graphite, hard carbon, soft carbon or a silicon-based negative electrode; the second electrolyte is lithium hexafluorophosphate (LIPF6), lithium bis(fluorosulfonyl)imide (LiFSI) or sodium hexafluorophosphate (NaPF6).
[0027] The second carbonate solvent is at least one of ethylene carbonate, dimethyl carbonate, diethyl carbonate or ethyl methyl carbonate; the second additive is lithium lanthanum zirconium oxide (LLZO / LiLaZrO), lithium aluminum titanium phosphate (LATP / LiAITi(PO 4 )) or lithium lanthanum titanium oxide (LLTO / LiLaTiO). Using the second electrolyte as a liquid electrolyte and the second additive as a solid electrolyte can well ensure the transmission of lithium ions.
[0028] The negative electrode material layer is a semi-solid material layer; the thickness of the negative electrode material layer is 0.010 mm to 2 mm; the second current collector is an aluminum foil current collector or a copper foil current collector.
[0029] In the present application, by adding a liquid second electrolyte to the negative electrode material layer and controlling the dosage ratio of each component of the negative electrode material layer, the negative electrode material layer forms a semi-solid coating, and the coating of the electrode material of the negative electrode sheet can be achieved by extrusion, so that the thickness of the electrode of the negative electrode sheet using the present application can be more than 1.2 times the thickness of the electrode using the traditional coating process, that is, the preparation of thick electrodes can be achieved by extrusion, which can effectively improve the energy density of the battery.
[0030] As a preferred implementation, in step S03,
[0031] A separator is arranged between the positive electrode sheet and the negative electrode sheet.
[0032] The battery core is a lithium battery core or a sodium battery core.
[0033] On the other hand, an embodiment of the present invention further provides a power battery, which is prepared by the above preparation method.
[0034] The present application realizes the coating of the electrode material of the positive electrode sheet and the negative electrode sheet by extrusion, so that the thickness of the electrode of the positive electrode sheet and the negative electrode sheet of the present application can be more than 1.2 times the thickness of the electrode of the traditional coating process, that is, the preparation of thick electrodes by extrusion can effectively improve the energy density of the battery. Moreover, the electrode material layer of the positive and negative electrode sheets of the present application adopts a semi-solid layer, which can greatly increase the voltage of the single cell, and at the same time prevent the occurrence of liquid channeling between the positive and negative electrode sheets, thereby effectively avoiding the problem of electrolyte channeling and electrolyte decomposition. The preparation method of the present application is simple, no solvent is used in the preparation process, the use of toxic solvent NMP is eliminated, and there is no need for repeated drying of the electrode, which greatly reduces the energy consumption in the manufacturing process, and is low-carbon and environmentally friendly. The preparation method of the present application does not have a coating process, the equipment capital investment is small, the process is simple, the production efficiency is high, the overall manufacturing cost can be reduced by 10-20% compared with the traditional process, and the production cycle is shortened by about 20%, which can effectively improve the capital turnover rate. BRIEF DESCRIPTION OF THE DRAWINGS
[0035] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on the structures shown in these drawings without paying creative work.
[0036] Figure 1 It is a battery cycle curve diagram of the power battery prepared by Example 1 of the present application. DETAILED DESCRIPTION
[0037] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0038] It should be noted that if the embodiments of the present invention involve directional indications (such as up, down, left, right, front, back, top, bottom...), the directional indications are only used to explain the relative position relationship, movement status, etc. between the components in a certain specific posture. If the specific posture changes, the directional indication will also change accordingly.
[0039] In this application, unless otherwise clearly specified and limited, the terms "installed", "connected", "connected", "fixed" and the like should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection or an indirect connection through an intermediate medium, it can be the internal connection of two elements or the interaction relationship between two elements, unless otherwise clearly defined. For ordinary technicians in this field, the specific meanings of the above terms in this application can be understood according to specific circumstances.
[0040] It should be noted that when an element is referred to as being "fixed to" or "disposed on" another element, it may be directly on the other element or there may be an intermediate element. When an element is considered to be "connected to" another element, it may be directly connected to the other element or there may be an intermediate element at the same time.
[0041] In addition, if there are descriptions involving "first", "second", etc. in the embodiments of the present invention, the descriptions of "first", "second", etc. are only used for descriptive purposes and cannot be understood as indicating or suggesting their relative importance or implicitly indicating the number of the indicated technical features. Therefore, the features defined as "first" and "second" may explicitly or implicitly include at least one of the features. In addition, the technical solutions between the various embodiments can be combined with each other, but they must be based on the ability of ordinary technicians in the field to implement them. When the combination of technical solutions is contradictory or cannot be implemented, it should be deemed that such a combination of technical solutions does not exist and is not within the scope of protection required by the present invention.
[0042] In the embodiments of the present application, the present application can be implemented by controlling the usage ratio of each component of the positive electrode mixture and the negative electrode mixture so that it is within the above-mentioned required range.
[0043] In the embodiments of the present application, the moisture content of all raw materials is required to be less than 400ppm; the diaphragm, current collector housing and other accessories are removed from the packaging materials before use and dried at an ambient dew point temperature of less than -35°C for a drying time of more than 4 hours before use.
[0044] Example 1
[0045] A method for preparing a power battery comprises the following steps:
[0046] S01, uniformly extruding the positive electrode mixture onto both sides of the first current collector to obtain a positive electrode sheet having a positive electrode material layer extruded on the side;
[0047] S02, uniformly extruding the negative electrode mixture onto both sides of the second current collector to obtain a negative electrode sheet having a negative electrode material layer extruded on the side;
[0048] S03, stacking the positive electrode sheets of step S01 and the negative electrode sheets of step S02, with the positive electrode sheets and the negative electrode sheets arranged alternately, to obtain a battery core; placing the battery core in a battery casing to obtain a power battery.
[0049] In step S01,
[0050] Taking the mass of the positive electrode mixture as 100%, the positive electrode mixture includes the following components in percentage by mass: 20% of a first carbonate solvent, 75% of a positive electrode active mixture and 5% of a first additive.
[0051] The preparation method of the positive electrode mixture comprises the following steps: 20% of a first carbonate solvent, 75% of a positive electrode active mixture and 5% of a first additive are uniformly mixed to obtain a positive electrode mixture; the solid content of the positive electrode mixture is 80%.
[0052] The mixing is achieved by a double planetary vacuum mixer, comprising the following steps: stirring at 15 Hz revolution for 10 min, and then stirring at 800 rpm and 40 Hz revolution for 2 h.
[0053] Based on 100% by mass of the positive electrode active mixture, the positive electrode active mixture includes the following components by mass percentage: 0.1% of a first binder, 96.9% of a first metal compound, 1% of a first conductive agent, and 2% of a first electrolyte.
[0054] The preparation method of the positive electrode active mixture comprises the following steps: 0.1% of a first binder, 96.9% of a first metal compound, 1% of a first conductive agent and 2% of a first electrolyte are uniformly mixed to obtain a positive electrode active mixture.
[0055] The mixing is achieved by a double planetary vacuum mixer, comprising the following steps: stirring at a rotation speed of 500 rpm and a revolution speed of 15 Hz for 10 min, and then stirring at a rotation speed of 1000 rpm and a revolution speed of 40 Hz for 1 h.
[0056] The first binder is PEO; the first metal compound is lithium iron phosphate; the first conductive agent is carbon black; and the first electrolyte is lithium hexafluorophosphate.
[0057] The first carbonate solvent is ethylene carbonate; and the first additive is lithium lanthanum zirconium oxide.
[0058] The positive electrode material layer is a semi-solid material layer; the thickness of the positive electrode material layer is 2 mm; and the first current collector is an aluminum foil current collector.
[0059] In step S02,
[0060] Taking the mass of the negative electrode mixture as 100%, the negative electrode mixture includes the following components in percentage by mass: 25% of a second carbonate solvent, 65% of a negative electrode active mixture and 10% of a second additive.
[0061] The method for preparing the negative electrode mixture comprises the following steps: uniformly mixing 25% of a second carbonate solvent, 65% of a negative electrode active mixture and 10% of a second additive to obtain a negative electrode mixture.
[0062] The mixing is achieved by a double planetary vacuum mixer, comprising the following steps: stirring at a rotation speed of 1800 rpm and a revolution speed of 40 Hz for 1 hour, and then stirring at a rotation speed of 1500 rpm and a revolution speed of 40 Hz for 2 hours.
[0063] Based on 100% of the mass of the negative electrode active mixture, the negative electrode active mixture includes the following components in mass percentage: 3% of a second binder, 86% of a second metal compound, 5% of a second conductive agent, and 6% of a second electrolyte.
[0064] The method for preparing the negative electrode active mixture comprises the following steps: uniformly mixing 3% of a second binder, 86% of a second metal compound, 5% of a second conductive agent and 6% of a second electrolyte to obtain a negative electrode active mixture.
[0065] The mixing is achieved by a double planetary vacuum mixer, comprising the following steps: stirring at a rotation speed of 500 rpm and a revolution speed of 15 Hz for 10 min, and then stirring at a rotation speed of 1800 rpm and a revolution speed of 40 Hz for 1.5 h.
[0066] The second binder is PTFE; the second metal compound is graphite; and the second electrolyte is lithium hexafluorophosphate.
[0067] The second carbonate solvent is ethylene carbonate; and the second additive is lithium lanthanum zirconium oxide.
[0068] The negative electrode material layer is a semi-solid material layer; the thickness of the negative electrode material layer is 2 mm; and the second current collector is an aluminum foil current collector.
[0069] In step S03,
[0070] A diaphragm is arranged between the positive electrode sheet and the negative electrode sheet; and the battery core is a lithium battery core.
[0071] The power battery of this embodiment is subjected to formation-fluid replenishment-standing-sealing-capacity division-standing-OCV1 test-aging-OCV2 test-resistance matching-warehousing in sequence, wherein, in the several processes from battery cell matching to sealing, the ambient dew point temperature is less than -35°C, and the other processes can be controlled according to the conventional battery production process. Figure 1: is a battery cycle curve diagram of the power battery prepared in this embodiment. Figure 1 It can be seen that the power battery prepared in the embodiment of the present application has good cycle performance.
[0072] Example 2
[0073] A method for preparing a power battery comprises the following steps:
[0074] S01, uniformly extruding the positive electrode mixture onto both sides of the first current collector to obtain a positive electrode sheet having a positive electrode material layer extruded on the side;
[0075] S02, uniformly extruding the negative electrode mixture onto both sides of the second current collector to obtain a negative electrode sheet having a negative electrode material layer extruded on the side;
[0076] S03, stacking the positive electrode sheets of step S01 and the negative electrode sheets of step S02, with the positive electrode sheets and the negative electrode sheets arranged alternately, to obtain a battery core; placing the battery core in a battery casing to obtain a power battery.
[0077] In step S01,
[0078] Taking the mass of the positive electrode mixture as 100%, the positive electrode mixture includes the following components in percentage by mass: 25% of a first carbonate solvent, 65% of a positive electrode active mixture and 10% of a first additive.
[0079] The preparation method of the positive electrode mixture comprises the following steps: 25% of a first carbonate solvent, 65% of a positive electrode active mixture and 10% of a first additive are uniformly mixed to obtain a positive electrode mixture; the solid content of the positive electrode mixture is 75%.
[0080] The mixing is achieved by a double planetary vacuum mixer, comprising the following steps: stirring at 20 Hz for 10 min, and then stirring at 850 rpm and 45 Hz for 2 h.
[0081] Based on 100% of the mass of the positive electrode active mixture, the positive electrode active mixture includes the following components in mass percentage: 3% of a first binder, 81% of a first metal compound, 10% of a first conductive agent, and 6% of a first electrolyte.
[0082] The preparation method of the positive electrode active mixture comprises the following steps: 3% of a first binder, 81% of a first metal compound, 10% of a first conductive agent and 6% of a first electrolyte are uniformly mixed to obtain a positive electrode active mixture.
[0083] The mixing is achieved by a double planetary vacuum mixer, comprising the following steps: stirring at a rotation speed of 450 rpm and a revolution speed of 10 Hz for 10 min, and then stirring at a rotation speed of 1050 rpm and a revolution speed of 35 Hz for 1 h.
[0084] The first binder is PTFE; the first metal compound is lithium nickel cobalt manganese oxide; the first conductive agent is carbon nanotubes; and the first electrolyte is lithium bis(fluorosulfonyl)imide.
[0085] The first carbonate solvent is ethyl methyl carbonate; and the first additive is lithium aluminum titanium phosphate.
[0086] The positive electrode material layer is a semi-solid material layer; the thickness of the positive electrode material layer is 1 mm; and the first current collector is an aluminum foil current collector.
[0087] In step S02,
[0088] Taking the mass of the negative electrode mixture as 100%, the negative electrode mixture includes the following components in percentage by mass: 20% of a second carbonate solvent, 75% of a negative electrode active mixture and 5% of a second additive.
[0089] The method for preparing the negative electrode mixture comprises the following steps: uniformly mixing 20% of a second carbonate solvent, 75% of a negative electrode active mixture and 5% of a second additive to obtain a negative electrode mixture.
[0090] The mixing is achieved by a double planetary vacuum mixer, comprising the following steps: stirring at a rotation of 1850 rpm and a revolution of 35 Hz for 1 hour, and then stirring at a rotation of 1550 rpm and a revolution of 45 Hz for 2 hours.
[0091] Based on 100% of the mass of the negative electrode active mixture, the negative electrode active mixture includes the following components in mass percentage: 0.1% of a second binder, 96.9% of a second metal compound, 1% of a second conductive agent, and 2% of a second electrolyte.
[0092] The method for preparing the negative electrode active mixture comprises the following steps: uniformly mixing 0.1% of a second binder, 96.9% of a second metal compound, 1% of a second conductive agent and 2% of a second electrolyte to obtain a negative electrode active mixture.
[0093] The mixing is achieved by a double planetary vacuum mixer, comprising the following steps: stirring at a rotation of 450 rpm and a revolution of 20 Hz for 10 min, and then stirring at a rotation of 1850 rpm and a revolution of 45 Hz for 1.5 h.
[0094] The second binder is PEO; the second metal compound is soft carbon; and the second electrolyte is lithium hexafluorophosphate.
[0095] The second carbonate solvent is diethyl carbonate; and the second additive is lithium lanthanum titanate.
[0096] The negative electrode material layer is a semi-solid material layer; the thickness of the negative electrode material layer is 1 mm; and the second current collector is a copper foil current collector.
[0097] In step S03,
[0098] A diaphragm is arranged between the positive electrode sheet and the negative electrode sheet; and the battery core is a lithium battery core.
[0099] Example 3
[0100] A method for preparing a power battery comprises the following steps:
[0101] S01, uniformly extruding the positive electrode mixture onto both sides of the first current collector to obtain a positive electrode sheet having a positive electrode material layer extruded on the side;
[0102] S02, uniformly extruding the negative electrode mixture onto both sides of the second current collector to obtain a negative electrode sheet having a negative electrode material layer extruded on the side;
[0103] S03, stacking the positive electrode sheets of step S01 and the negative electrode sheets of step S02, with the positive electrode sheets and the negative electrode sheets arranged alternately, to obtain a battery core; placing the battery core in a battery casing to obtain a power battery.
[0104] In step S01,
[0105] Taking the mass of the positive electrode mixture as 100%, the positive electrode mixture includes the following components in percentage by mass: 22% of a first carbonate solvent, 70% of a positive electrode active mixture and 8% of a first additive.
[0106] The preparation method of the positive electrode mixture comprises the following steps: 22% of a first carbonate solvent, 70% of a positive electrode active mixture and 8% of a first additive are uniformly mixed to obtain a positive electrode mixture; the solid content of the positive electrode mixture is 78%.
[0107] The mixing is achieved by a double planetary vacuum mixer, comprising the following steps: stirring at 20 Hz for 10 min, and then stirring at 850 rpm and 45 Hz for 2 h.
[0108] Based on 100% of the mass of the positive electrode active mixture, the positive electrode active mixture includes the following components in mass percentage: 2% of a first binder, 90% of a first metal compound, 4% of a first conductive agent, and 4% of a first electrolyte.
[0109] The preparation method of the positive electrode active mixture comprises the following steps: 2% of a first binder, 90% of a first metal compound, 4% of a first conductive agent and 4% of a first electrolyte are uniformly mixed to obtain a positive electrode active mixture.
[0110] The mixing is achieved by a double planetary vacuum mixer, comprising the following steps: stirring at a rotation speed of 450 rpm and a revolution speed of 15 Hz for 10 min, and then stirring at a rotation speed of 1050 rpm and a revolution speed of 40 Hz for 1 h.
[0111] The first binder is PTFE; the first metal compound is sodium phosphate; the first conductive agent is conductive graphite; and the first electrolyte is sodium hexafluorophosphate.
[0112] The first carbonate solvent is ethylene carbonate; the first additive is lithium lanthanum titanate.
[0113] The positive electrode material layer is a semi-solid material layer; the thickness of the positive electrode material layer is 0.010 mm; and the first current collector is an aluminum foil current collector.
[0114] In step S02,
[0115] Taking the mass of the negative electrode mixture as 100%, the negative electrode mixture includes the following components in percentage by mass: 23% of a second carbonate solvent, 71% of a negative electrode active mixture and 6% of a second additive.
[0116] The method for preparing the negative electrode mixture comprises the following steps: 23% of a second carbonate solvent, 71% of a negative electrode active mixture and 6% of a second additive are uniformly mixed to obtain a negative electrode mixture.
[0117] The mixing is achieved by a double planetary vacuum mixer, comprising the following steps: stirring at a rotation of 1800 rpm and a revolution of 40 Hz for 1 hour, and then stirring at a rotation of 1550 rpm and a revolution of 40 Hz for 2 hours.
[0118] Based on 100% of the mass of the negative electrode active mixture, the negative electrode active mixture includes the following components in mass percentage: 1% of a second binder, 92% of a second metal compound, 3% of a second conductive agent, and 4% of a second electrolyte.
[0119] The method for preparing the negative electrode active mixture comprises the following steps: uniformly mixing 1% of a second binder, 92% of a second metal compound, 3% of a second conductive agent and 4% of a second electrolyte to obtain a negative electrode active mixture.
[0120] The mixing is achieved by a double planetary vacuum mixer, comprising the following steps: stirring at a rotation of 550 rpm and a revolution of 15 Hz for 10 min, and then stirring at a rotation of 1800 rpm and a revolution of 40 Hz for 1.5 h.
[0121] The second binder is PEO; the second metal compound is soft carbon; and the second electrolyte is sodium hexafluorophosphate.
[0122] The second carbonate solvent is diethyl carbonate; and the second additive is lithium lanthanum titanate.
[0123] The negative electrode material layer is a semi-solid material layer; the thickness of the negative electrode material layer is 0.010 mm; and the second current collector is a copper foil current collector.
[0124] In step S03,
[0125] A diaphragm is arranged between the positive electrode sheet and the negative electrode sheet; and the battery core is a sodium battery core.
[0126] In the description of this specification, the description with reference to the terms "an embodiment", "example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example.
[0127] In addition, it should be understood that although this specification is described according to implementation methods, not every implementation method contains only one independent technical solution. This narrative method of the specification is only for the sake of clarity. Those skilled in the art should regard the specification as a whole. The technical solutions in each embodiment may also be appropriately combined to form other implementation methods that can be understood by those skilled in the art.
[0128] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for preparing a power battery, characterized in that: The steps include: S01, uniformly extruding the positive electrode mixture onto both sides of the first current collector to obtain a positive electrode sheet having a positive electrode material layer extruded on the side; S02, uniformly extruding the negative electrode mixture onto both sides of the second current collector to obtain a negative electrode sheet having a negative electrode material layer extruded on the side; S03, stacking the positive electrode sheets of step S01 and the negative electrode sheets of step S02, with the positive electrode sheets and the negative electrode sheets arranged alternately, to obtain a battery core; placing the battery core in a battery casing to obtain a power battery.
2. The method for preparing a power battery according to claim 1, characterized in that: In step S01, taking the mass of the positive electrode mixture as 100%, the positive electrode mixture includes the following components in percentage by mass: 20% to 25% of a first carbonate solvent, 65% to 75% of a positive electrode active mixture and 5% to 10% of a first additive.
3. The method for preparing a power battery according to claim 2, characterized in that: Taking the mass of the positive electrode active mixture as 100%, the positive electrode active mixture includes the following components in mass percentage: 0.1% to 3% of a first binder, 81% to 96.9% of a first metal compound, 1% to 10% of a first conductive agent, and 2% to 6% of a first electrolyte.
4. The method for preparing a power battery according to claim 3, characterized in that: The first binder is a fiber binder, one of PEO or PTFE, or a mixture of at least two of them; the first metal compound is at least one of lithium iron phosphate, lithium manganese oxide, lithium nickel cobalt manganese oxide, or a sodium-containing compound; the first conductive agent is one of carbon black, graphene, carbon nanotubes, and conductive graphite, or a mixture of at least two of them; the first electrolyte is lithium hexafluorophosphate, lithium bis(fluorosulfonyl)imide, or sodium hexafluorophosphate.
5. The method for preparing a power battery according to claim 2, characterized in that: The first carbonate solvent is at least one of ethylene carbonate, dimethyl carbonate, diethyl carbonate or ethyl methyl carbonate; the first additive is lithium lanthanum zirconium oxide, lithium aluminum titanium phosphate or lithium lanthanum titanium oxide; The positive electrode material layer is a semi-solid material layer; the thickness of the positive electrode material layer is 0.010 mm to 2 mm; and the first current collector is an aluminum foil current collector.
6. The method for preparing a power battery according to claim 1, characterized in that: In step S02, taking the mass of the negative electrode mixture as 100%, the negative electrode mixture includes the following components in percentage by mass: 20% to 25% of a second carbonate solvent, 65% to 75% of a negative electrode active mixture and 5% to 10% of a second additive.
7. The method for preparing a power battery according to claim 6, characterized in that: Taking the mass of the negative electrode active mixture as 100%, the negative electrode active mixture includes the following components in mass percentage: 0.1% to 3% of a second binder, 86% to 96.9% of a second metal compound, 1% to 5% of a second conductive agent and 2% to 6% of a second electrolyte.
8. The method for preparing a power battery according to claim 7, characterized in that: The second binder is a fiber binder, PEO or PTFE; the second metal compound is at least one of lithium titanate, graphite, hard carbon, soft carbon or a silicon-based negative electrode; the second electrolyte is lithium hexafluorophosphate, lithium bis(fluorosulfonyl)imide or sodium hexafluorophosphate. The second carbonate solvent is at least one of ethylene carbonate, dimethyl carbonate, diethyl carbonate or ethyl methyl carbonate; the second additive is lithium lanthanum zirconium oxide, lithium aluminum titanium phosphate or lithium lanthanum titanium oxide; The negative electrode material layer is a semi-solid material layer; the thickness of the negative electrode material layer is 0.010 mm to 2 mm; the second current collector is an aluminum foil current collector or a copper foil current collector.
9. The method for preparing a power battery according to claim 1, characterized in that: In step S03, a separator is provided between the positive electrode sheet and the negative electrode sheet; The battery core is a lithium battery core or a sodium battery core.
10. A power battery, characterized in that: The power battery is prepared by the preparation method according to any one of claims 1 to 9.