All-solid-state battery with reduced interface resistance
By adopting a multi-layer solid electrolyte layer structure in an all-solid-state battery, utilizing the particle size difference between the first solid electrolyte and the second solid electrolyte, combined with a binder, the problems of high interlayer interface resistance and poor water stability are solved, achieving Improved battery performance and safety.
Patent Information
- Application Number
- CN202311113234.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2023-04-06
- Filing Date
- 2023-08-31
- Publication Date
- 2024-10-15
AI Technical Summary
The problems of high interlayer interface resistance and poor water stability in all-solid-state batteries lead to battery performance degradation and safety risks.
A multi-layer solid electrolyte layer composed of a first solid electrolyte and a second solid electrolyte is used. The first solid electrolyte has a larger average particle size in the core layer part, and the second solid electrolyte has a smaller average particle size in the surface layer part. Combined with Binder to improve water stability and reduce interfacial resistance.
The interface resistance of the all-solid-state battery is reduced and the water stability is improved, which extends the battery life and improves the performance, ensuring the safety of the battery.
Smart Images

Figure CN118782887A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to an all-solid-state battery with reduced interface resistance. Background Art
[0002] As environmental issues such as climate change emerge, the proportion of electric vehicles equipped with lithium-ion batteries using liquid electrolytes is increasing. However, batteries using liquid electrolytes have the risk of fire and explosion, so all-solid-state batteries including solid electrolytes to replace liquid electrolytes are being actively developed.
[0003] All-solid-state batteries include a positive electrode (cathode), a solid electrolyte layer and a negative electrode (anode). Since each component of an all-solid-state battery is solid, many factors need to be considered, such as the resistance of the interface between the layers, the lithium ion conductivity of the solid electrolyte layer, the water stability in the process, the flexibility of the solid electrolyte layer, etc. Summary of the invention
[0004] An object of the present invention is to provide an all-solid-state battery in which the interface resistance between layers is reduced.
[0005] Another object of the present invention is to provide an all-solid-state battery with excellent water stability.
[0006] The purpose of the present invention is not limited to the foregoing content. Through the following description, the purpose of the present invention will be clearly understood and achieved by the means described in the attached claims and their combinations.
[0007] An embodiment of the present invention provides an all-solid-state battery, which includes a positive electrode layer containing a positive electrode active material, a negative electrode layer containing a negative electrode active material, and a solid electrolyte layer between the positive electrode layer and the negative electrode layer, wherein the solid electrolyte layer may include a core part (core part) containing a first solid electrolyte and a surface layer part arranged on at least one side of the core part and containing a second solid electrolyte, and the average particle size (D50) of the first solid electrolyte may be greater than the average particle size (D50) of the second solid electrolyte.
[0008] The thickness of the core portion may be 10 μm to 50 μm.
[0009] The first solid electrolyte may include at least one selected from an oxide-based solid electrolyte, a sulfide-based solid electrolyte, and a combination thereof.
[0010] The first solid electrolyte may include at least one selected from the group consisting of a crystalline solid electrolyte, an amorphous solid electrolyte, and a combination thereof.
[0011] The average particle size (D50) of the first solid electrolyte may be 2 μm to 5 μm.
[0012] The thickness of the surface layer portion may be 0.5 μm to 2 μm.
[0013] The average particle size (D50) of the second solid electrolyte may be 0.1 μm to 1 μm.
[0014] The second solid electrolyte may include at least one selected from an oxide-based solid electrolyte, a sulfide-based solid electrolyte, and a combination thereof.
[0015] The second solid electrolyte may include at least one selected from the group consisting of a crystalline solid electrolyte, an amorphous solid electrolyte, and a combination thereof.
[0016] The solid electrolyte layer may further include a binder.
[0017] The binder may include at least one selected from the group consisting of butadiene rubber, nitrile rubber, hydrogenated nitrile rubber, polyvinylidene fluoride, polytetrafluoroethylene, and combinations thereof.
[0018] The positive electrode layer may include a first interface portion which is a region ranging from a main surface in contact with the solid electrolyte layer to a predetermined depth in a thickness direction, and the first interface portion may include a positive electrode active material having an average particle size (D50) of about 5 μm to 20 μm.
[0019] The first interface portion may have a thickness of about 10 μm to 30 μm.
[0020] The negative electrode layer may include a second interface portion which is a region ranging from a main surface in contact with the solid electrolyte layer to a predetermined depth in a thickness direction, and the second interface portion may include a negative electrode active material having an average particle size (D50) of about 5 μm to 20 μm.
[0021] The second interface portion may have a thickness of about 10 μm to 30 μm. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] The above and other features of the present invention will now be described in detail with reference to certain exemplary embodiments of the invention shown in the accompanying drawings, which are given hereinafter only as examples and therefore do not limit the present invention, in which:
[0023] Figure 1 An example all-solid-state battery according to the present invention is shown;
[0024] Figure 2 An example solid electrolyte layer according to the present invention is shown;
[0025] Figure 3An example positive electrode layer according to the present invention is shown;
[0026] Figure 4 An example negative electrode layer according to the present invention is shown. DETAILED DESCRIPTION
[0027] The above and other purposes, features and advantages of the present invention will be more clearly understood from the preferred embodiments below in conjunction with the accompanying drawings. However, the present invention is not limited to the embodiments disclosed herein and can be modified into different forms. These embodiments are provided to thoroughly explain the present invention and fully convey the spirit of the present invention to those skilled in the art.
[0028] In all the accompanying drawings, the same reference numerals will refer to the same or similar elements. In order to make the present invention clearer, the size of the structure is depicted as being larger than its actual size. It should be understood that although various elements may be described herein using terms such as "first", "second", etc., these elements are not limited by these terms. These terms are only used to distinguish one element from another element. For example, the "first" element discussed below may be referred to as the "second" element without departing from the scope of the present invention. Similarly, the "second" element may also be referred to as the "first" element. As used herein, unless the context clearly states otherwise, the singular form is also intended to include the plural form.
[0029] Unless otherwise indicated, all numbers, values and / or expressions expressing the amounts of components, reaction conditions, polymer compositions and mixtures used herein are considered to be approximate, including the various uncertainties that necessarily affect the measurements in obtaining these values, and therefore should be understood to be modified in all cases by the term "about". In addition, unless otherwise indicated, when a numerical range is disclosed in this specification, the range is continuous and includes all values from the minimum value to the maximum value of the range. In addition, unless otherwise indicated, when such a range pertains to integer values, all integers from the minimum value to the maximum value are included.
[0030] Figure 1 An all-solid-state battery 100 according to an embodiment of the present invention is shown. The all-solid-state battery 100 may include a solid electrolyte layer 10, a positive electrode layer 20 disposed on one surface of the solid electrolyte layer 10, and a negative electrode layer 30 disposed on a surface opposite to the solid electrolyte layer 10.
[0031] Figure 2 A solid electrolyte layer 10 according to an embodiment of the present invention is shown. The solid electrolyte layer 10 includes a core layer portion 11 containing a first solid electrolyte 13, and a surface layer portion 12 provided on at least one surface of the core layer portion 11 and containing a second solid electrolyte 14.
[0032] The solid electrolyte layer of a typical all-solid-state battery is usually composed of only one solid electrolyte. That is to say, the solid electrolytes constituting the solid electrolyte layer usually have the same particle size, composition, etc. Therefore, if a solid electrolyte with a small average particle size (D50) and a large specific surface area is used, the area in contact with the electrode layer may increase, thereby reducing the interface resistance. However, when the solid electrolyte layer is manufactured in an environment where water is not completely removed, such as a dry room, many side reactions may occur with water due to the large specific surface area of the solid electrolyte, thereby deteriorating the battery performance. On the other hand, if a solid electrolyte with a large average particle size (D50) and a small specific surface area is used, the stability to water can be improved, but when the battery is rolled, due to the size difference with the electrode active material, a void may be formed between the solid electrolyte layer and the electrode layer, resulting in problems such as poor contact and increased interface resistance.
[0033] In the present invention, the first solid electrolyte 13 contained in the core layer portion 11 has a relatively large average particle size (D50), and the second solid electrolyte 14 contained in the surface layer portion 12 in contact with the positive electrode layer 20 and / or the negative electrode layer 30 has a relatively small average particle size (D50), thereby increasing the water stability of the solid electrolyte layer 10 and reducing the interface resistance between the solid electrolyte layer 10 and the positive electrode layer 20 and / or the negative electrode layer 30.
[0034] In the core layer portion 11, the first solid electrolyte 13 may exist in the form of particles, or the particles may exist in a dense form at a predetermined pressure. When the particles exist in a dense form, there may be an interface between the particles. When the first solid electrolyte 13 exists in the form of particles, the average particle size (D50) of the first solid electrolyte 13 may be a physical property of the particles. When the first solid electrolyte 13 exists in a dense form, the average particle size (D50) of the first solid electrolyte 13 may be a physical property of any one region of the particle form separated from other regions by an interface.
[0035] The average particle size (D50) of the first solid electrolyte 13 may be about 2 μm to 5 μm, or about 3 μm to 4 μm. If the average particle size (D50) of the first solid electrolyte 13 is less than 2 μm, the specific surface area may increase, and thus the water stability of the solid electrolyte layer 10 may deteriorate. The average particle size (D50) of the first solid electrolyte 13 may be a volume-converted median diameter measured using a laser-type particle size distribution analyzer.
[0036] The first solid electrolyte 13 may include at least one selected from an oxide-based solid electrolyte, a sulfide-based solid electrolyte, and a combination thereof. In addition, the first solid electrolyte 13 may be a crystalline solid electrolyte, an amorphous solid electrolyte, or a mixture thereof.
[0037] Examples of oxide-based solid electrolytes may include perovskite-type LLTO (Li 3x La 2 / 3-x TiO 3 ), phosphate-based NASICON-type LATP (Li 1+x Al x Ti 2-x (PO 4 ) 3 )wait.
[0038] Examples of sulfide-based solid electrolytes may include Li 2 SP 2 S 5 , Li 2 SP 2 S 5 -LiI, Li 2 SP 2 S 5 -LiCl, Li 2 SP 2 S 5 -LiBr, Li 2 SP 2 S 5 -Li 2 O. Li 2 SP 2 S 5 -Li 2 O-LiI、Li 2 S-SiS 2 , Li 2 S-SiS 2 -LiI, Li 2 S-SiS2 -LiBr, Li 2 S - SiS 2 -LiCl, Li 2 S - SiS 2 -B 2 S 3 -LiI, Li 2 S - SiS 2 -P 2 S 5 -LiI, Li 2 S - B 2 S 3 , Li 2 S - P 2 S 5 -Z m S n (where m and n are positive numbers, and Z is any one selected from Ge, Zn, and Ga), Li 2 S - GeS 2 , Li 2 S - SiS 2 -Li 3 PO 4 , Li 2 S - SiS 2 -Li x MO y (where x and y are positive numbers, and M is any one selected from P, Si, Ge, B, Al, Ga, and In) Li 10 GeP 2 S 12 etc.
[0039] In some embodiments, the first solid electrolyte 13 may include a sulfide - based solid electrolyte having an argyrodite crystal structure. The sulfide - based solid electrolyte having an argyrodite crystal structure may include at least one selected from Li 7-x PS 6-x Cl x (0 < x ≤ 2), Li 7-x PS 6-x Br x (0 < x ≤ 2), Li 7-x PS 6-x I x (0 < x ≤ 2) and combinations thereof.
[0040] In the surface layer portion 12, the second solid electrolyte 14 may exist in the form of particles, or the particles may exist in a dense form at a predetermined pressure. When the particles exist in a dense form, there may be an interface between the particles. When the second solid electrolyte 14 exists in the form of particles, the average particle size (D50) of the second solid electrolyte 14 may be a physical property of the particles. When the second solid electrolyte 14 exists in a dense form, the average particle size (D50) of the second solid electrolyte 14 may be a physical property of any region of the form of particles separated from other regions by an interface.
[0041] The average particle size (D50) of the second solid electrolyte 14 may be about 20% or less of the average particle size (D50) of the first solid electrolyte 13. Specifically, the average particle size (D50) of the second solid electrolyte 14 may be about 0.1 μm to 1 μm. If the average particle size (D50) of the second solid electrolyte 14 exceeds 1 μm, the interface contact between the surface layer portion 12 and the positive electrode layer 20 and / or the negative electrode layer 30 may deteriorate. The average particle size (D50) of the second solid electrolyte 14 may be a volume-converted median diameter measured using a laser-type particle size distribution analyzer.
[0042] The second solid electrolyte 14 may include at least one selected from an oxide-based solid electrolyte, a sulfide-based solid electrolyte, and a combination thereof. In addition, the second solid electrolyte 14 may be a crystalline solid electrolyte, an amorphous solid electrolyte, or a mixture thereof. The second solid electrolyte 14 may have a composition or crystallinity that is the same as or different from that of the first solid electrolyte 13.
[0043] Examples of oxide-based solid electrolytes may include perovskite-type LLTO (Li 3x La 2 / 3-x TiO 3 ), phosphate-based NASICON-type LATP (Li 1+x Al x Ti 2-x (PO 4 ) 3 )wait.
[0044] Examples of sulfide-based solid electrolytes may include Li 2 SP 2 S 5 , Li 2 SP 2 S 5 -LiI, Li 2 SP 2 S 5 -LiCl, Li 2 SP 2 S 5-LiBr, Li 2 SP 2 S 5 -Li 2 O. Li 2 SP 2 S 5 -Li 2 O-LiI、Li 2 S-SiS 2 , Li 2 S-SiS 2 -LiI, Li 2 S-SiS 2 -LiBr, Li 2 S-SiS 2 -LiCl, Li 2 S-SiS 2 -B 2 S 3 -LiI, Li 2 S-SiS 2 -P 2 S 5 -LiI, Li 2 SB 2 S 3 , Li 2 SP 2 S 5 -Z m S n (wherein m and n are positive numbers, and Z is any one selected from Ge, Zn and Ga), Li 2 S-GeS 2 , Li 2 S-SiS 2 -Li 3 PO 4 , Li 2 S-SiS 2 -Li x MO y (wherein x and y are positive numbers and M is any one selected from P, Si, Ge, B, Al, Ga and In), Li 10 G 2 S 12 wait.
[0045] In some embodiments, the second solid electrolyte 14 includes a sulfide-based solid electrolyte having an argyrodite crystal structure. The sulfide-based solid electrolyte having an argyrodite crystal structure may include a material selected from Li 7-x PS 6-x Cl x (0 <x≤2)、Li 7-x PS 6-x Brx (0 < x ≤ 2), Li 7-x PS 6-x I x At least one of (0 < x ≤ 2) and combinations thereof.
[0046] The thickness of the core layer portion 11 can be about 10 μm to 50 μm. If the thickness of the core layer portion 11 is less than 10 μm, the durability of the all-solid-state battery 100 will deteriorate, and if it exceeds 50 μm, the energy density per unit volume of the all-solid-state battery 100 will decrease.
[0047] The thickness of the surface layer portion 12 can be about 0.5 μm to 2 μm. If the thickness of the surface layer portion 12 is less than 0.5 μm, the interfacial contact between the solid electrolyte layer 10 and the positive electrode layer 20 and / or the negative electrode layer 30 may be poor, and if it exceeds 2 μm, the water stability of the solid electrolyte layer 10 may deteriorate.
[0048] The solid electrolyte layer 10 may further include a binder. The binder may include at least one selected from butadiene rubber, nitrile rubber, hydrogenated nitrile rubber, polyvinylidene fluoride, polytetrafluoroethylene, and combinations thereof.
[0049] The method for manufacturing the solid electrolyte layer 10 is not particularly limited. For example, the method may include manufacturing the core layer portion 11 and manufacturing the surface layer portion 12 on at least one surface of the core layer portion 11.
[0050] Manufacturing the core layer portion 11 may include preparing a slurry including a first solid electrolyte 13, a binder, and a solvent, coating the slurry onto a substrate, and drying the slurry.
[0051] Here, any suitable solvent may be included as long as it does not react with the first solid electrolyte 13. Examples of the solvent may include non-polar organic solvents, aprotic organic solvents, etc. Specifically, the solvent may include at least one selected from toluene, chloroform, ethyl acetate, 1,2-dimethoxyethane, tetrahydrofuran (THF), dichloromethane, pyridine, 2-butanone, acetone, N-methylpyrrolidone, acetonitrile, sulfolane, dimethyl sulfoxide, carbon tetrachloride, hexane, heptane, pentane, decalin, dioxane, and combinations thereof.
[0052] Manufacturing the surface layer portion 12 may include preparing a slurry including the second solid electrolyte 14, a binder, and a solvent, applying the slurry to at least one surface of the core layer portion 11, and drying the slurry. However, manufacturing the surface layer portion 12 is not limited to applying the slurry directly to the core layer portion 11, and the surface layer portion 12 obtained by applying the slurry to a release paper and then drying it may be transferred to the core layer portion 11.
[0053] In other embodiments, the method of manufacturing solid electrolyte layer 10 is not limited to the above-mentioned wet method, and may be performed by a dry method without using a solvent.
[0054] The positive electrode layer 20 may include a positive electrode active material, a solid electrolyte, a conductive material, a binder, a dispersant, and the like.
[0055] Figure 3 The positive electrode layer 20 is shown. The positive electrode layer 20 may include a first interface portion 21, which is a region ranging from a main surface A in contact with the solid electrolyte layer 10 to a predetermined depth in the thickness direction. The thickness T of the first interface portion 21 is 1 It may be about 10 μm to 30 μm.
[0056] In the present invention, the average particle size (D50) of the positive electrode active material contained in the first interface portion 21 in contact with the surface layer portion 12 is not greatly adjusted compared with the second solid electrolyte 14, so that the interface between the solid electrolyte layer 10 and the positive electrode layer 20 can be well formed.
[0057] The average particle size (D50) of the positive electrode active material contained in the first interface portion 21 may be about 5 μm to 20 μm, or about 7 μm to 15 μm. If the average particle size (D50) of the positive electrode active material exceeds 20 μm, voids may be formed at the interface between the solid electrolyte layer 10 and the positive electrode layer 20, resulting in poor contact.
[0058] The positive electrode active material is capable of occluding and releasing lithium ions.
[0059] The positive electrode active material may include a rock-salt-layer-type active material, such as LiCoO 2 、LiMnO 2 、LiNiO 2 、LiVO 2 , Li 1+x Ni 1 / 3 Co 1 / 3 Mn 1 / 3 O 2 etc.; spinel-type active materials, such as LiMn2 O 4 , Li(Ni 0.5 Mn 1.5 )O 4 etc.; inverse-spinel-type active materials, such as LiNiVO 4 , LiCoVO 4 etc.; olivine-type active materials, such as LiFePO 4 , LiMnPO 4 , LiCoPO 4 , LiNiPO 4 etc.; silicon-containing active materials, such as Li 2 FeSiO 4 , Li 2 MnSiO 4 etc.; rock-salt-layer-type active materials in which part of the transition metals are replaced by different metals, such as LiNi 0.8 Co (0.2-x) Al x O 2 (0 < x < 0.2); spinel-type active materials in which part of the transition metals are replaced by different metals, such as Li 1+x Mn 2-x-y M y O 4 (M is at least one selected from Al, Mg, Co, Fe, Ni, and Zn, 0 < x + y < 2); lithium titanate, such as Li 4 Ti 5 O 12 etc.
[0060] The negative electrode layer 30 may include a negative electrode active material, a solid electrolyte, a conductive material, a binder, a dispersant, etc.
[0061] Figure 4 The negative electrode layer 30 is shown. The negative electrode layer 30 may include a second interface portion 31, which is a region ranging from the main surface B in contact with the solid electrolyte layer 10 to a predetermined depth in the thickness direction. The thickness T2 of the second interface portion 31 may be about 10 μm to 30 μm.
[0062] In the present invention, the average particle diameter (D50) of the negative electrode active material contained in the second interface portion 31 in contact with the surface layer portion 12 is not greatly adjusted compared with the second solid electrolyte 14, so that the interface between the solid electrolyte layer 10 and the negative electrode layer 30 can be well formed.
[0063] The average particle diameter (D50) of the negative electrode active material included in the second interface portion 31 may be about 5 μm to 20 μm, or about 7 μm to 15 μm. If the average particle diameter (D50) of the negative electrode active material exceeds 20 μm, voids may be formed at the interface between the solid electrolyte layer 10 and the negative electrode layer 30, resulting in poor contact.
[0064] The negative electrode active material may include at least one selected from carbon-based active materials, silicon-based active materials, and combinations thereof.
[0065] The carbon-based active material may include natural graphite, artificial graphite, and the like.
[0066] The silicon-based active material may include Si, SiO x (0 < x < 2), etc.
[0067] The present invention can be better understood through the following examples. These examples are merely for illustrating the present invention and should not be construed as limiting the scope of the present invention. Examples
[0068] As the first solid electrolyte, a sulfide-based solid electrolyte having an average particle diameter (D50) of 3 μm to 4 μm, a thiargillite crystal structure, and represented by Li 6 PS 5 Cl was prepared.
[0069] As the second solid electrolyte, a sulfide-based solid electrolyte having an average particle diameter (D50) of less than 1 μm, a thiargillite crystal structure, and represented by Li 6 PS 5 Cl was prepared.
[0070] The core layer portion was manufactured by coating a first slurry including the first solid electrolyte, a binder, and a solvent onto a substrate and then drying. The binder used was butadiene rubber.
[0071] The surface layer portion was manufactured by coating a second slurry including the second solid electrolyte, a binder, and a solvent onto each of both sides of the core layer portion and then drying.
[0072] The solid electrolyte layer was obtained by pressing the laminate manufactured above. The thickness of the core layer portion was about 10 μm, and the thickness of the surface layer portion was about 0.5 μm to 2 μm.
[0073] The all-solid-state battery was manufactured by stacking a positive electrode layer including a positive electrode active material on one side of the solid electrolyte layer and stacking a negative electrode layer including a negative electrode active material on the remaining side thereof.
[0074] Comparative Example 1
[0075] As a solid electrolyte, a argyrodite crystal structure having an average particle size (D50) of less than 1 μm and composed of Li 6 PS 5 Sulfide-based solid electrolyte represented by Cl.
[0076] The solid electrolyte layer was produced by applying a slurry containing a solid electrolyte, a binder and a solvent onto a substrate, followed by drying and rolling. The thickness of the solid electrolyte layer was adjusted to be the same as that of the solid electrolyte layer of Example 1.
[0077] An all-solid-state battery was manufactured by stacking the same positive electrode layer and negative electrode layer as in Example 1 on the respective sides of the solid electrolyte layer.
[0078] Comparative Example 2
[0079] As a solid electrolyte, a argyrodite crystal structure having an average particle size (D50) of 3 μm to 4 μm and composed of Li 6 PS 5 Sulfide-based solid electrolyte represented by Cl.
[0080] The solid electrolyte layer was produced by applying a slurry containing a solid electrolyte, a binder and a solvent onto a substrate, followed by drying and rolling. The thickness of the solid electrolyte layer was adjusted to be the same as that of the solid electrolyte layer of Example 1.
[0081] An all-solid-state battery was manufactured by stacking the same positive electrode layer and negative electrode layer as in Example 1 on the respective sides of the solid electrolyte layer.
[0082] The all-solid-state batteries according to Example 1, Comparative Example 1 and Comparative Example 2 were analyzed by electrochemical impedance spectroscopy, and the charge transfer resistance of each all-solid-state battery was measured. The results are shown in Table 1 below.
[0083] [Table 1] item Example 1 Comparative Example 1 Comparative Example 2 <![CDATA[Charge transfer resistance (R ct )]]> 2.8Ω 3.2Ω 2.5Ω
[0084] Example 1 including a core layer portion and a surface layer portion shows low charge transfer resistance compared to Comparative Example 1 using only a solid electrolyte having a small average particle size (D50). Thus, it can be found that the core layer portion of Example 1 includes a solid electrolyte having a large average particle size (D50), and therefore has high water stability, so that the battery performance is not deteriorated during the manufacturing process.
[0085] Comparative Example 3
[0086] A solid electrolyte layer and an all-solid-state battery including the solid electrolyte layer were manufactured in the same manner as in Example 1, except that the thickness of the surface layer portion was adjusted to less than 0.5 μm.
[0087] Comparative Example 4
[0088] A solid electrolyte layer and an all-solid-state battery including the solid electrolyte layer were manufactured in the same manner as in Example 1, except that the thickness of the surface layer portion was adjusted to be greater than 2 μm.
[0089] Comparative Example 5
[0090] A solid electrolyte layer and an all-solid-state battery including the solid electrolyte layer were manufactured in the same manner as in Example 1, except that a first solid electrolyte having an average particle size (D50) of less than 3 μm was used.
[0091] Comparative Example 6
[0092] A solid electrolyte layer and an all-solid-state battery including the solid electrolyte layer were manufactured in the same manner as in Example 1, except that a first solid electrolyte having an average particle size (D50) of more than 4 μm was used.
[0093] When the all-solid-state batteries according to Example 1 and Comparative Examples 2 to 6 were charged and discharged for 30 cycles, the capacity retention rate was measured. The results are shown in Table 2 below.
[0094] [Table 2]
[0095] According to the present invention, Example 1, which satisfies the thickness of the surface layer portion and the average particle size (D50) of the first solid electrolyte constituting the core layer portion, shows a capacity retention rate of about 90%. In contrast, Comparative Example 2, in which the surface layer portion is not formed, exhibits a very low capacity retention rate of 65%. This is attributed to the fact that the interface is not well formed between the solid electrolyte layer and the electrode layer in Comparative Example 2. In Comparative Example 3, the thickness of the surface layer portion is less than the thickness of the surface layer portion of Example 1, so that the interface resistance between the solid electrolyte layer and the electrode layer is not reduced, and the measured capacity retention rate is low. In Comparative Example 4, the thickness of the surface layer portion is greater than the thickness of the surface layer portion of Example 1, so the core layer portion is relatively thin, resulting in poor water stability, and thus determining that the capacity retention rate is low. In Comparative Example 5, since a first solid electrolyte having a small average particle size (D50) is used, water stability becomes a problem, resulting in a low capacity retention rate. In Comparative Example 6, the average particle size (D50) difference between the first solid electrolyte and the second solid electrolyte is large, so a gap is generated between them, resulting in a low capacity retention rate.
[0096] As is apparent from the above description, according to the present invention, an all-solid-state battery having reduced interlayer interface resistance can be obtained.
[0097] According to the present invention, an all-solid-state battery having excellent water stability can be obtained.
[0098] According to the present invention, an all-solid-state battery having a long life and excellent performance can be obtained.
[0099] The effects of the present invention are not limited to the above-mentioned effects. It should be understood that the effects of the present invention include all effects that can be inferred from the description of the present invention.
[0100] Although the present invention has been described in detail above, the scope of the present invention is not limited thereto, and various modifications and improvements made by those skilled in the art using the basic concept of the present invention defined in the appended claims are also included in the scope of the present invention.
Claims
1. An all-solid-state battery, include: A positive electrode layer comprising a positive electrode active material; a negative electrode layer comprising a negative electrode active material; and a solid electrolyte layer between the positive electrode layer and the negative electrode layer, The solid electrolyte layer comprises: a core portion comprising a first solid electrolyte; and a surface layer portion disposed on at least one surface of the core layer portion and comprising a second solid electrolyte; and The average particle size D50 of the first solid electrolyte is greater than the average particle size D50 of the second solid electrolyte. 2 . The all-solid-state battery according to claim 1 , wherein the thickness of the core layer portion is 10 μm to 50 μm. 3 . The all-solid-state battery according to claim 1 , wherein an average particle size D50 of the first solid electrolyte is 2 μm to 5 μm. 4 . The all-solid-state battery according to claim 1 , wherein the first solid electrolyte comprises an oxide-based solid electrolyte, a sulfide-based solid electrolyte, or a combination thereof. 5 . The all-solid-state battery according to claim 1 , wherein the first solid electrolyte comprises a crystalline solid electrolyte, an amorphous solid electrolyte, or a combination thereof. The all-solid-state battery according to claim 1 , wherein the thickness of the surface layer portion is 0.5 μm to 2 μm. 7 . The all-solid-state battery according to claim 1 , wherein an average particle size D50 of the second solid electrolyte is 0.1 μm to 1 μm. 8 . The all-solid-state battery according to claim 1 , wherein the second solid electrolyte comprises an oxide-based solid electrolyte, a sulfide-based solid electrolyte, or a combination thereof. 9 . The all-solid-state battery according to claim 1 , wherein the second solid electrolyte comprises a crystalline solid electrolyte, an amorphous solid electrolyte, or a combination thereof. 10 . The all-solid-state battery according to claim 1 , wherein the solid electrolyte layer further comprises a binder. 11 . The all-solid-state battery according to claim 10 , wherein the binder comprises butadiene rubber, nitrile rubber, hydrogenated nitrile rubber, polyvinylidene fluoride, polytetrafluoroethylene, or a combination thereof.
12. An all-solid-state battery according to claim 1, wherein the positive electrode layer includes a first interface portion, the first interface portion is a region ranging from a main surface in contact with the solid electrolyte layer to a predetermined depth along the thickness direction, and the first interface portion contains the positive electrode active material having an average particle size D50 of 5 μm to 20 μm.
13. The all-solid-state battery according to claim 12, in, The first interface portion has a thickness of 10 μm to 30 μm.
14. An all-solid-state battery according to claim 1, wherein the negative electrode layer includes a second interface portion, the second interface portion is a region ranging from a main surface in contact with the solid electrolyte layer to a predetermined depth along the thickness direction, and the second interface portion contains the negative electrode active material having an average particle size D50 of 5 μm to 20 μm.
15. The all-solid-state battery according to claim 14, in, The second interface portion has a thickness of 10 μm to 30 μm.