All-solid-state battery including negative electrode layer in form of thick film and method of manufacturing same
By introducing multiple lithiophilic layers into the negative electrode layer of all-solid-state batteries, combined with carbon-based or silicon-based active materials, the problem of uneven lithium ion migration caused by thick-film negative electrodes is solved, and the energy density and durability of the battery are improved. This ensures uniform diffusion of lithium ions and stability of the electrode interface.
Patent Information
- Application Number
- CN202311143026.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2023-04-07
- Filing Date
- 2023-09-06
- Publication Date
- 2024-10-15
AI Technical Summary
In all-solid-state batteries, the thick-film negative electrode increases the migration distance of lithium ions, making it impossible to use the entire negative electrode, and the amount of lithium charged cannot be fully absorbed, causing metal lithium to precipitate in the middle of the negative electrode, affecting the energy density and electrode interface. Poor contact.
It adopts a structure of multiple lithiophilic layers, including a first lithiophilic layer and a second lithiophilic layer, which respectively contain metals and their oxides that can be alloyed with lithium, combined with carbon-based or silicon-based active materials, and form a thickness through deposition technology. In the negative electrode layer of 70 μm to 150 μm, the second lithiophilic layer is located in the space between the first plane and the second plane, promoting the uniform diffusion of lithium ions.
It achieves uniform diffusion of lithium ions to the entire negative electrode layer, improves the energy density and durability of the battery, prevents lithium from precipitating in the negative electrode layer, and ensures the uniformity of the electrochemical reaction.
Smart Images

Figure CN118782888A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to an all-solid-state battery and a method for manufacturing the same, wherein the all-solid-state battery comprises a negative electrode layer in the form of a thick film having a plurality of lithium-philic layers. Background Art
[0002] Recently, there has been a growing demand for batteries with high energy density in various fields including electric vehicles. Therefore, there has been a demand to form the electrode as a thick film to increase the energy density. However, in an all-solid-state battery, when the electrode is formed in the form of a thick film, the migration distance of lithium ions will increase. Therefore, the entire negative electrode may not be used. In addition, the amount of lithium charged cannot be fully received, resulting in the problem of precipitation of metallic lithium in the middle of the negative electrode.
[0003] In order to overcome the above problems and simultaneously improve the energy density of all-solid-state batteries, research has been conducted to improve the lithium ion conductivity of solid electrolytes or to use negative electrode active materials having high energy density such as silicon.
[0004] However, the improvement of lithium ion conductivity may be difficult to achieve in thick film form due to the direction of ion transport and the resistance between materials. In addition, in the method of using silicon-based negative electrode active materials, there is a problem of poor contact at the electrode interface due to the volume expansion of the material during charging. Summary of the invention
[0005] In a preferred aspect, the present invention provides an all-solid-state battery having high energy density and excellent durability.
[0006] In one aspect, an all-solid-state battery is provided, comprising: a negative electrode collector; a negative electrode layer disposed on the negative electrode collector; a solid electrolyte layer disposed on the negative electrode layer; a positive electrode layer disposed on the solid electrolyte layer; and a positive electrode collector disposed on the positive electrode layer.
[0007] The negative electrode layer may include: a first lithium-philic layer, which is arranged on the negative electrode collector and contains a first metal, an oxide of the first metal, or a combination thereof that can be alloyed with lithium; a first negative electrode active material layer, which is arranged on the first lithium-philic layer and contains a first negative electrode active material; a second lithium-philic layer, which is arranged on the first negative electrode active material layer and contains a second metal, an oxide of the second metal, or a combination thereof that can be alloyed with lithium; and a second negative electrode active material layer, which is arranged on the second lithium-philic layer and contains a second negative electrode active material.
[0008] As used herein, the term "lithiophilic" refers to the property of a material having an affinity or attraction for a lithium component (such as lithium ions). In general, a lithiophilic material (particularly a lithiophilic metal) that forms an alloy or complex with lithium can be used to control the nucleation site and stabilize the Li (Li ion) deposition (such as dendrites) by adjusting the nucleation overpotential of Li. Exemplary lithiophilic materials (such as metals) can include lithium (Li), indium (In), gold (Au), silver (Ag), bismuth (Bi), zinc (Zn), aluminum (Al), iron (Fe), tin (Sn), and titanium (Ti).
[0009] Preferably, the first metal may appropriately include one or more selected from lithium (Li), indium (In), gold (Au), silver (Ag), bismuth (Bi), zinc (Zn), aluminum (Al), iron (Fe), tin (Sn) and titanium (Ti).
[0010] The first negative electrode active material may suitably include a carbon-based active material, a silicon-based active material, or a combination thereof.
[0011] Preferably, the second metal may appropriately include one or more selected from lithium (Li), indium (In), gold (Au), silver (Ag), bismuth (Bi), zinc (Zn), aluminum (Al), iron (Fe), tin (Sn) and titanium (Ti).
[0012] The second negative electrode active material may suitably include a carbon-based active material, a silicon-based active material, or a combination thereof.
[0013] The thickness of the negative electrode layer may be in the range of about 70 μm to about 150 μm.
[0014] The negative electrode layer may include a first major surface in contact with the negative electrode current collector and a second major surface in contact with the solid electrolyte layer.
[0015] The second lithium-philic layer can be located in the space between the first plane and the second plane, the first plane is spaced a certain distance from the first main surface toward the solid electrolyte layer, and the distance corresponds to about 40% of the thickness of the negative electrode layer along the thickness direction, and the second plane is spaced a certain distance from the second main surface toward the negative electrode collector, and the distance corresponds to about 40% of the thickness of the negative electrode layer along the thickness direction.
[0016] All-solid-state batteries can meet condition 1,
[0017] [Condition 1]
[0018]
[0019] where x 1 can be the thickness of the first lithiophilic layer, x 2 It may be the thickness of the second lithiophilic layer.
[0020] In one aspect, a method for manufacturing an all-solid-state battery is provided, the method comprising the following steps: forming a negative electrode layer on a negative electrode collector; forming a solid electrolyte layer on the negative electrode layer; forming a positive electrode layer on the solid electrolyte layer; and forming a positive electrode collector on the positive electrode layer.
[0021] The formation of the negative electrode layer may include: forming a first lithium-philic layer by depositing a first metal, an oxide of the first metal, or a combination thereof that can alloy with lithium on the negative electrode collector; forming a first negative electrode active material layer containing a first negative electrode active material on the first lithium-philic layer; forming a second lithium-philic layer by depositing a second metal, an oxide of the second metal, or a combination thereof that can alloy with lithium on the first negative electrode active material layer; and forming a second negative electrode active material layer containing a second negative electrode active material on the second lithium-philic layer.
[0022] When forming the first lithium-philic layer, the first metal, the oxide of the first metal, or a combination thereof may be sputtered on the negative electrode current collector.
[0023] When forming the second lithium-philic layer, the second metal, the oxide of the second metal, or a combination thereof may be sputtered on the first negative electrode active material layer.
[0024] The manufacturing method can satisfy condition 2,
[0025] [Condition 2]
[0026]
[0027] Among them, t 1 It can be the deposition time required to form the first lithium-philic layer, t 2 It may be the deposition time required to form the second lithiophilic layer.
[0028] A vehicle is also provided, comprising the all-solid-state battery described herein.
[0029] According to various exemplary embodiments of the present invention, an all-solid-state battery having high energy density and excellent durability may be obtained.
[0030] Other aspects of the invention are disclosed below. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] Figure 1 An exemplary all-solid-state battery according to an exemplary embodiment of the present invention is shown;
[0032] Figure 2 shows an exemplary negative electrode layer according to an exemplary embodiment of the present invention;
[0033] Figure 3 shows details of an exemplary negative electrode layer according to an exemplary embodiment of the present invention;
[0034] Figure 4 shows the results of analyzing a cross section of a negative electrode layer according to an exemplary embodiment of the present invention using a scanning electron microscope (SEM); and
[0035] Figure 5 Energy dispersive X-ray spectroscopy (EDS) is used to show Figure 4 Results of analysis of the same cross section of the negative electrode layer in . DETAILED DESCRIPTION
[0036] The above-mentioned purpose, other purposes, features and advantages of the present invention will be easily understood by the following preferred embodiments related to the accompanying drawings. However, the present invention is not limited to the embodiments described herein, but can be implemented in other forms. The embodiments described herein are provided so that the present invention can be thorough and complete, and the spirit of the present invention can be fully conveyed to those skilled in the art. In the entire accompanying drawings, the same elements are represented by the same reference numerals.
[0037] In the accompanying drawings, the size of the structure is larger than the actual size in order to make the present invention clear. The terms "first", "second", etc. used in the specification can be used to describe various components, but these components should not be understood as limited to these terms. These terms are only used to distinguish one component from another component. For example, a first component may be referred to as a second component, and a second component may also be referred to as a first component without departing from the scope of the present invention.
[0038] As used herein, the singular forms "a", "an", and "the / said" are intended to include the plural forms as well, unless the context clearly indicates otherwise. It will also be understood that the terms "comprise", "include", or "have" when used in this specification indicate the presence of the described features, regions, values, steps, operations, elements, and / or components, but do not exclude the presence or addition of one or more other features, regions, values, steps, operations, elements, components, and / or combinations thereof.
[0039] It will also be understood that when an element such as a layer, film, region or sheet is referred to as being "on" another element, it can be directly on the other element or intervening elements may be present between them. Similarly, when an element such as a layer, film, region or sheet is referred to as being "under" another element, it can be directly under the other element or intervening elements may be present between them.
[0040] Unless otherwise indicated, all numbers, values and / or expressions expressing quantities of components, reaction conditions, polymer compositions and mixtures used herein are to be construed as approximations containing the various uncertainties inherent in obtaining such values, particularly those that affect the measurements, and are therefore to be understood as being modified in all instances by the term "about".
[0041] Further, unless otherwise stated or apparent from the context, the term "about" as used herein is understood to be within the normal tolerance range in the art, such as within two standard deviations of the mean. "About" may be understood to be within 10%, 9%, 8%, 7%, 6%, 5%, 4%, 3%, 2%, 1%, 0.5%, 0.1%, 0.05%, or 0.01% of the stated value. Unless the context clearly indicates otherwise, all numerical values provided herein are modified by the term "about".
[0042] In addition, when a numerical range is disclosed in this specification, the range is continuous and includes all values from the minimum value of the range to its maximum value, unless otherwise specified. In addition, when such a range involves an integer value, all integers including the minimum value to the maximum value are included, unless otherwise specified. In this specification, when describing the range of a variable, it will be understood that the variable includes all values, including the endpoints described in the range. For example, the range "5 to 10" will be understood to include any sub-ranges (e.g., 6 to 10, 7 to 10, 6 to 9, 7 to 9, etc.) and individual values of 5, 6, 7, 8, 9 and 10, and will also be understood to include any value between the valid integers in the range, such as 5.5, 6.5, 7.5, 5.5 to 8.5, 6.5 to 9, etc. In addition, for example, the range "10% to 30%" will be understood to include sub-ranges (e.g., 10% to 15%, 12% to 18%, 20% to 30%, etc.) and all integers (including values of 10%, 11%, 12%, 13%, etc. up to 30%), and will also be understood to include any values between the valid integers in the stated range, e.g., 10.5%, 15.5%, 25.5%, etc.
[0043] It should be understood that the term "vehicle" or "vehicular" or other similar terms as used herein generally include motor vehicles, such as passenger vehicles including sport utility vehicles (SUVs), buses, trucks, various commercial vehicles, watercraft including various boats and ships, aircraft, etc., and include hybrid vehicles, electric vehicles, plug-in hybrid electric vehicles, hydrogen-powered vehicles, and other alternative fuel vehicles (e.g., fuels derived from non-petroleum energy sources). As referred to herein, a hybrid vehicle is a vehicle having two or more sources of power, such as a vehicle that has both gasoline power and electric power.
[0044] Figure 1 An exemplary all-solid-state battery according to an exemplary embodiment of the present invention is shown. Figure 1As shown, the all-solid-state battery may include: a negative electrode collector 10, a negative electrode layer 20 arranged on the negative electrode collector 10, a solid electrolyte layer 30 arranged on the negative electrode layer 20, a positive electrode layer 40 arranged on the solid electrolyte layer 30, and a positive electrode collector 50 arranged on the positive electrode layer 40.
[0045] The negative electrode current collector 10 may be a conductive plate-shaped substrate. For example, the negative electrode current collector 10 may be in the form of a sheet, a film, or a foil.
[0046] The negative electrode current collector 10 may include a material that does not react with lithium. For example, the negative electrode current collector may include at least one material selected from nickel (Ni), copper (Cu), stainless steel, and a combination thereof.
[0047] The thickness of the negative electrode collector 10 is not particularly limited, and may be, for example, in the range of about 1 μm to 500 μm.
[0048] The negative electrode layer 20 is formed as a thick film, and the thickness thereof is in the range of about 70 μm to about 150 μm.
[0049] In conventional all-solid-state batteries, when a thick negative electrode is manufactured, the passage of lithium ions grows, so that lithium ions cannot be transferred to a part of the negative electrode. As a result, the energy density is not sufficiently improved. Therefore, the present invention is characterized in that a plurality of lithium-philic layers capable of promoting the migration of lithium ions to the negative electrode layer 20 are introduced to solve the above problem.
[0050] Figure 2 20 according to the present invention is shown. Figure 2 As shown, the negative electrode layer 20 may include: a first lithium-philic layer 21 disposed on the negative electrode collector 10, a first negative electrode active material layer 23 disposed on the first lithium-philic layer 21, a second lithium-philic layer 25 disposed on the first negative electrode active material layer 23, and a second negative electrode active material layer 27 disposed on the second lithium-philic layer 25.
[0051] When charging the all-solid-state battery, lithium ions released from the positive electrode layer 40 migrate through the solid electrolyte layer 30 to the negative electrode layer 20. The lithium ions are attracted to the second lithium-philic layer 25 and allowed to diffuse and migrate toward the negative electrode current collector 10. Then, the lithium ions passing through the second lithium-philic layer 25 are attracted to the first lithium-philic layer 21 and allowed to diffuse and migrate toward the negative electrode current collector 10. Particularly in the existing thick-film negative electrode, the diffusion direction of lithium ions is not uniform, so it is difficult for lithium ions to diffuse throughout the negative electrode. However, in the negative electrode layer 20 according to an exemplary embodiment of the present invention, the first lithium-philic layer 21 and the second lithium-philic layer 25 promote the diffusion of lithium ions toward the negative electrode current collector 10. Therefore, lithium ions can diffuse throughout the negative electrode layer 20. In addition, in the negative electrode layer 20 according to an exemplary embodiment of the present invention, the diffusion of lithium ions occurs uniformly in the direction toward the negative electrode current collector 10, thus shortening the channels for lithium ions. Therefore, according to an exemplary embodiment of the present invention, the entire region of the thick-film negative electrode layer 20 can be used for the electrochemical reaction of the battery. In addition, lithium precipitation within the negative electrode layer 20 can be prevented.
[0052] The first lithium-philic layer 21 may include a first metal capable of alloying with lithium, an oxide of the first metal, or a combination thereof.
[0053] The first metal may include one or more selected from lithium (Li), indium (In), gold (Au), silver (Ag), bismuth (Bi), zinc (Zn), aluminum (Al), iron (Fe), tin (Sn), and titanium (Ti).
[0054] The first lithium-philic layer 21 may suitably include zinc oxide (ZnO), gold (Au), or silver (Ag).
[0055] The first negative electrode active material layer 23 may include a first negative electrode active material, a first solid electrolyte, a first binder, etc.
[0056] The first negative electrode active material may include a carbon-based active material, a silicon-based active material, or a combination thereof. The first negative electrode active material may preferably be a combination of a carbon-based active material and a silicon-based active material. For example, it may be in a form in which a core unit containing a carbon-based active material is coated with a shell unit containing a silicon-based active material.
[0057] Examples of the carbon-based active material may include natural graphite, artificial graphite, etc.
[0058] Examples of the silicon-based active material may include Si, SiO x (where 0 < x < 2), etc.
[0059] The average particle size of the first negative electrode active material may not be particularly limited, but for example, it may be in the range of about 8 μm to 10 μm.
[0060] The first solid electrolyte may include a sulfide-based solid electrolyte.
[0061] Examples of sulfide-based solid electrolytes may include: Li 2 SP 2 S 5 , Li 2 SP 2 S 5 -LiI, Li 2 SP 2 S 5 -LiCl, Li 2 SP 2 S 5 -LiBr, Li 2 SP 2 S 5 -Li 2 O. Li 2 SP 2 S 5 -Li 2 O-LiI、Li 2 S-SiS 2 , Li 2 S-SiS 2 -LiI, Li 2 S-SiS 2 -LiBr, Li 2 S-SiS 2 -LiCl, Li 2 S-SiS 2 -B 2 S 3 -LiI, Li 2 S-SiS 2 -P 2 S 5 -LiI, Li 2 SB 2 S 3 , Li 2 SP 2 S 5 -Z m S n (wherein m and n are each independently a positive number, and Z is one of Ge, Zn and Ga), Li 2 S-GeS 2 , Li 2 S-SiS 2 -Li 3 PO 4 , Li 2 S-SiS 2 -Li x MO y(wherein x and y are each independently a positive number, and M is one of P, Si, Ge, B, Al, Ga, and In), Li 10 GeP 2 S 12 etc.
[0062] Examples of the first binder may include styrene-butadiene rubber (SBR), nitrile rubber (NBR), butadiene rubber (BR), polyvinylidene fluoride, polytetrafluoroethylene, etc.
[0063] The first negative electrode active material layer 23 may contain a first negative electrode active material and a first solid electrolyte in a mass ratio range of about 6:4 to 8.5:1.5. In addition, based on 100 parts by weight of the sum of the first negative electrode active material and the first solid electrolyte, the first negative electrode active material layer 23 may contain about 1 part by weight to 5 parts by weight of a first binder.
[0064] The second lithium-philic layer 25 may contain a second metal capable of alloying with lithium, an oxide of the second metal, or a combination thereof.
[0065] The second metal may suitably include one or more selected from lithium (Li), indium (In), gold (Au), silver (Ag), bismuth (Bi), zinc (Zn), aluminum (Al), iron (Fe), tin (Sn), and titanium (Ti).
[0066] The second lithium-philic layer 25 may suitably contain zinc oxide (ZnO), gold (Au), or silver (Ag). The composition of the second lithium-philic layer 25 may be the same as or different from that of the first lithium-philic layer 21.
[0067] The second negative electrode active material layer 27 may contain a second negative electrode active material, a second solid electrolyte, a second binder, etc.
[0068] The second negative electrode active material may include a carbon-based active material, a silicon-based active material, or a combination thereof. The second negative electrode active material is preferably a combination of a carbon-based active material and a silicon-based active material. For example, it may be in a form in which a core unit containing a carbon-based active material is coated with a shell unit containing a silicon-based active material. The second negative electrode active material may be the same as or different from the first negative electrode active material.
[0069] Examples of the carbon-based active material may include natural graphite, artificial graphite, etc.
[0070] Examples of the silicon-based active material may include Si, SiO x (where 0 < x < 2) etc.
[0071] The average particle diameter (D50) of the second negative electrode active material may not be particularly limited, but for example, it may be in the range of about 8 μm to 10 μm.
[0072] The second solid electrolyte may include a sulfide-based solid electrolyte. The second solid electrolyte may be the same as or different from the first solid electrolyte.
[0073] Examples of sulfide-based solid electrolytes may include: Li 2 SP 2 S 5 , Li 2 SP 2 S 5 -LiI, Li 2 SP 2 S 5 -LiCl, Li 2 SP 2 S 5 -LiBr, Li 2 SP 2 S 5 -Li 2 O. Li 2 SP 2 S 5 -Li 2 O-LiI、Li 2 S-SiS 2 , Li 2 S-SiS 2 -LiI, Li 2 S-SiS 2 -LiBr, Li 2 S-SiS 2 -LiCl, Li 2 S-SiS 2 -B 2 S 3 -LiI, Li 2 S-SiS 2 -P 2 S 5 -LiI, Li 2 SB 2 S 3 , Li 2 SP 2 S 5 -Z m S n (wherein m and n are each independently a positive number, and Z is one of Ge, Zn and Ga), Li 2 S-GeS 2 , Li 2 S-SiS 2 -Li 3 PO 4 , Li 2 S-SiS 2 -Li x MOy (wherein x and y are each independently a positive number, and M is one of P, Si, Ge, B, Al, Ga and In), Li 10 G 2 S 12 wait.
[0074] Examples of the second adhesive may include styrene butadiene rubber (SBR), nitrile butadiene rubber (NBR), butadiene rubber (BR), polyvinylidene fluoride, polytetrafluoroethylene, etc. The second adhesive may be the same as or different from the first adhesive.
[0075] The second negative electrode active material layer 27 may include the second negative electrode active material and the second solid electrolyte in a mass ratio ranging from about 6:4 to 8.5:1.5. In addition, the second negative electrode active material layer 27 may include about 1 to 5 parts by weight of the second binder based on 100 parts by weight of the sum of the second negative electrode active material and the second solid electrolyte.
[0076] Figure 3 Specific details of the negative electrode layer 20 according to the exemplary embodiment of the present invention are shown.
[0077] The negative electrode layer 20 may include a first major surface A in contact with the negative electrode collector 10 and a second major surface B in contact with the solid electrolyte layer 30 .
[0078] In the negative electrode layer 20 , the second lithium-philic layer 25 may be located in a space between a first plane A′ facing the periphery of the first major surface A and a second plane B′ facing the periphery of the second major surface B.
[0079] The first plane A′ may be an imaginary plane spaced apart from the first major surface A toward the solid electrolyte layer 30 by a distance corresponding to about 40% of the thickness of the negative electrode layer 20 in the thickness direction.
[0080] The second plane B′ may be an imaginary plane spaced apart from the second major surface B toward the negative electrode current collector 10 by a distance corresponding to about 40% of the thickness of the negative electrode layer 20 in the thickness direction.
[0081] When the second lithium-philic layer 25 is located in the above space, the migration of lithium ions can be effectively promoted.
[0082] The negative electrode layer 20 may satisfy Condition 1.
[0083] [Condition 1]
[0084]
[0085] In this case, x 1 can be the thickness of the first lithiophilic layer, x 2It may be the thickness of the second lithiophilic layer.
[0086] When the thickness of the lithium-philic layer 25 falls within the above range, migration of lithium ions can be promoted without increasing the electrode resistance of the negative electrode layer 20 .
[0087] The solid electrolyte layer 30 is interposed between the negative electrode layer 20 and the positive electrode layer 40 , and may include a lithium ion conductive solid electrolyte.
[0088] The solid electrolyte may include an oxide-based solid electrolyte, a sulfide-based solid electrolyte, or the like.
[0089] Examples of oxide-based solid electrolytes may include perovskite-type LLTO (Li 3x La 2 / 3-x TiO 3 ), phosphate-based NASICON-type LATP (Li 1+x Al x Ti 2-x (PO 4 ) 3 )wait.
[0090] Examples of sulfide-based solid electrolytes may include: Li 2 SP 2 S 5 , Li 2 SP 2 S 5 -LiI, Li 2 SP 2 S 5 -LiCl, Li 2 SP 2 S 5 -LiBr, Li 2 SP 2 S 5 -Li 2 O. Li 2 SP 2 S 5 -Li 2 O-LiI、Li 2 S-SiS 2 , Li 2 S-SiS 2 -LiI, Li 2 S-SiS 2 -LiBr, Li 2 S-SiS 2 -LiCl, Li 2 S-SiS 2 -B 2 S 3 -LiI, Li2 S-SiS 2 -P 2 S 5 -LiI, Li 2 SB 2 S 3 , Li 2 SP 2 S 5 -Z m S n (wherein m and n are each independently a positive number, and Z is one of Ge, Zn and Ga), Li 2 S-GeS 2 , Li 2 S-SiS 2 -Li 3 PO 4 , Li 2 S-SiS 2 -Li x MO y (wherein x and y are each independently a positive number, and M is one of P, Si, Ge, B, Al, Ga and In), Li 10 G 2 S 12 wait.
[0091] The positive electrode layer 40 may include a positive electrode active material, a solid electrolyte, a conductive material, a binder, and the like.
[0092] The positive electrode active material can store and release lithium ions.
[0093] Examples of positive electrode active materials may include: rock salt layer type active materials such as LiCoO 2 、LiMnO 2 、LiNiO 2 、LiVO 2 , Li 1+x Ni 1 / 3 Co 1 / 3 Mn 1 / 3 O 2 etc.; spinel active materials, such as LiMn 2 O 4 、Li(Ni 0.5 Mn 1.5 ) 4 etc.; Inverse spinel active materials, such as LiNiVO 4 、LiCoVO 4 etc.; Olivine-type active materials, such as LiFePO 4 、LiMnPO 4 、LiCoPO 4 、LiNiPO 4etc.; Silicon-containing active materials, such as Li 2 FeSiO 4 , Li 2 MnSiO 4 etc.; rock salt layer type active materials where part of the transition metal is replaced by different metals, such as LiNi 0.8 Co (0.2-x) Al x O 2 (where 0<x<0.2), etc.; spinel-type active materials in which a portion of transition metals are replaced by different metals, such as Li 1+x Mn 2-x-y M y O 4 (wherein M is at least one of Al, Mg, Co, Fe, Ni and Zn, 0<x+y<2); lithium titanate, such as Li 4 Ti 5 O 12 wait.
[0094] The solid electrolyte may include an oxide-based solid electrolyte or a sulfide-based solid electrolyte. However, it is preferred to use a sulfide-based solid electrolyte having high lithium ion conductivity. The sulfide-based solid electrolyte is not particularly limited, but examples thereof may include: Li 2 SP 2 S 5 , Li 2 SP 2 S 5 -LiI, Li 2 SP 2 S 5 -LiCl, Li 2 SP 2 S 5 -LiBr, Li 2 SP 2 S 5 -Li 2 O. Li 2 SP 2 S 5 -Li 2 O-LiI、Li 2 S-SiS 2 , Li 2 S-SiS 2 -LiI, Li 2 S-SiS 2 -LiBr, Li 2 S-SiS 2 -LiCl, Li 2 S-SiS 2 -B 2 S 3-LiI, Li 2 S-SiS 2 -P 2 S 5 -LiI, Li 2 SB 2 S 3 , Li 2 SP 2 S 5 -Z m S n (wherein m and n are each independently a positive number, and Z is one of Ge, Zn and Ga), Li 2 S-GeS 2 , Li 2 S-SiS 2 -Li 3 PO 4 , Li 2 S-SiS 2 -Li x MO y (wherein x and y are each independently a positive number, and M is one of P, Si, Ge, B, Al, Ga and In), Li 10 G 2 S 12 The solid electrolyte contained in the positive electrode layer 40 may be the same as or different from the solid electrolyte contained in the solid electrolyte layer 30 .
[0095] Examples of the conductive material may include carbon black, conductive graphite, acetylene black, graphene, and the like.
[0096] Examples of the binder may include butadiene rubber (BR), nitrile rubber (NBR), hydrogenated nitrile rubber (HNBR), polyvinylidene fluoride, polytetrafluoroethylene, and the like.
[0097] The positive electrode current collector 50 may include a conductive plate-shaped substrate. The positive electrode current collector 50 may include an aluminum foil.
[0098] The thickness of the positive electrode collector 50 may not be particularly limited, and may be, for example, in the range of about 1 μm to 500 μm.
[0099] In one aspect, a method for manufacturing an all-solid-state battery is provided, which may include the following steps: forming a negative electrode layer on a negative electrode collector; forming a solid electrolyte layer on the negative electrode layer; forming a positive electrode layer on the solid electrolyte layer; and forming a positive electrode collector on the positive electrode layer.
[0100] The formation of the negative electrode layer may include: forming a first lithium-philic layer by depositing at least one selected from a first metal capable of alloying with lithium, an oxide of the first metal, and a combination thereof on the negative electrode collector; forming a first negative electrode active material layer containing a first negative electrode active material on the first lithium-philic layer; forming a second lithium-philic layer by depositing at least one selected from a second metal capable of alloying with lithium, an oxide of the second metal, and a combination thereof on the first negative electrode active material layer; and forming a second negative electrode active material layer containing a second negative electrode active material on the second lithium-philic layer.
[0101] When forming the first lithium-philic layer, the first metal, the oxide of the first metal, or a combination thereof may be sputtered on the negative electrode current collector.
[0102] When forming the first negative electrode active material layer, a first slurry containing the first negative electrode active material may be applied on the first lithium-philic layer and then dried. The first slurry may further contain a first solid electrolyte, a first binder, and the like.
[0103] When forming the second lithium-philic layer, the second metal, the oxide of the second metal, or a combination thereof may be sputtered on the second negative electrode active material layer.
[0104] When forming the second negative electrode active material layer, a second slurry containing the second negative electrode active material may be applied on the second lithium-philic layer and then dried. The second slurry may further contain a second solid electrolyte, a second binder, and the like.
[0105] The formation of the negative electrode layer can satisfy condition 2.
[0106] [Condition 2]
[0107]
[0108] In this case, t 1 It can be the deposition time required to form the first lithium-philic layer, t 2 It may be the deposition time required to form the second lithiophilic layer.
[0109] The deposition time is a variable related to the thickness of each lithiophilic layer, and the thickness of the lithiophilic layer increases in proportion to the deposition time, regardless of the applied power and pressure. Therefore, condition 2 can be aimed at achieving condition 1 above.
[0110] The method of forming the solid electrolyte layer, the positive electrode layer and the positive electrode current collector is not particularly limited. The respective components may be formed simultaneously or at different times.
[0111] In addition, the manufacturing method may include not only directly forming the solid electrolyte layer, the positive electrode layer and the positive electrode collector on the negative electrode layer, the solid electrolyte layer and the positive electrode layer, respectively, but also separately forming each component and then stacking these components as shown in FIG. Figure 1 The structure shown.
[0112] Example
[0113] The exemplary embodiments of the present invention will be described in more detail by the following examples. The following examples are only used to help understand the present invention, and the scope of the present invention is not limited thereto.
[0114] Example
[0115] A nickel foil was prepared as a negative electrode current collector.
[0116] A first metal gold (Au) is sputtered on the negative electrode current collector for about 60 seconds to form a first lithium-philic layer.
[0117] The first negative electrode active material, the first solid electrolyte and the first binder are introduced into a non-polar solvent to prepare a first slurry. Graphite coated with silicon is used as the first negative electrode active material. 6 PS 5 A sulfide-based solid electrolyte represented by Cl is used as the first solid electrolyte. Butadiene rubber (BR) is used as the first binder. The first slurry is applied on the first lithium-philic layer and then dried to form a first negative electrode active material layer.
[0118] A second metal gold (Au) is sputtered on the first negative electrode active material layer for about 30 seconds to form a second lithium-philic layer.
[0119] The second negative electrode active material, the second solid electrolyte and the second binder are introduced into a non-polar solvent to prepare a second slurry. Graphite coated with silicon is used as the second negative electrode active material. 6 PS 5 A sulfide-based solid electrolyte represented by Cl is used as the second solid electrolyte. Butadiene rubber (BR) is used as the second binder. The second slurry is applied on the second lithium-philic layer and then dried to form a second negative electrode active material layer.
[0120] The first lithiophilic layer, the first negative electrode active material layer, the second lithiophilic layer, and the second negative electrode active material layer were compressed to obtain a negative electrode layer having a thickness of about 100 μm.
[0121] Figure 3 The location where the second lithiophilic layer is formed is shown.
[0122] The solid electrolyte layer, the positive electrode layer, and the positive electrode collector are attached to the negative electrode layer to complete the fabrication of the all-solid-state battery.
[0123] Figure 4 The results of analyzing a cross section of a negative electrode layer according to one embodiment using a scanning electron microscope (SEM) are shown. Figure 5Energy dispersive X-ray spectroscopy (EDS) is used to show Figure 4 Referring to the results shown on the gold (Au) element, the first lithium-philic layer and the second lithium-philic layer are well deposited in the negative electrode layer.
[0124] Comparative Example 1
[0125] A negative electrode layer is formed in which the first lithium-philic layer and the second lithium-philic layer are not formed.
[0126] The negative electrode active material, the solid electrolyte and the binder are introduced into a non-polar solvent to prepare a slurry. The negative electrode active material, the solid electrolyte and the binder are respectively the same as the first negative electrode active material, the first solid electrolyte and the binder in the embodiment. The slurry is applied on a nickel foil (negative electrode collector) and then dried to form a negative electrode layer. The negative electrode layer is compressed so that its thickness is adjusted to about 100 μm.
[0127] The solid electrolyte layer, the positive electrode layer, and the positive electrode collector are attached to the negative electrode layer to complete the fabrication of the all-solid-state battery.
[0128] Comparative Example 2
[0129] The negative electrode layer was formed in the same manner as in Example 1, except that only the second lithium-philic layer was formed without forming the first lithium-philic layer. A solid electrolyte layer, a positive electrode layer, and a positive electrode collector were attached to the negative electrode layer to complete the manufacture of the all-solid-state battery.
[0130] Comparative Example 3
[0131] The negative electrode layer was formed in the same manner as in Example 1, except that only the first lithium-philic layer was formed without forming the second lithium-philic layer. A solid electrolyte layer, a positive electrode layer, and a positive electrode collector were attached to the negative electrode layer to complete the manufacture of the all-solid-state battery.
[0132] Comparative Example 4
[0133] The negative electrode layer was formed in the same manner as in Example 1, except that the second lithium-philic layer was located at Figure 3 In the space between the first main surface A and the first plane A' in the solid electrolyte layer, the positive electrode layer and the positive electrode collector are attached to the negative electrode layer to complete the manufacture of the all-solid-state battery.
[0134] Comparative Example 5
[0135] The negative electrode layer was formed in the same manner as in Example 1, except that the second lithium-philic layer was located at Figure 3In the space between the second main surface B and the second plane B' in the embodiment of the present invention, a solid electrolyte layer, a positive electrode layer and a positive electrode collector are attached to the negative electrode layer to complete the manufacture of the all-solid-state battery.
[0136] Comparative Example 6
[0137] The negative electrode layer was formed in the same manner as in Example 1, except that Figure 3 The required deposition times for the first and second lithiophilic layers are varied as described. A solid electrolyte layer, a positive electrode layer, and a positive current collector are attached to the negative electrode layer to complete the fabrication of the all-solid-state battery.
[0138] Comparative Example 7
[0139] The negative electrode layer was formed in the same manner as in Example 1, except that Figure 3 The required deposition times for the first and second lithiophilic layers are varied as described. A solid electrolyte layer, a positive electrode layer, and a positive current collector are attached to the negative electrode layer to complete the fabrication of the all-solid-state battery.
[0140] Under the same conditions, the capacity retention rates of the all-solid-state batteries manufactured in Examples and Comparative Examples 1 to 7 after 30 charge and discharge cycles were measured. The results are shown in Table 1.
[0141] Table 1
[0142]
[0143] 1) The position of the second lithium-philic layer is based on Figure 3 shown.
[0144] 2) Deposition time required to form the first lithium-philic layer (t 1 ) and the deposition time required to form the second lithium-philic layer (t 2 ) is set to satisfy
[0145] 3) Deposition time required to form the first lithium-philic layer (t 1 ) and the deposition time required to form the second lithium-philic layer (t 2 ) is set to satisfy
[0146] As shown in Table 1, Comparative Examples 1 to 3 (including only at most one of the first lithiophilic layer and the second lithiophilic layer) exhibited extremely low capacity retention rates of 71% or less. On the other hand, the examples satisfying the conditions of the second lithiophilic layer position and the required deposition time of each lithiophilic layer exhibited extremely high capacity retention rates of about 91%.
[0147] While the present invention has been particularly shown and described with reference to exemplary embodiments thereof, it is to be understood that the scope of the present invention is not limited to the disclosed exemplary embodiments. Modifications are also included within the scope of the present invention.
Claims
1. An all-solid-state battery, include: A negative electrode current collector; A negative electrode layer, which is disposed on the negative electrode current collector; a solid electrolyte layer disposed on the negative electrode layer; a positive electrode layer disposed on the solid electrolyte layer; and a positive electrode current collector disposed on the positive electrode layer, Wherein, the negative electrode layer comprises: A first lithium-philic layer, which is disposed on the negative electrode current collector and comprises a first metal capable of alloying with lithium, an oxide of the first metal, or a combination thereof; a first negative electrode active material layer, which is disposed on the first lithium-philic layer and comprises a first negative electrode active material; a second lithium-philic layer disposed on the first negative electrode active material layer and comprising a second metal capable of alloying with lithium, an oxide of the second metal, or a combination thereof; and The second negative electrode active material layer is disposed on the second lithium-philic layer and comprises a second negative electrode active material.
2. The all-solid-state battery according to claim 1, in, The first metal includes lithium, indium, gold, silver, bismuth, zinc, aluminum, iron, tin, titanium or a combination thereof.
3. The all-solid-state battery according to claim 1, in, The first negative electrode active material includes a carbon-based active material, a silicon-based active material or a combination thereof.
4. The all-solid-state battery according to claim 1, in, The second metal includes lithium, indium, gold, silver, bismuth, zinc, aluminum, iron, tin, titanium or a combination thereof.
5. The all-solid-state battery according to claim 1, in, The second negative electrode active material includes a carbon-based active material, a silicon-based active material or a combination thereof.
6. The all-solid-state battery according to claim 1, in, The thickness of the negative electrode layer is in the range of 70 μm to 150 μm.
7. The all-solid-state battery according to claim 1, in, The negative electrode layer comprises: a first major surface in contact with the negative electrode current collector; and a second major surface in contact with the solid electrolyte layer, In which, the second lithium-philic layer is located in the space between the first plane and the second plane, the distance between the first plane and the first main surface toward the solid electrolyte layer corresponds to 40% of the thickness of the negative electrode layer along the thickness direction, and the distance between the second plane and the second main surface toward the negative electrode collector corresponds to 40% of the thickness of the negative electrode layer along the thickness direction.
8. The all-solid-state battery according to claim 1, in, The all-solid-state battery meets condition 1, Condition 1 where x 1 is the thickness of the first lithiophilic layer, x 2 is the thickness of the second lithiophilic layer.
9. A method for manufacturing an all-solid-state battery, the method include: forming a negative electrode layer on the negative electrode current collector; forming a solid electrolyte layer on the negative electrode layer; forming a positive electrode layer on the solid electrolyte layer; as well as forming a positive electrode collector on the positive electrode layer; Wherein, the formation of the negative electrode layer comprises: forming a first lithium-philic layer by depositing a first metal, an oxide of the first metal, or a combination thereof capable of alloying with lithium on the negative electrode current collector; forming a first negative electrode active material layer including a first negative electrode active material on the first lithium-philic layer; forming a second lithium-philic layer by depositing a second metal, an oxide of the second metal, or a combination thereof capable of alloying with lithium on the first negative electrode active material layer; and A second negative electrode active material layer including a second negative electrode active material is formed on the second lithium-philic layer.
10. The method for manufacturing an all-solid-state battery according to claim 9, in, The first metal includes lithium, indium, gold, silver, bismuth, zinc, aluminum, iron, tin, titanium or a combination thereof.
11. The method for manufacturing an all-solid-state battery according to claim 9, in, When forming the first lithium-philic layer, a first metal, an oxide of the first metal, or a combination thereof is sputtered onto the negative electrode current collector.
12. The method for manufacturing an all-solid-state battery according to claim 9, in, The first negative electrode active material includes a carbon-based active material, a silicon-based active material or a combination thereof.
13. The method for manufacturing an all-solid-state battery according to claim 9, in, The second metal includes lithium, indium, gold, silver, bismuth, zinc, aluminum, iron, tin, titanium or a combination thereof.
14. The method for manufacturing an all-solid-state battery according to claim 9, in, When forming the second lithium-philic layer, a second metal, an oxide of the second metal, or a combination thereof is sputtered onto the first negative electrode active material layer.
15. The method for manufacturing an all-solid-state battery according to claim 9, in, The second negative electrode active material includes a carbon-based active material, a silicon-based active material or a combination thereof.
16. The method for manufacturing an all-solid-state battery according to claim 9, in, The thickness of the negative electrode layer is in the range of 70 μm to 150 μm.
17. The method for manufacturing an all-solid-state battery according to claim 9, in, The negative electrode layer comprises: a first major surface in contact with the negative electrode current collector; and a second major surface in contact with the solid electrolyte layer, In which, the second lithium-philic layer is located in the space between the first plane and the second plane, the distance between the first plane and the first main surface toward the solid electrolyte layer corresponds to 40% of the thickness of the negative electrode layer along the thickness direction, and the distance between the second plane and the second main surface toward the negative electrode collector corresponds to 40% of the thickness of the negative electrode layer along the thickness direction.
18. The method for manufacturing an all-solid-state battery according to claim 9, in, The all-solid-state battery meets condition 1, Condition 1 where x 1 is the thickness of the first lithiophilic layer, x 2 is the thickness of the second lithiophilic layer.
19. The method for manufacturing an all-solid-state battery according to claim 9, in, The method satisfies condition 2, Condition 2 where t 1 is the deposition time required to form the first lithium-philic layer, t 2 is the deposition time required to form the second lithiophilic layer.
20. A vehicle comprising the all-solid-state battery according to claim 1.