Solid electrolyte and preparation method and application thereof

By doping high-valent elements in the garnet-type solid electrolyte matrix layer and depositing a Sn-Li alloy layer, the problem of lithium dendrite formation in the oxide solid electrolyte is solved, the ionic conductivity and cycle performance of the solid electrolyte are improved, and the Efficient lithium-ion battery performance.

CN118782890APending Publication Date: 2024-10-15HUNAN FARNLET NEW ENERGY TECH CO LTD +1
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202410662342.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-05-27
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

Existing oxide solid electrolytes are prone to generate lithium dendrites during the charge and discharge process, resulting in a decrease in ionic conductivity and poor cycle performance. Existing doping and interface modification methods have decomposition reactions at high points and complicated preparation processes. question.

Method used

The garnet-type solid electrolyte matrix layer is doped with high-valent elements (such as Al, Ga, Ta) through the Li site, and a Sn-Li alloy layer is deposited on the surface. An interface modification layer is formed through a magnetron sputtering process to improve the ionic conductivity. and cyclic stability.

Benefits of technology

It achieves excellent ionic conductivity and cycle performance of the solid electrolyte, maintains a capacity retention rate of more than 94%, simplifies the preparation process and reduces the interface impedance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004860080040000101
    Figure BDA0004860080040000101
  • Figure BDA0004860080040000111
    Figure BDA0004860080040000111
  • Figure BDA0004860080040000112
    Figure BDA0004860080040000112
Patent Text Reader

Abstract

The invention relates to the technical field of lithium batteries, and discloses a solid electrolyte and a preparation method and application thereof.The solid electrolyte comprises a solid electrolyte matrix layer and a Sn-Li alloy layer, the structural expression of the solid electrolyte matrix layer is Li < 7-3x > M < x > La < 3 > Zr < 2 > O < 12 >, and x is larger than 0 and smaller than or equal to 0.3; the M element is selected from any one of Al, Ga and Ta; the Sn-Li alloy layer is deposited on the surface of the solid electrolyte matrix layer. The Sn-Li alloy layer in the solid electrolyte not only can be used as a conductive layer to uniformly distribute an internal electric field and inhibit nucleation of lithium dendrites, but also has relatively good stone affinity, and is beneficial to solving the problem of poor interface contact between a lithium metal negative electrode and the LLZO-based solid electrolyte. In addition, the lithium ion battery prepared from the solid electrolyte has excellent cycle stability, and the capacity retention ratio of 94% or above can still be maintained after 500 cycles.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of lithium batteries, and in particular to a solid electrolyte and a preparation method and application thereof. Background Art

[0002] As the demand for portable electronic products and electric vehicles continues to increase, the demand for high-performance, long-life and safe batteries is becoming increasingly urgent. Solid electrolytes have attracted widespread attention due to their light weight, compact structure, high energy density and higher safety. The current mainstream solid electrolytes are polymers, oxides and sulfides, among which oxide solid electrolytes have become the main research hotspot due to their better electrochemical and mechanical stability compared to sulfides and polymers. However, since oxide solid electrolytes are usually composed of micron-sized particles with defects and micropores, lithium dendrites are easily generated during the charge and discharge process, resulting in a decrease in ionic conductivity and poor cycle performance.

[0003] Related studies have shown that lithium dendrites can form at different locations in solid electrolytes, and their locations mainly include the following three types: ① Reduced Li accumulates in cracks or pre-existing pores to form lithium dendrites; ② Li dendrites penetrate the electrolyte at the Li / oxide electrolyte interface through grains or grain boundaries; ③ Due to electron leakage from the electrolyte, reduced Li accumulates inside the electrolyte. In the related art, in order to reduce the harm caused by lithium dendrites, researchers have tried to inhibit lithium dendrites by element doping or interface modification. For example, CN 109980272 A discloses that Al-doped sheet LLZO solid electrolyte has a good inhibitory effect on lithium dendrites. It has good flexibility and a stable cubic phase, can provide more lithium ion fast conduction channels, and has high ionic conductivity; CN 115882052 A discloses an interface modification layer of a garnet-type solid electrolyte and a preparation method thereof, which uses an in-situ conversion reaction to construct an ultra-thin Al2O3 nanolayer on the surface of the solid electrolyte, and improves the interface wettability between the solid electrolyte and lithium metal, reduces the interface impedance, and improves the interface flatness, eliminates part of the interface gap, and thus prevents excessive deposition of lithium (lithium dendrites). However, in actual applications, at higher points (0.004-0.55V), Al doping will accelerate the decomposition reaction of LLZO to generate metal / alloy phases (such as Zr4Al3, Zr2Al3, ZrAl2, etc.), resulting in Li + The reduction of LLZO and the formation of Li dendrites affect the cycle performance; although the Al2O3 nanolayer can effectively improve the interface contact between LLZO and the negative electrode and prevent the formation of lithium dendrites at the interface, its preparation process is complicated and its chemical stability and ionic conductivity are limited.

[0004] Based on this, there is an urgent need to seek a solid electrolyte material and a preparation method thereof with excellent ionic conductivity, good chemical stability and excellent cycle performance. Summary of the invention

[0005] The present invention aims to solve at least one of the technical problems existing in the prior art. To this end, the present invention provides a solid electrolyte having excellent ionic conductivity and good cycle performance, and maintaining a capacity retention rate of more than 94% after 500 cycles.

[0006] The invention also provides a method for preparing the solid electrolyte.

[0007] The invention also provides a lithium ion battery.

[0008] The present invention also proposes an application of a solid electrolyte or a solid electrolyte preparation method in the preparation of energy storage materials.

[0009] A first aspect of the present invention provides a solid electrolyte, comprising:

[0010] Solid electrolyte matrix layer, the structural expression of the solid electrolyte matrix layer is Li 7-3x M x La3Zr2O 12 , wherein 0<x≤0.3, the M element is selected from any one of Al, Ga and Ta;

[0011] The Sn-Li alloy layer is deposited on the surface of the solid electrolyte matrix layer.

[0012] The solid electrolyte according to the embodiment of the present invention has at least the following beneficial effects:

[0013] (1) The solid electrolyte matrix layer of the present invention is obtained by further doping high-valent elements (such as Al, Ga or Ta) at the Li position on the basis of the garnet-type electrolyte matrix. The high-valent elements doped at the Li site can increase the concentration of Li vacancies and generate a stable and fast conductive cubic phase (such as Ga doping), which helps to further improve the ionic conductivity of the solid electrolyte.

[0014] (2) The solid electrolyte of the present invention further deposits a Sn-Li interface modification layer on the basis of the garnet-type electrolyte matrix doped with Li-site elements, which helps to reduce the interface impedance between the solid electrolyte and the lithium metal negative electrode, making Li + Flow homogenization promotes Li + They are evenly distributed at the interface, thereby reducing the formation of lithium dendrites and improving cycle stability.

[0015] (3) The Sn-Li alloy modified layer of the solid electrolyte of the present invention can not only serve as a conductive layer to make the internal electric field uniform and inhibit the nucleation of lithium dendrites, but also has good lithophilicity, which helps to solve the problem of poor interface contact between the lithium metal negative electrode and the LLZO-based solid electrolyte.

[0016] In some embodiments of the present invention, the element ratio of Sn to Li in the Sn-Li alloy layer is 1 to 4:1; preferably, the element ratio of Sn to Li is 1.5 to 2:1.

[0017] In some embodiments of the present invention, the deposition method is magnetron sputtering.

[0018] In some embodiments of the present invention, the thickness ratio of the solid electrolyte matrix layer to the Sn—Li alloy layer is 100,000 nm: 5 to 20 nm.

[0019] In some embodiments of the present invention, the thickness of the solid electrolyte matrix layer is 0.8 to 1.5 mm, and the thickness of the Sn-Li alloy layer is 50 to 200 nm.

[0020] A second aspect of the present invention provides a method for preparing the solid electrolyte according to any one of the first aspects, comprising the following steps:

[0021] S1. According to the molar ratio of the structural expression of the solid electrolyte matrix layer described in the first aspect, a lithium source, lanthanum trioxide, zirconium dioxide and an oxide of the M element are mixed, and pre-sintered at 900-980° C. to obtain a composite electrolyte powder;

[0022] S2, molding the composite electrolyte powder, and calcining it at 1100-1300° C. to obtain a solid electrolyte substrate;

[0023] S3, fixing the solid electrolyte substrate in a magnetron sputtering chamber, performing magnetron sputtering with metal tin as a target, and then performing magnetron sputtering with metal lithium as a target under heating conditions to deposit the Sn-Li alloy layer on the solid electrolyte substrate.

[0024] The preparation method according to the embodiment of the present invention has at least the following beneficial effects: the preparation process of the present invention is simple and does not require the addition of additional sintering aids. In addition, during the preparation process, the present invention uses a magnetron sputtering process to deposit the Sn-Li alloy layer, which helps to improve the uniformity of the Sn-Li alloy layer and thus promote the Li + Evenly distributed at the interface.

[0025] In some embodiments of the present invention, the lithium source includes lithium hydroxide monohydrate (LiOH·H2O).

[0026] In some embodiments of the present invention, in step S1, the mixing further includes ball milling and drying.

[0027] In some embodiments of the present invention, the rotation speed of the ball mill is 300-400 rpm, and the ball milling time is 4-5 hours.

[0028] In some embodiments of the present invention, the pre-sintering time is 10 to 18 hours.

[0029] In some embodiments of the present invention, the compression molding pressure is 50-100 MPa.

[0030] In some embodiments of the present invention, the calcination time is 10 to 18 hours.

[0031] In some embodiments of the present invention, the cooling rate after calcination is 4-6°C / min.

[0032] In some embodiments of the present invention, the cooling further includes surface grinding and polishing.

[0033] In some embodiments of the present invention, during the magnetron sputtering process, when the metal tin is used as the target material, the vacuum degree is 0.8-1.2 Pa.

[0034] In some embodiments of the present invention, during the magnetron sputtering process, when the metallic lithium is used as a target material, the vacuum degree is 1.8 to 2.5 Pa, and the heating temperature of the solid electrolyte substrate is 350 to 450°C.

[0035] By adjusting the vacuum degree and substrate temperature during the magnetron sputtering process, it helps to promote the melting of metallic lithium into the metallic tin layer, so that the gaps between the Sn metal layer particles are filled and compacted by Li metal, thereby improving the contact between the two and reducing the interface resistance.

[0036] In some embodiments of the present invention, the power of the magnetron sputtering is 60-100W.

[0037] In some embodiments of the present invention, the atmosphere of the magnetron sputtering is an inert atmosphere.

[0038] In some embodiments of the present invention, the inert atmosphere is selected from at least one of helium (He), neon (Ne), argon (Ar), krypton (Kr), and xenon (Xn); preferably, the inert atmosphere is argon.

[0039] Since the chemical reactivity of inert gas is very low, it can be used as a protective gas under high temperature conditions. Under the preparation conditions of the present invention, it basically does not react with the solid electrolyte of the present invention or any of its precursors or intermediates, thereby avoiding the occurrence of potential side reactions in the preparation process and ensuring that the prepared solid electrolyte has an ideal lattice structure.

[0040] In some embodiments of the present invention, the purity of the inert atmosphere is greater than or equal to 98%. Preferably, the purity of the inert atmosphere is greater than or equal to 99%.

[0041] A third aspect of the present invention provides a lithium-ion battery, comprising the solid electrolyte described in any one of the first aspects, wherein the Sn-Li alloy layer of the solid electrolyte is arranged on a side close to the lithium metal negative electrode.

[0042] The lithium ion battery according to the embodiment of the present invention has at least the following beneficial effects: the lithium ion battery made by using the solid electrolyte of the present invention has excellent cycle stability and can still maintain a capacity retention rate of more than 94% after 500 cycles.

[0043] A fourth aspect of the present invention provides an application of the solid electrolyte described in any one of the first aspect or the solid electrolyte preparation method described in any one of the second aspect in the preparation of energy storage materials.

[0044] Other features and advantages of the present invention will be set forth in the description which follows, and in part will be apparent from the description, or may be learned by practice of the present invention. DETAILED DESCRIPTION

[0045] The following will be combined with the embodiments to clearly and completely describe the concept of the present invention and the technical effects produced, so as to fully understand the purpose, characteristics and effects of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, other embodiments obtained by those skilled in the art without creative work are all within the scope of protection of the present invention.

[0046] When a numerical range is disclosed herein, the above range is considered to be continuous and includes the minimum and maximum values ​​of the range, as well as every value between such minimum and maximum values. Further, when a range refers to an integer, every integer between the minimum and maximum values ​​of the range is included. In addition, when multiple ranges are provided to describe features or characteristics, the ranges can be combined. In other words, unless otherwise indicated, all ranges disclosed herein should be understood to include any and all subranges included therein.

[0047] In the description of the present invention, the description with reference to the terms "one embodiment", "some embodiments", "illustrative embodiments", "examples", "specific examples", or "some examples" means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described may be combined in any one or more embodiments or examples in a suitable manner.

[0048] In the description of the present invention, the reference term "and / or" includes all and any combinations of one or more of the associated listed items.

[0049] Unless otherwise specified, "about" in the present invention means that the allowable error is within ±2%.

[0050] Unless otherwise specified, "room temperature" in the present invention means 25°C±5°C.

[0051] If the specific conditions are not specified in the examples, the experiments were carried out under conventional conditions or conditions recommended by the manufacturer. If the manufacturers of the reagents or instruments are not specified, they are all conventional products that can be purchased commercially.

[0052] Example 1: LALZO solid electrolyte

[0053] The present embodiment provides a solid electrolyte and a preparation method thereof. The solid electrolyte of the present embodiment comprises a solid electrolyte matrix layer and a Sn-Li interface modification layer (i.e., Sn-Li alloy layer), wherein the solid electrolyte matrix layer is obtained by doping Al at the Li position on the basis of a garnet-type electrolyte, i.e., Li 6.25 Al 0.25 La3Zr2O 12 The thickness of the solid electrolyte matrix layer is about 1 mm, and the thickness of the Sn-Li interface modification layer is about 150 nm.

[0054] The method for preparing the solid electrolyte of this embodiment specifically comprises the following steps:

[0055] (1) Preparation of composite electrolyte powder

[0056] According to the chemical formula Li 6.25 Al 0.25 La3Zr2O 12 The molar ratio of lithium hydroxide monohydrate (LiOH·H2O), aluminum oxide powder (Al2O3), lanthanum trioxide powder (La2O3) and zirconium dioxide powder (ZrO2) were respectively weighed, and then an appropriate amount of ball milling beads and a dispersion medium of isopropanol were added, and the mixture was ball milled at a speed of 300-400 rpm for 4-5 h. After ball milling, the mixture was dried at 80°C, and the dried mixture was pre-sintered in a muffle furnace at 950°C for 12 h, and then cooled to room temperature at a rate of 5°C / min to obtain a composite electrolyte powder.

[0057] (2) Preparation of solid electrolyte substrate

[0058] The composite electrolyte powder is placed in a mold, pressed into a circular sheet with a diameter of about 15 mm and a thickness of about 1 mm under 60 MPa, and calcined in a muffle furnace at 1250° C. for 12 hours. During the calcination process, a layer of mother powder (i.e., the composite electrolyte powder) is covered on the surface of the circular sheet to reduce lithium volatilization during the calcination process. After the calcination is completed, it is cooled to room temperature at a rate of 5° C. / min, and the surface is polished to obtain a solid electrolyte substrate;

[0059] (3) Sn-Li interface modification layer

[0060] The solid electrolyte substrate is fixed in a magnetron sputtering chamber, with a tin sheet as a target, the power of the magnetron sputtering is adjusted to 80W, the vacuum degree is 1Pa, and the sputtering time is controlled within 25 to 30s. At the same time, an argon atmosphere with a purity of 99.9% is introduced during the sputtering process. After the sputtering is completed, the temperature of the solid electrolyte substrate is heated to 400°C, the vacuum degree is adjusted to 2Pa, and then the lithium sheet is used as a target for sputtering. The sputtering time is 10 to 15s. After the sputtering is completed, it is cooled to room temperature to obtain a solid electrolyte.

[0061] Example 2: LGLZO solid electrolyte

[0062] The present embodiment provides a solid electrolyte and a preparation method thereof. The solid electrolyte of the present embodiment comprises a solid electrolyte matrix layer and a Sn-Li interface modification layer, wherein the solid electrolyte matrix layer is obtained by doping Ga at the Li position on the basis of a garnet-type electrolyte, i.e., Li 6.25 Ga 0.25 La3Zr2O 12 The thickness of the solid electrolyte matrix layer is about 1 mm, and the thickness of the Sn-Li interface modification layer is about 150 nm.

[0063] The method for preparing the solid electrolyte of this embodiment specifically comprises the following steps:

[0064] (1) Preparation of composite electrolyte powder

[0065] According to the chemical formula Li 6.25 Ga 0.25 La3Zr2O 12 The molar ratio of lithium hydroxide monohydrate (LiOH·H2O), gallium trioxide powder (Ga2O3), lanthanum trioxide powder (La2O3) and zirconium dioxide powder (ZrO2) were respectively weighed, and then an appropriate amount of ball milling beads and dispersion medium ethanol were added, and the mixture was ball milled at 300-400 rpm for 4-5 h. After ball milling, the mixture was dried at 80°C, and the dried mixture was pre-sintered in a muffle furnace at 950°C for 12 h, and then cooled to room temperature at a rate of 5°C / min to obtain a composite electrolyte powder.

[0066] (2) Preparation of solid electrolyte substrate

[0067] The above-mentioned composite electrolyte powder is placed in a mold and pressed into a circular sheet with a diameter of about 15 mm and a thickness of about 1 mm under 60 MPa conditions, and calcined in a muffle furnace at 1200°C for 12 hours. During the calcination process, a layer of mother powder is covered on the surface of the circular sheet to reduce lithium volatilization during the calcination process. After the calcination, it is cooled to room temperature at a rate of 5°C / min, and the surface is polished to obtain a solid electrolyte substrate.

[0068] (3) Sn-Li interface modification layer

[0069] The solid electrolyte substrate is fixed in a magnetron sputtering chamber, with a tin sheet as a target, the power of the magnetron sputtering is adjusted to 80W, the vacuum degree is 1Pa, and the sputtering time is controlled within 25 to 30s. At the same time, an argon atmosphere with a purity of 99.9% is introduced during the sputtering process. After the sputtering is completed, the temperature of the solid electrolyte substrate is heated to 400°C, the vacuum degree is adjusted to 2Pa, and then the lithium sheet is used as a target for sputtering. The sputtering time is 10 to 15s. After the sputtering is completed, it is cooled to room temperature to obtain a solid electrolyte.

[0070] Example 3: LTLZO solid electrolyte

[0071] The present embodiment provides a solid electrolyte and a preparation method thereof. The solid electrolyte of the present embodiment comprises a solid electrolyte matrix layer and a Sn-Li interface modification layer, wherein the solid electrolyte matrix layer is obtained by doping Ta at the Li position on the basis of a garnet-type electrolyte, i.e., Li 6.25 Ta 0.25 La3Zr2O 12 The thickness of the solid electrolyte matrix layer is about 1 mm, and the thickness of the Sn-Li interface modification layer is about 150 nm.

[0072] The method for preparing the solid electrolyte of this embodiment specifically comprises the following steps:

[0073] (1) Preparation of composite electrolyte powder

[0074] According to the chemical formula Li 6.25 Ta 0.25 La3Zr2O 12The molar ratio of lithium hydroxide monohydrate (LiOH·H2O), tantalum oxide powder (Ta2O5), lanthanum trioxide powder (La2O3) and zirconium dioxide powder (ZrO2) were respectively weighed, and then an appropriate amount of ball milling beads and a dispersion medium of isopropanol were added, and the mixture was ball milled at a speed of 300-400 rpm for 4-5 h. After ball milling, the mixture was dried at 80°C, and the dried mixture was pre-sintered in a muffle furnace at 950°C for 12 h, and then cooled to room temperature at a rate of 5°C / min to obtain a composite electrolyte powder.

[0075] (2) Preparation of solid electrolyte substrate

[0076] The above-mentioned composite electrolyte powder is placed in a mold and pressed into a circular sheet with a diameter of about 15 mm and a thickness of about 1 mm under 60 MPa conditions, and calcined in a muffle furnace at 1200°C for 12 hours. During the calcination process, a layer of mother powder is covered on the surface of the circular sheet to reduce lithium volatilization during the calcination process. After the calcination, it is cooled to room temperature at a rate of 5°C / min, and the surface is polished to obtain a solid electrolyte substrate.

[0077] (3) Sn-Li interface modification layer

[0078] The solid electrolyte substrate is fixed in a magnetron sputtering chamber, with a tin sheet as a target, the power of the magnetron sputtering is adjusted to 80W, the vacuum degree is 1Pa, and the sputtering time is controlled within 25 to 30s. At the same time, an argon atmosphere with a purity of 99.9% is introduced during the sputtering process. After the sputtering is completed, the temperature of the solid electrolyte substrate is heated to 400°C, the vacuum degree is adjusted to 2Pa, and then the lithium sheet is used as a target for sputtering. The sputtering time is 10 to 15s. After the sputtering is completed, it is cooled to room temperature to obtain a solid electrolyte.

[0079] Example 4: LALZO solid electrolyte

[0080] The present embodiment provides a solid electrolyte and a preparation method thereof. The solid electrolyte of the present embodiment comprises a solid electrolyte matrix layer and a Sn-Li interface modification layer, wherein the solid electrolyte matrix layer is obtained by doping Al at the Li position on the basis of a garnet-type electrolyte, i.e., Li 6.25 Al 0.25 La3Zr2O 12 The thickness of the solid electrolyte matrix layer is about 1 mm, and the thickness of the Sn-Li interface modification layer is about 100 nm.

[0081] The method for preparing the solid electrolyte of this embodiment specifically comprises the following steps:

[0082] (1) Preparation of composite electrolyte powder

[0083] According to the chemical formula Li 6.25 Al0.25 La3Zr2O 12 The molar ratio of lithium hydroxide monohydrate (LiOH·H2O), aluminum oxide powder (Al2O3), lanthanum trioxide powder (La2O3) and zirconium dioxide powder (ZrO2) were respectively weighed, and then an appropriate amount of ball milling beads and a dispersion medium of isopropanol were added, and the mixture was ball milled at a speed of 300-400 rpm for 4-5 h. After ball milling, the mixture was dried at 80°C, and the dried mixture was pre-sintered in a muffle furnace at 950°C for 12 h, and then cooled to room temperature at a rate of 5°C / min to obtain a composite electrolyte powder.

[0084] (2) Preparation of solid electrolyte substrate

[0085] The above-mentioned composite electrolyte powder is placed in a mold and pressed into a circular sheet with a diameter of about 15 mm and a thickness of about 1 mm under 60 MPa conditions, and calcined in a muffle furnace at 1250°C for 12 hours. During the calcination process, a layer of mother powder (i.e., the above-mentioned composite electrolyte powder) is covered on the surface of the circular sheet to reduce lithium volatilization during the calcination process. After the calcination is completed, it is cooled to room temperature at a rate of 5°C / min, and the surface is polished to obtain a solid electrolyte substrate.

[0086] (3) Sn-Li interface modification layer

[0087] The solid electrolyte substrate is fixed in a magnetron sputtering chamber, a tin sheet is used as a target, the power of the magnetron sputtering is adjusted to 80W, the vacuum degree is 1Pa, and the sputtering time is controlled within 15 to 20 seconds. At the same time, an argon atmosphere with a purity of 99.9% is introduced during the sputtering process. After the sputtering is completed, the temperature of the solid electrolyte substrate is heated to 400°C, the vacuum degree is adjusted to 2Pa, and then the lithium sheet is used as a target for sputtering. The sputtering time is 10 to 15 seconds. After the sputtering is completed, it is cooled to room temperature to obtain a solid electrolyte.

[0088] Comparative Example 1: LALZO solid electrolyte

[0089] This comparative example provides a solid electrolyte and a preparation method thereof, wherein the solid electrolyte is obtained by doping Al at the Li position on the basis of a garnet-type electrolyte, and has a thickness of about 1 mm. The preparation method of the solid electrolyte specifically comprises the following steps:

[0090] (1) Preparation of composite electrolyte powder

[0091] According to the chemical formula Li 6.25 Al 0.25 La3Zr2O 12The molar ratio of lithium hydroxide monohydrate (LiOH·H2O), aluminum oxide powder (Al2O3), lanthanum trioxide powder (La2O3) and zirconium dioxide powder (ZrO2) were respectively weighed, and then an appropriate amount of ball milling beads and a dispersion medium of isopropanol were added, and the mixture was ball milled at a speed of 300-400 rpm for 4-5 h. After ball milling, the mixture was dried at 80°C, and the dried mixture was pre-sintered in a muffle furnace at 950°C for 12 h, and then cooled to room temperature at a rate of 5°C / min to obtain a composite electrolyte powder.

[0092] (2) Preparation of solid electrolyte

[0093] The above-mentioned composite electrolyte powder is placed in a mold and pressed into a circular sheet with a diameter of about 15 mm and a thickness of about 1 mm under 60 MPa conditions, and calcined in a muffle furnace at 1250°C for 12 hours. During the calcination process, a layer of mother powder (i.e., the above-mentioned composite electrolyte powder) is covered on the surface of the circular sheet to reduce lithium volatilization during the calcination process. After the calcination is completed, it is cooled to room temperature at a rate of 5°C / min, and the surface is polished.

[0094] Comparative Example 2: LALZO solid electrolyte

[0095] This comparative example provides a solid electrolyte and a preparation method thereof, wherein the solid electrolyte comprises a solid electrolyte matrix layer and a Sn-Li interface modification layer, wherein the solid electrolyte matrix layer is a garnet-type electrolyte matrix layer (i.e., LLZO) with a thickness of about 1 mm, and the Sn-Li interface modification layer has a thickness of about 150 nm.

[0096] The preparation method of the solid electrolyte of this comparative example specifically comprises the following steps:

[0097] (1) Preparation of composite electrolyte powder

[0098] According to the chemical formula Li7La3Zr2O 12 The molar ratio of lithium hydroxide monohydrate (LiOH·H2O), lanthanum trioxide powder (La2O3) and zirconium dioxide powder (ZrO2) were respectively weighed, and then an appropriate amount of ball milling beads and a dispersion medium of isopropanol were added, and the mixture was ball milled at a speed of 300-400 rpm for 4-5 h. After ball milling, the mixture was dried at 80°C, and the dried mixture was pre-sintered in a muffle furnace at 950°C for 12 h, and then cooled to room temperature at a rate of 5°C / min to obtain a composite electrolyte powder.

[0099] (2) Preparation of solid electrolyte substrate

[0100] The above-mentioned composite electrolyte powder is placed in a mold and pressed into a circular sheet with a diameter of about 15 mm and a thickness of about 1 mm under 60 MPa conditions, and calcined in a muffle furnace at 1250°C for 12 hours. During the calcination process, a layer of mother powder (i.e., the above-mentioned composite electrolyte powder) is covered on the surface of the circular sheet to reduce lithium volatilization during the calcination process. After the calcination is completed, it is cooled to room temperature at a rate of 5°C / min, and the surface is polished to obtain a solid electrolyte substrate.

[0101] (3) Sn-Li interface modification layer

[0102] The solid electrolyte substrate is fixed in a magnetron sputtering chamber, with a tin sheet as a target, the power of the magnetron sputtering is adjusted to 80W, the vacuum degree is 1Pa, and the sputtering time is controlled within 25 to 30s. At the same time, an argon atmosphere with a purity of 99.9% is introduced during the sputtering process. After the sputtering is completed, the temperature of the solid electrolyte substrate is heated to 400°C, the vacuum degree is adjusted to 2Pa, and then the lithium sheet is used as a target for sputtering. The sputtering time is 10 to 15s. After the sputtering is completed, it is cooled to room temperature to obtain a solid electrolyte.

[0103] Comparative Example 3: LALZO solid electrolyte

[0104] This comparative example provides a solid electrolyte and a preparation method thereof. The solid electrolyte of this comparative example comprises a solid electrolyte matrix layer and an Al2O3 interface modification layer, wherein the solid electrolyte matrix layer is obtained by doping Al at the Li position on the basis of a garnet-type electrolyte, i.e., Li 6.25 Al 0.25 La3Zr2O 12 The thickness of the solid electrolyte matrix layer is about 1 mm, and the thickness of the Al2O3 interface modification layer is about 150 nm.

[0105] The preparation method of the solid electrolyte of this comparative example specifically comprises the following steps:

[0106] (1) Preparation of composite electrolyte powder

[0107] According to the chemical formula Li 6.25 Al 0.25 La3Zr2O 12 The molar ratio of lithium hydroxide monohydrate (LiOH·H2O), aluminum oxide powder (Al2O3), lanthanum trioxide powder (La2O3) and zirconium dioxide powder (ZrO2) were respectively weighed, and then an appropriate amount of ball milling beads and a dispersion medium of isopropanol were added, and the mixture was ball milled at a speed of 300-400 rpm for 4-5 h. After ball milling, the mixture was dried at 80°C, and the dried mixture was pre-sintered in a muffle furnace at 950°C for 12 h, and then cooled to room temperature at a rate of 5°C / min to obtain a composite electrolyte powder.

[0108] (2) Preparation of solid electrolyte substrate

[0109] The composite electrolyte powder is placed in a mold, pressed into a circular sheet with a diameter of about 15 mm and a thickness of about 1 mm under 60 MPa, and calcined in a muffle furnace at 1250° C. for 12 hours. During the calcination process, a layer of mother powder (i.e., the composite electrolyte powder) is covered on the surface of the circular sheet to reduce lithium volatilization during the calcination process. After the calcination is completed, it is cooled to room temperature at a rate of 5° C. / min, and the surface is polished to obtain a solid electrolyte substrate;

[0110] (3) Al2O3 interface modification layer

[0111] The above-mentioned solid electrolyte substrate was fixed in a magnetron sputtering chamber, with aluminum sheet as the target material, the power of magnetron sputtering was adjusted to 80W, the vacuum degree was 1Pa, the sputtering time was controlled within 40-45s, and an argon atmosphere with a purity of 99.9% was introduced during the sputtering process. After the sputtering was completed, the solid electrolyte substrate containing the Al layer was placed in 60°C hot water for oxidation reaction, taken out after 24 hours, and then placed in a 120°C vacuum oven for drying for 12 hours, and cooled to room temperature to obtain a solid electrolyte.

[0112] Comparative Example 4: LALZO solid electrolyte

[0113] The present comparative example provides a solid electrolyte and a preparation method thereof. The solid electrolyte of the present comparative example comprises a solid electrolyte matrix layer, a Sn metal layer and a Li metal layer, wherein the solid electrolyte matrix layer is obtained by doping Al at the Li position on the basis of a garnet-type electrolyte, i.e., Li 6.25 Al 0.25 La3Zr2O 12 The solid electrolyte matrix layer has a thickness of about 1 mm, the Sn metal layer has a thickness of about 100 nm, and the Li metal layer has a thickness of about 50 nm.

[0114] The preparation method of the solid electrolyte of this comparative example specifically comprises the following steps:

[0115] (1) Preparation of composite electrolyte powder

[0116] According to the chemical formula Li 6.25 Al 0.25 La3Zr2O 12The molar ratio of lithium hydroxide monohydrate (LiOH·H2O), aluminum oxide powder (Al2O3), lanthanum trioxide powder (La2O3) and zirconium dioxide powder (ZrO2) were respectively weighed, and then an appropriate amount of ball milling beads and a dispersion medium of isopropanol were added, and the mixture was ball milled at a speed of 300-400 rpm for 4-5 h. After ball milling, the mixture was dried at 80°C, and the dried mixture was pre-sintered in a muffle furnace at 950°C for 12 h, and then cooled to room temperature at a rate of 5°C / min to obtain a composite electrolyte powder.

[0117] (2) Preparation of solid electrolyte substrate

[0118] The composite electrolyte powder is placed in a mold, pressed into a circular sheet with a diameter of about 15 mm and a thickness of about 1 mm under 60 MPa, and calcined in a muffle furnace at 1250° C. for 12 hours. During the calcination process, a layer of mother powder (i.e., the composite electrolyte powder) is covered on the surface of the circular sheet to reduce lithium volatilization during the calcination process. After the calcination is completed, it is cooled to room temperature at a rate of 5° C. / min, and the surface is polished to obtain a solid electrolyte substrate;

[0119] (3) Preparation of Sn metal layer and Li metal layer

[0120] The solid electrolyte substrate is fixed in a magnetron sputtering chamber, with a tin sheet as the target material, the power of the magnetron sputtering is adjusted to 80 W, the vacuum degree is 1 Pa, and the sputtering time is controlled within 25 to 30 s. At the same time, an argon atmosphere with a purity of 99.9% is introduced during the sputtering process. After the sputtering is completed, the target tin sheet is replaced with a lithium sheet, and the sputtering time is 10 to 15 s. After the sputtering is completed, it is cooled to room temperature to obtain a solid electrolyte.

[0121] Test example 1: Ionic conductivity test

[0122] This test example performs electrochemical impedance spectroscopy test on the solid electrolytes prepared in the above-mentioned Examples 1 to 4 and Comparative Examples 1 to 4 by assembling blocking electrodes to obtain the ionic conductivity of the solid electrolytes, which includes the following steps:

[0123] First, stainless steel sheets were used as blocking electrodes on both sides of the prepared inorganic oxide solid electrolyte sheet to form a symmetrical battery, in which the frequency range was 0.01 to 10 6 Hz, test the EIS of solid electrolyte sheet at 25°C. The ionic conductivity of solid electrolyte is calculated as follows:

[0124] δ = L / (R·S);

[0125] Where δ is the ionic conductivity, in S / cm; L is the thickness of the solid electrolyte sheet, in cm; R is the intrinsic resistance of the solid electrolyte, in Ω; S is the effective cross-sectional area of ​​the solid electrolyte sheet, in cm 2 The test results are shown in Table 1.

[0126] Table 1: Ionic conductivity test results

[0127]

[0128]

[0129] From the above results, it can be seen that the solid electrolyte prepared in the embodiment of the present invention has excellent ionic conductivity. When the Li-doped element is Al, Ga or Ta and a Sn-Li interface modification layer is used, a higher ionic conductivity of about 5.65×10 -3 ~6.52×10 -3 S / cm.

[0130] Compared with Example 1, the solid electrolyte prepared in Comparative Example 1 does not contain a Sn-Li interface modification layer, and the Li position of the solid electrolyte prepared in Comparative Example 2 is not doped with other elements. The results show that it has a lower ionic conductivity than that of Example 1, which is presumably related to the Li + The Sn-Li interface modification layer helps to improve the Li + The uniform distribution at the interface improves the wettability of the LLZO-based electrolyte interface and reduces the interface impedance.

[0131] Compared with Example 1, Comparative Example 3 replaces the Sn-Li interface modification layer in the solid electrolyte with an Al2O3 interface modification layer. The results show that its ionic conductivity decreases, which is presumably related to the conductivity of the interface modification layer; while Comparative Example 4 replaces the Sn metal layer and the Li metal layer in the solid electrolyte with the Sn-Li interface modification layer. The results show that it is not conducive to improving the ionic conductivity. This is mainly because the superposition of a single Sn metal layer and a Li metal layer reduces the interface contact, and during the preparation of the Sn-Li interface modification layer (composite layer), the Li metal layer melts into the Sn metal layer, so that the gaps between the Sn metal layer particles are filled and compacted by the Li metal, thereby improving the contact between the two, thereby reducing the interface resistance, and the ionic conductivity is relatively higher.

[0132] Test Example 2: Cyclic Performance Test

[0133] This test example tests the cycle performance of batteries made of solid electrolytes prepared in the above Examples 1 to 4 and Comparative Examples 1 to 4. The specific test method is as follows:

[0134] Firstly, lithium cobalt oxide, conductive agent Super P, and binder PVDF were mixed in a ratio of 9:0.5:0.5, and an appropriate amount of solvent NMP was added and stirred to prepare a positive electrode slurry, which was coated on an aluminum foil. After drying at 100°C, the slurry was cut into discs with a diameter of 10 mm as the positive electrode. Then the obtained solid electrolyte sheets were assembled into CR2032 button cells in the order of positive electrode sheet-solid electrolyte sheet-lithium foil, in which the Sn-Li interface modification layer was in contact with the lithium foil, and the battery cycle performance was tested.

[0135] During the cycle performance test, the battery was operated at a temperature of 30°C, with an operating voltage range of 3V to 4.2V and a current density of 0.15 mA / cm 2 ) was charged to 4.2V and then to 0.05C for 300 cycles. The test results are shown in Table 2.

[0136] Table 2: Cycle performance test results

[0137]

[0138]

[0139] From the above test results, it can be seen that the solid electrolyte prepared in the embodiment of the present invention has excellent cycle performance. After 500 cycles, its capacity retention rate is still above 94%. Compared with Example 1, Comparative Example 1 is not modified with the Sn-Li composite layer. The results show that its cycle performance is significantly reduced, indicating that the Sn-Li interface modification layer helps to improve the cycle stability, which is presumably related to the improvement of interface wettability and the reduction of interface resistance.

[0140] In summary, the present invention provides a solid electrolyte and a preparation method and application thereof. The solid electrolyte of the present invention comprises a solid electrolyte matrix layer and a Sn-Li interface modification layer, wherein the solid electrolyte matrix layer is obtained by doping elements at the Li position on the basis of a garnet-type electrolyte. In the process of preparing the solid electrolyte, the present invention combines element doping and interface modification. The preparation method is simple. The prepared solid electrolyte not only has high ionic conductivity, but also has a Sn-Li interface modification layer at 5.65×10 -3 ~6.52×10 -3 S / cm, and has excellent cycle performance.

[0141] The above is a detailed description of the embodiments of the present invention, but the present invention is not limited to the above embodiments. Various changes can be made within the knowledge of ordinary technicians in the relevant technical field without departing from the purpose of the present invention. In addition, the embodiments of the present invention and the features in the embodiments can be combined with each other without conflict.

Claims

1. A solid electrolyte, characterized in that include: Solid electrolyte matrix layer, the structural expression of the solid electrolyte matrix layer is Li 7-3x M x La3Zr2O 12 , wherein 0<x≤0.3, the M element is selected from any one of Al, Ga and Ta; The Sn-Li alloy layer is deposited on the surface of the solid electrolyte matrix layer.

2. The solid electrolyte according to claim 1, characterized in that The deposition method is magnetron sputtering.

3. The solid electrolyte according to claim 1, characterized in that The thickness of the Sn-Li alloy layer is 50-200 nm.

4. The method for preparing a solid electrolyte according to any one of claims 1 to 3, characterized in that: The following steps are involved: S1. According to the molar ratio of the structural expression of the solid electrolyte matrix layer of claim 1, a lithium source, lanthanum trioxide, zirconium dioxide and an oxide of the M element are mixed, and pre-sintered at 900-980° C. to obtain a composite electrolyte powder; S2, molding the composite electrolyte powder, and calcining it at 1100-1300° C. to obtain a solid electrolyte substrate; S3, fixing the solid electrolyte substrate in a magnetron sputtering chamber, performing magnetron sputtering with metal tin as a target, and then performing magnetron sputtering with metal lithium as a target under heating conditions to deposit the Sn-Li alloy layer on the solid electrolyte substrate.

5. The preparation method according to claim 4, characterized in that: The pre-sintering time is 10 to 18 hours.

6. The preparation method according to claim 4, characterized in that: The compression molding pressure is 50-100 MPa; And / or, the calcination time is 10 to 18 hours.

7. The preparation method according to any one of claims 4 to 6, characterized in that: During the magnetron sputtering process, when the metal tin is used as the target material, the vacuum degree is 0.8-1.2 Pa; And / or, during the magnetron sputtering process, when the metallic lithium is used as the target material, the vacuum degree is 1.8 to 2.5 Pa; And / or, during the magnetron sputtering process, when the metallic lithium is used as the target material, the heating temperature is 350-450°C.

8. The preparation method according to claim 7, characterized in that: The power of the magnetron sputtering is 60-100W, and / or the atmosphere of the magnetron sputtering is an inert atmosphere.

9. A lithium ion battery, characterized in that: The solid electrolyte comprises the solid electrolyte according to any one of claims 1 to 3, wherein the Sn-Li alloy layer of the solid electrolyte is arranged on a side close to the lithium metal negative electrode.

10. Use of the solid electrolyte according to any one of claims 1 to 3 or the method for preparing the solid electrolyte according to any one of claims 4 to 8 in preparing energy storage materials.

Citation Information

Cited By

  • Garnet type solid electrolyte with interface modification layer, preparation method and application of garnet type solid electrolyte in lithium metal symmetric battery