Ceramic diaphragm, preparation method thereof and lithium ion battery
By adding high-temperature-resistant polymer nanofibers and ceramic particles to the ceramic separator to form a porous network structure, the problem of melting, shrinkage and pulverization of the lithium-ion battery separator at high temperatures is solved, and the thermal stability and safety of the battery are improved.
Patent Information
- Application Number
- CN202410899292.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-05
- Publication Date
- 2024-10-15
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing lithium-ion battery separators tend to melt, shrink, pulverize and break under high temperatures, resulting in insufficient battery safety and unable to meet the heat resistance and thermal dimensional stability requirements of large-capacity and high-specific-energy lithium-ion batteries.
High-temperature-resistant polymer nanofibers and ceramic particles are added to the ceramic coating to form a porous network structure to form a continuous self-supporting ceramic coating, which improves the thermal stability and mechanical properties of the ceramic diaphragm and prevents the ceramic particles from being pulverized and broken.
It significantly improves the temperature resistance and battery safety of the ceramic separator, reduces the risk of short circuits caused by shrinkage at high temperatures, and extends the service life.
Smart Images

Figure BDA0004930038350000081 
Figure BDA0004930038350000091
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of battery diaphragms, and in particular to a ceramic diaphragm and a preparation method thereof, and a lithium ion battery. Background Art
[0002] At present, lithium-ion batteries generally use polyolefin separators. However, due to their poor thermal stability, polyolefin separators are prone to melting and shrinking at high temperatures above 120°C, causing contact between the positive and negative electrodes. Under conditions of overcharge, over-discharge, rapid charge and discharge, abuse or high temperature, the separator can easily melt and break, causing a short circuit in the battery and triggering thermal runaway, leading to battery fire and explosion, and cannot meet the strict safety requirements of large-capacity and high-energy-density lithium-ion batteries.
[0003] Inorganic particles such as ceramics have excellent heat resistance, wettability, and non-flammable and non-melting intrinsic properties. Therefore, people prepare inorganic particles such as alumina, silicon oxide, boehmite, and other additives such as binders and solvents into ceramic slurries, which are coated on one or both sides of the polyolefin base film, and develop ceramic diaphragms with inorganic ceramic particles coated with modified polyolefin diaphragms. Although the temperature resistance of ceramic diaphragms has been significantly improved, and the excellent mechanical properties of the base film have been maintained, with the advancement of battery technology and the continuous improvement of material requirements, polyolefin diaphragms modified by ceramic coatings have also shown many problems and application bottlenecks. The biggest problem is that the powdery accumulation structure of particles in the ceramic coating cannot form a continuous self-supporting structure by itself, so it usually shows problems such as easy powder loss and coating shedding during use. More importantly, ceramic diaphragms generally experience pulverization and crushing of ceramic particles at high temperatures, which leads to the collapse of the diaphragm, and cannot suppress the occurrence of thermal runaway, and cannot meet the requirements of lithium-ion batteries for high heat resistance and high thermal dimensional stability of the diaphragm. Summary of the invention
[0004] Based on the technical problems existing in the background technology, the present invention proposes a ceramic diaphragm, a preparation method thereof and a lithium-ion battery. The ceramic diaphragm includes a base membrane and a ceramic coating. The ceramic coating contains high-temperature resistant polymer nanofibers, which can form a more solid composite structure with ceramic particles, thereby giving the ceramic diaphragm better thermal stability, mechanical properties and service life.
[0005] The present invention provides a ceramic diaphragm, which comprises a base film and a ceramic coating attached to at least one side surface of the base film;
[0006] The ceramic coating comprises ceramic particles, a binder and high temperature resistant polymer nanofibers, and the mass ratio thereof is 100:1-10:2-15.
[0007] In the present invention, the ceramic coating is formed by ceramic particles, a binder and high-temperature resistant polymer nanofibers. The high-temperature resistant polymer nanofibers and the ceramic particles are compounded to form a porous network structure, so that the ceramic coating as a whole has the characteristics of continuous self-support, thereby ensuring that the ceramic coating maintains good integrity under high temperature and melting of the base film, does not break or pulverize, exhibits more excellent thermal stability and mechanical properties, and avoids the high-temperature pulverization and pulverization problem of the ceramic coating formed by simple ceramic particles, thereby significantly improving the temperature resistance of the ceramic diaphragm and the battery safety.
[0008] Preferably, the ceramic particles are at least one of aluminum oxide, silicon oxide, titanium oxide, zirconium oxide, barium oxide, boehmite, magnesium oxide and magnesium hydroxide;
[0009] Preferably, the particle size of the ceramic particles is 0.01-5 μm.
[0010] Preferably, the binder is polyamic acid lithium salt, which is obtained by reacting polyamic acid with lithium hydroxide to form a salt;
[0011] Preferably, the mass ratio of the polyamic acid to lithium hydroxide is 1:0.01-0.05.
[0012] In the present invention, since the aromatic polymer chain in the polyamic acid lithium salt has excellent temperature resistance and the amide group contained has excellent adhesion, and the lithium salt not only has a certain ion conductivity, but also ensures that this type of binder can obtain an excellent ceramic coating in water-based ceramic coating, polyamic acid lithium salt is selected as a binder to form a ceramic coating, which can not only improve the adhesion between the ceramic coating and the base film, but also make the obtained ceramic coating further have better heat resistance, thereby reducing the risk of short circuit caused by shrinkage of the composite diaphragm containing the ceramic coating at high temperature, and greatly improving the safety of the diaphragm.
[0013] Preferably, the polyamic acid is obtained by polycondensation of aromatic dianhydride and aromatic diamine;
[0014] Preferably, the aromatic dianhydride is one of pyromellitic dianhydride, 3,3',4,4'-biphenyltetracarboxylic dianhydride, 3,3',4,4'-benzophenonetetracarboxylic dianhydride, 2,3,3',4'-diphenyl ether tetracarboxylic dianhydride or 4,4'-(hexafluoroisopropylene) diphthalic anhydride; the aromatic diamine is one of p-phenylenediamine 4,4'-diaminodiphenyl ether, 4,4'-diaminodiphenylmethane, 4,4'-diaminodiphenyl sulfone, 4,4'-diaminobenzophenone or 2,2'-bis(trifluoromethyl)-4,4'-diaminobiphenyl.
[0015] Preferably, the high temperature resistant polymer nanofiber is at least one of aramid nanofiber, polyimide nanofiber or polyamide-imide nanofiber.
[0016] Preferably, the surface of the high temperature resistant polymer nanofiber contains ammonium salt groups;
[0017] Preferably, the high temperature resistant polymer nanofiber is an aramid fiber having amino and carboxyl groups on the surface.
[0018] In the present invention, although the presence of high-temperature resistant polymer nanofibers can further improve the heat resistance of the ceramic coating, there is a lack of interaction between the nanofibers, and their bonding strength is completely dependent on the binder. If the binder cannot provide sufficient bonding strength for the nanofibers, it cannot provide support for the ceramic coating. The inventors of the present invention select high-temperature resistant polymer nanofibers containing ammonium salt groups on the surface, which can form electrostatic attraction with the aforementioned polyamic acid lithium salt, thereby giving sufficient bonding force between the nanofibers and the ceramic particles, forming a more stable ceramic coating structure, which can not only increase the bonding strength of the entire ceramic coating, but also will not affect the air permeability of the ceramic coating.
[0019] Preferably, the aramid fiber having amino and carboxyl groups on the surface is obtained by immersing the aramid fiber in an alkaline alcohol solution for reaction;
[0020] Preferably, the aramid fiber has a diameter of 50-150 nm and an aspect ratio of 2000-5000.
[0021] Preferably, the base film is at least one of a polypropylene microporous film, a polyethylene microporous film or a polypropylene / polyethylene microporous film;
[0022] Preferably, the base film has a thickness of 5-50 μm, and the ceramic coating has a thickness of 1-10 μm.
[0023] The present invention also proposes a method for preparing the above-mentioned ceramic diaphragm, comprising: coating a ceramic slurry comprising ceramic particles, a binder and high-temperature resistant polymer nanofibers on at least one surface of a base membrane, and drying to form a ceramic coating to obtain the ceramic diaphragm.
[0024] The present invention also provides a lithium ion battery, which comprises the ceramic diaphragm.
[0025] The present invention mixes ceramic particles, a binder and high-temperature resistant polymer nanofibers to obtain a ceramic slurry which is then coated on the surface of the base membrane body. The resulting ceramic diaphragm after curing has good thermal stability, puncture resistance, and mechanical strength, effectively solving the problems of poor thermal stability and poor puncture resistance in existing diaphragms. At the same time, the ceramic diaphragm prepared by the present invention also has excellent cyclic stability and safety performance. DETAILED DESCRIPTION
[0026] The technical solutions of the present invention are described in detail below through specific embodiments. However, it should be clearly stated that these embodiments are for illustration only and are not to be construed as limiting the scope of the present invention.
[0027] Example 1
[0028] A ceramic diaphragm is prepared by the following method:
[0029] (1) under nitrogen protection, 4,4'-diaminodiphenyl ether is added to N-methylpyrrolidone (NMP) and stirred to dissolve completely, then 3,3',4,4'-biphenyltetracarboxylic acid dianhydride is added in an amount equal to the molar amount of 4,4'-diaminodiphenyl ether, and stirred for reaction for 10 hours to obtain a polyamic acid solution; lithium hydroxide (LiOH) of 3 wt% by weight of the polyamic acid is added to deionized water and dissolved completely, and the obtained lithium hydroxide aqueous solution is added to the polyamic acid solution, and stirred for reaction for 5 hours to obtain a polyamic acid lithium salt solution; the polyamic acid lithium salt solution is added to acetone for precipitation, filtered, washed, and dried to obtain a polyamic acid lithium salt;
[0030] (2) Add the above-mentioned polyamic acid lithium salt into water and stir and disperse it evenly, then add alumina powder (average particle size is 0.5 μm) with a mass of 25 times that of the polyamic acid lithium salt and aramid nanofiber (aramid 1414 fiber, average diameter is 0.06 μm) with a mass of 2.5 times that of the polyamic acid lithium salt, stir and disperse evenly at a rate of 2000 r / min to obtain a ceramic slurry (solid content is 30 wt%); put the ceramic slurry into a vacuum oven for 1 hour to complete defoaming, and then use a gravure roller coating method to coat it on one surface of a polyethylene single-layer diaphragm (thickness is 12 μm, porosity is 45%) to form a ceramic coating, the thickness of the ceramic coating is controlled to be 4 μm, and after drying at 60°C, the lithium ion battery composite diaphragm is obtained.
[0031] Example 2
[0032] A ceramic diaphragm, the operation is the same as that of Example 1, except that in step (1), p-phenylenediamine is used instead of 4,4'-diaminodiphenyl ether, and pyromellitic acid dianhydride is used instead of 3,3',4,4'-biphenyltetracarboxylic acid dianhydride; in step (2), polyimide nanofiber is used instead of aramid nanofiber, and the polyimide nanofiber is prepared by the following method: under nitrogen protection, p-phenylenediamine is added to N,N-dimethylacetamide (DMF) and stirred to dissolve completely, then an equal molar amount of 3,3',4,4'-biphenyltetracarboxylic acid dianhydride is added to p-phenylenediamine, and stirred to react. After 6 hours, a polyamic acid solution with a solid content of 15wt% is obtained; after filtering and vacuum degassing, it is used as a spinning stock solution and added into a closed storage tank of a high-voltage electrospinning device, and electrospinning is performed under the conditions of a spinning temperature of room temperature, a humidity of 60%, an output voltage of a high-voltage power supply of 20KV, and a distance of 20cm between a receiving screen and a single electrode to obtain polyamic acid nanofibers, and then subjected to a gradient heating thermal imidization treatment (the thermal imidization temperature is 50-450°C, and the heating rate is 15°C / min) to obtain the polyimide nanofibers (with an average diameter of 0.06μm).
[0033] Example 3
[0034] A ceramic diaphragm, the operation is the same as that of Example 1, except that in step (1), 2,3,3',4'-diphenyl ether tetracarboxylic dianhydride is used instead of 3,3',4,4'-biphenyl tetracarboxylic dianhydride; in step (2), polyamide-imide nanofiber is used instead of aramid nanofiber, and the polyamide-imide nanofiber is prepared by the following method: under nitrogen protection, p-phenylenediamine is added to N,N-dimethylacetamide (DMF) and stirred to dissolve completely, then an equal molar amount of p-phenylenediamine and a molar amount of 1. 5 times of pyridine catalyst, stirring and reacting for 24 hours, adding acetic anhydride as a dehydrating agent in an equal molar amount of p-phenylenediamine, and continuing to stir and react for 24 hours to obtain a polyamide-imide solution with a solid content of 10wt%; filtering, vacuum degassing and using it as a spinning stock solution, adding it to a closed storage tank of a high-voltage electrospinning device, and electrospinning is carried out under the conditions of a spinning temperature of room temperature, a humidity of 60%, an output voltage of a high-voltage power supply of 20KV, and a distance of 20cm between a receiving screen and a single electrode to obtain the polyamide-imide nanofibers (with an average diameter of 0.06μm).
[0035] Example 4
[0036] A ceramic diaphragm, the operation is the same as that of Example 1, except that silicon dioxide powder is used instead of aluminum oxide powder in step (3).
[0037] Example 5
[0038] A ceramic diaphragm, the operation is the same as that of Example 1, except that zirconium dioxide powder is used instead of aluminum oxide powder in step (3).
[0039] Example 6
[0040] A ceramic diaphragm is prepared by the following method:
[0041] (1) under nitrogen protection, 4,4'-diaminodiphenyl ether is added to N-methylpyrrolidone (NMP) and stirred to dissolve completely, then 3,3',4,4'-biphenyltetracarboxylic acid dianhydride is added in an amount equal to the molar amount of 4,4'-diaminodiphenyl ether, and stirred for reaction for 10 hours to obtain a polyamic acid solution; lithium hydroxide (LiOH) of 3 wt% by weight of the polyamic acid is added to deionized water and dissolved completely, and the obtained lithium hydroxide aqueous solution is added to the polyamic acid solution, and stirred for reaction for 5 hours to obtain a polyamic acid lithium salt solution; the polyamic acid lithium salt solution is added to acetone for precipitation, filtered, washed, and dried to obtain a polyamic acid lithium salt;
[0042] (2) adding aramid nanofibers (aramid 1414 fibers, with an average diameter of 0.06 μm) to an ethanol solution (solid content of 10 wt%) containing sodium hydroxide, and shaking the solution at 70° C. for 6 h. After the reaction, washing and drying were performed to obtain aramid fibers having amino and carboxyl groups on the surface.
[0043] (3) Add the above-mentioned polyamic acid lithium salt into water and stir and disperse it evenly, then add alumina powder (average particle size is 0.5 μm) with a mass of 25 times of the polyamic acid lithium salt and aramid fiber with amino and carboxyl groups on the surface with a mass of 2.5 times of the polyamic acid lithium salt, stir and disperse evenly at a rate of 2000 r / min to obtain a ceramic slurry (solid content is 30 wt%); put the ceramic slurry into a vacuum oven for 1 hour to complete defoaming, and then use a gravure roller coating method to coat it on one surface of a polyethylene single-layer diaphragm (thickness is 12 μm, porosity is 45%) to form a ceramic coating, the thickness of the ceramic coating is controlled to 4 μm, and after drying at 60°C, the lithium ion battery composite diaphragm is obtained.
[0044] Comparative Example 1
[0045] A ceramic diaphragm, the operation is the same as that of Example 1, omitting step (1), and the difference in step (3) is that a water-based polyacrylate binder (BYK-381) is used instead of polyamic acid lithium salt.
[0046] Performance Testing:
[0047] The ceramic diaphragms obtained in the above examples and comparative examples were tested for mechanical properties, thermal shrinkage, bonding strength and battery performance, and the test results are shown in Table 1.
[0048] Mechanical properties: Use an electronic universal testing machine to stretch a ceramic diaphragm of a certain size and shape, and record its tensile strength; use an electronic universal testing machine to pierce a ceramic diaphragm of a certain size and shape, and record its piercing strength;
[0049] Thermal shrinkage rate: Before baking the ceramic diaphragm, measure the longitudinal (MD) and transverse (TD) dimensions, record them as L1 and H1 respectively. Then bake the ceramic diaphragm at 130°C for 1h, measure the MD and TD dimensions again, record them as L2 and H2 respectively. The MD thermal shrinkage rate is (L1-L2) / L1×100%, and the TD thermal shrinkage rate is (H1-H2) / H1×100%;
[0050] Peel strength: Use 3M tape to stick the ceramic diaphragm on the side with ceramic coating, then fix the ceramic diaphragm between two steel plate clamps, use an electronic universal tensile testing machine to reversely stretch the ceramic coating and base film 180 degrees to peel off, and record the peel strength;
[0051] Battery performance: The obtained composite diaphragm is mixed with positive electrode sheet (lithium cobalt oxide, conductive agent acetylene black, and polyvinylidene fluoride are mixed in N-methylpyrrolidone solvent in a mass ratio of 97:1:2 to form positive electrode slurry, coated on aluminum foil and dried, and then cold pressed and striped to form positive electrode sheet), negative electrode sheet (graphite, conductive carbon black SuperP, and styrene-butadiene rubber are mixed in deionized water in a mass ratio of 97:1:2 to form negative electrode slurry, coated on copper foil and dried, and then cold pressed and striped to form negative electrode sheet) and 1 mol / L lithium hexafluorophosphate electrolyte (lithium hexafluorophosphate LiPF 6 The electrolyte was prepared by dissolving in a mixed solvent consisting of ethylene carbonate EC, dimethyl carbonate DMC and ethyl methyl carbonate EMC in a volume ratio of 1:1:1) and assembling into a lithium-ion battery in a conventional manner, and then performing a battery performance test. Specifically, the battery was charged to 4.35V at a constant current and constant voltage of 1C, the battery was cut off at 0.1C, left for 10 minutes, and cycled 200 times, and the capacity retention rate of 200 times was recorded;
[0052] Table 1 Performance test results of the battery separators described in Examples and Comparative Examples
[0053]
[0054]
[0055] It can be seen from the above table that the ceramic diaphragm described in the embodiment has better thermal stability, mechanical properties and service life.
[0056] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.
Claims
1. A ceramic diaphragm, characterized in that: The ceramic diaphragm comprises a base film and a ceramic coating attached to at least one side surface of the base film; The ceramic coating comprises ceramic particles, a binder and high temperature resistant polymer nanofibers, and the mass ratio thereof is 100:1-10:2-15.
2. The ceramic diaphragm according to claim 1, characterized in that: The ceramic particles are at least one of aluminum oxide, silicon oxide, titanium oxide, zirconium oxide, barium oxide, boehmite, magnesium oxide and magnesium hydroxide; Preferably, the particle size of the ceramic particles is 0.01-5 μm.
3. The ceramic diaphragm according to claim 1 or 2, characterized in that: The binder is polyamic acid lithium salt, which is obtained by reacting polyamic acid with lithium hydroxide to form a salt; Preferably, the mass ratio of the polyamic acid to lithium hydroxide is 1:0.01-0.
05.
4. The ceramic diaphragm according to claim 3, characterized in that: The polyamic acid is obtained by polycondensation of aromatic dianhydride and aromatic diamine; Preferably, the aromatic dianhydride is one of pyromellitic dianhydride, 3,3',4,4'-biphenyltetracarboxylic dianhydride, 3,3',4,4'-benzophenonetetracarboxylic dianhydride, 2,3,3',4'-diphenyl ether tetracarboxylic dianhydride or 4,4'-(hexafluoroisopropylene) diphthalic anhydride; the aromatic diamine is one of p-phenylenediamine 4,4'-diaminodiphenyl ether, 4,4'-diaminodiphenylmethane, 4,4'-diaminodiphenyl sulfone, 4,4'-diaminobenzophenone or 2,2'-bis(trifluoromethyl)-4,4'-diaminobiphenyl.
5. The ceramic diaphragm according to any one of claims 1 to 4, characterized in that: The high temperature resistant polymer nanofiber is at least one of aramid nanofiber, polyimide nanofiber or polyamide-imide nanofiber.
6. The ceramic diaphragm according to claim 5, characterized in that: The surface of the high temperature resistant polymer nanofiber contains ammonium salt groups; Preferably, the high temperature resistant polymer nanofiber is an aramid fiber having amino and carboxyl groups on the surface.
7. The ceramic diaphragm according to claim 6, characterized in that: The aramid fiber having amino and carboxyl groups on the surface is obtained by immersing the aramid fiber in an alkaline alcohol solution for reaction; Preferably, the aramid fiber has a diameter of 50-150 nm and an aspect ratio of 2000-5000.
8. The ceramic diaphragm according to any one of claims 1 to 7, characterized in that: The base film is at least one of a polypropylene microporous film, a polyethylene microporous film or a polypropylene / polyethylene microporous film; Preferably, the base film has a thickness of 5-50 μm, and the ceramic coating has a thickness of 1-10 μm.
9. A method for preparing the ceramic diaphragm according to any one of claims 1 to 8, characterized in that: The preparation method comprises: coating a ceramic slurry comprising ceramic particles, a binder and high temperature resistant polymer nanofibers on at least one surface of a base film, and drying the slurry to form a ceramic coating, thereby obtaining the ceramic diaphragm.
10. A lithium ion battery, characterized in that: The lithium-ion battery comprises the ceramic separator according to any one of claims 1 to 8.
Citation Information
Patent Citations
Silicon-carbon negative electrode for lithium ion battery and lithium ion battery
CN113555535A
Adhesive for silicon-carbon negative electrode and electrode material for lithium ion battery
CN113555551A
Modified composite diaphragm and preparation method thereof
CN116315437A
Cited By
High-temperature-resistant composite diaphragm for lithium ion battery and preparation method of high-temperature-resistant composite diaphragm
CN118899623A
Diaphragm and preparation method thereof, battery, battery pack and electric equipment
CN121416765A