MEMS piezoelectric generator and its fabrication method
By employing a rectangular bridge diaphragm structure and a flexible material covering the slotted structure in the MEMS piezoelectric generator, the problem of balancing small size and high sound pressure level output is solved, improving sound quality and sound pressure level, and enhancing the frequency response curve.
Patent Information
- Application Number
- CN202410749659.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-11
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2044-06-11
AI Technical Summary
Existing MEMS piezoelectric generators struggle to balance small size with high sound pressure level output, and suffer from poor sound quality due to low damping, large displacement at resonant frequency, and small frequency bandwidth.
Design a MEMS piezoelectric generator that adopts a rectangular bridge diaphragm structure. By setting a slotted structure in the diaphragm structure and covering it with a flexible material, the internal stress is reduced, the system damping is increased, the diaphragm mass is reduced, and the vibration amplitude and air volume output are improved.
The sound pressure level (SPL) frequency response curve and the sound pressure level (THD) frequency response curve were improved, enhancing the sound quality and SPL output of the MEMS piezoelectric generator.
Smart Images

Figure CN118785061B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of sound generator technology, and in particular to a MEMS piezoelectric sound generator and its fabrication method. Background Technology
[0002] To expand the application of MEMS (Micro-Electro-Mechanical Systems) sound-generating devices and loudspeakers, the industry is dedicated to designing high-yield, small-size, and high-sound-pressure-level MEMS piezoelectric generators. However, devices based on silicon substrates and piezoelectric thin film materials often struggle to balance small size with high sound pressure level output. Furthermore, MEMS piezoelectric generators have low damping and a high quality factor for resonance, resulting in maximum displacement at the resonant frequency. This leads to resonance at the resonant frequency, characterized by a large displacement, a high-amplitude spike, and a narrow frequency bandwidth, deteriorating both the SPL (Sound Pressure Level) and THD (Total Harmonic Distortion) frequency response curves, ultimately resulting in poor sound quality. Additionally, the limited air volume propelled by MEMS piezoelectric generators in related technologies lowers the output SPL under excitation, also affecting the SPL frequency response curve. Summary of the Invention
[0003] The purpose of this invention is to provide a MEMS piezoelectric generator and its fabrication method to improve the sound pressure level, enhance the SPL frequency response curve and THD frequency response curve, and thereby improve the sound quality of the MEMS piezoelectric generator.
[0004] This invention provides a MEMS piezoelectric sound generator, comprising: a substrate; first piezoelectric composite layers symmetrically disposed at a set of designated edge positions opposite each other on the upper surface of the substrate; each first piezoelectric composite layer having a rectangular structure; a cavity in the bottom central region of the substrate; at least a portion of each first piezoelectric composite layer being located in the upper region of the substrate corresponding to the cavity; in the upper region, a plurality of slotted structures are disposed in designated areas other than at least a portion of each first piezoelectric composite layer, at least a portion of the slotted structures being covered with a flexible material, the upper region having the flexible material forming a diaphragm structure of the MEMS piezoelectric sound generator; the diaphragm structure being a rectangular bridge structure; a first diaphragm edge of the diaphragm structure being an anchored edge, and other diaphragm edges other than the first diaphragm edge being non-anchored edges; an edge slotted structure being disposed at each non-anchored edge, the first diaphragm edge being determined according to the relative position of the first piezoelectric composite layer on the substrate.
[0005] Furthermore, the edge slot structures corresponding to the two opposite non-anchored edges are parallel to each other, and the dimensions of the edge slot structures are the same.
[0006] Furthermore, the diaphragm structure is parallel to the upper surface of the substrate, and at least a portion of the anchoring edge is fixed to the substrate.
[0007] Furthermore, at least one second piezoelectric composite layer is provided in the upper region of the substrate; a slotted structure is provided on each second piezoelectric composite layer, and / or, a slotted structure is provided in a designated region other than each second piezoelectric composite layer; the slotted structure is covered with a flexible material.
[0008] Furthermore, the aspect ratio of the diaphragm structure is greater than the preset value; as the aspect ratio of the diaphragm structure increases, the value of the first-order resonant frequency of the MEMS piezoelectric generator increases, and the difference between the resonant frequencies decreases.
[0009] Furthermore, the thickness range of the diaphragm structure is 0.1μm to 50μm; as the thickness of the diaphragm structure becomes thinner, the value of the first-order resonant frequency becomes smaller, and under the same piezoelectric drive, the deflection displacement generated by the diaphragm structure is greater, and the amount of air pushed out is greater.
[0010] Furthermore, the larger the cavity size, the smaller the value of the first-order resonant frequency; wherein the size includes at least one of the following: cavity area, cavity length, cavity width, cavity radius, and cavity diameter.
[0011] Furthermore, the neutral layer of the diaphragm structure is located at the center of the diaphragm structure.
[0012] Furthermore, each first piezoelectric composite layer and each second piezoelectric composite layer include, from bottom to top, a bottom electrode layer, an intermediate layer, and a top electrode layer; wherein, the intermediate layer is a piezoelectric layer, or, the intermediate layer is formed by overlapping and stacking multiple piezoelectric layers and multiple electrode layers; wherein, the layer above the bottom electrode layer and the layer below the top electrode layer are both piezoelectric layers.
[0013] This invention provides a method for fabricating a MEMS piezoelectric sound generator. The method includes: thermally growing insulating layers on the upper and lower surfaces of a preset substrate; depositing a seed layer, a bottom electrode layer, an intermediate layer, and a top electrode layer sequentially from bottom to top on the insulating layer on the upper surface of the substrate to obtain a first element; wherein the intermediate layer is a piezoelectric layer, or the intermediate layer is formed by overlapping and stacking multiple piezoelectric layers and multiple electrode layers; wherein the layer above the bottom electrode layer and the layer below the top electrode layer are both piezoelectric layers; and sequentially patterning the top electrode layer, intermediate layer, and bottom electrode layer in the first element to form a symmetrical first piezoelectric composite layer at a set of specified edges opposite each other on the upper surface of the substrate, to obtain a patterned layer. The second element is processed; a passivation layer is deposited on the second element to isolate the electrical connection of each top electrode layer, and the passivation layer is patterned to form a pad area to bring out the bottom electrode layer, middle electrode layer and top electrode layer of each first piezoelectric composite layer, to obtain the third element; a metal layer is deposited on each pad area of the third element to form a pad, to obtain the fourth element; a designated area on the upper surface of the fourth element is etched to form multiple slot structures, and at least a portion of the slot structures are covered with a flexible material to obtain the fifth element; the bottom surface of the substrate of the fifth element is thinned and etched to form a cavity, to obtain the MEMS piezoelectric generator; wherein the etched cavity is located in the bottom center region of the substrate.
[0014] The present invention provides a MEMS piezoelectric sound generator and its fabrication method, comprising: a substrate, wherein first piezoelectric composite layers are symmetrically disposed at a set of designated edge positions opposite to each other on the upper surface of the substrate; each first piezoelectric composite layer is a rectangular structure; the bottom central region of the substrate has a cavity, and at least a portion of each first piezoelectric composite layer is located in the upper region of the substrate corresponding to the cavity; a plurality of slotted structures are disposed in a designated region of the upper region excluding at least a portion of each first piezoelectric composite layer, at least a portion of the slotted structures are covered with a flexible material, and the upper region with the flexible material forms a diaphragm structure of the MEMS piezoelectric sound generator; the diaphragm structure is a rectangular bridge structure; the first diaphragm edge corresponding to the first piezoelectric composite layer of the diaphragm structure is an anchored edge, and the other diaphragm edges other than the first diaphragm edge are non-anchored edges; and an edge slotted structure is disposed at each non-anchored edge. By incorporating a slotted structure, the internal stress of each diaphragm layer in the diaphragm structure caused by the manufacturing process can be reduced. Covering the slotted structure with a flexible material can improve the flexibility of the diaphragm structure, while reducing sound leakage at low frequencies in the MEMS piezoelectric generator, increasing the vibration amplitude and emitted sound pressure level of the MEMS piezoelectric generator. Replacing the high-density silicon diaphragm with a low-density flexible material reduces the mass of the diaphragm structure, and the rectangular bridge structure of the diaphragm structure can expel more air. The flexible material increases system damping, which is beneficial for improving the SPL and THD frequency response curves, thereby enhancing the sound quality of the MEMS piezoelectric generator. Attached Figure Description
[0015] To more clearly illustrate the specific embodiments of the present invention or the technical solutions in the prior art, the drawings used in the description of the specific embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are some embodiments of the present invention. For those skilled in the art, other drawings can be obtained from these drawings without creative effort.
[0016] Figure 1 This is a schematic diagram of the structure of a MEMS piezoelectric sound generator provided in an embodiment of the present invention;
[0017] Figure 2 This is a schematic diagram of the structure of a MEMS piezoelectric sound generator provided in an embodiment of the present invention;
[0018] Figure 3(a) , 3(b) Figure 3(c) is a schematic diagram of the structure of a piezoelectric composite unit provided in an embodiment of the present invention;
[0019] Figure 4(a) , 4(b) Figures 4(c), 4(d), 4(e), 4(f), 4(g), 4(h), 4(i), 4(j), 4(k), 4(m), 4(n), 4(o), 4(p), 4(q), and 4(r) are schematic diagrams of a MEMS piezoelectric sound generator provided in an embodiment of the present invention.
[0020] Figure 5(a) , 5(b) Figures 5(c) and 5(d) are schematic diagrams of the polarization mode and electrical connection of a MEMS piezoelectric generator provided in an embodiment of the present invention;
[0021] Figure 6(a) , 6(b) Figures 6(c) and 6(d) are schematic diagrams of simulation results of a MEMS piezoelectric sound generator provided in an embodiment of the present invention;
[0022] Figure 7(a) , 7(b) This invention provides a schematic diagram of the polarization method and electrical connection of a MEMS piezoelectric generator according to an embodiment of the present invention.
[0023] Figure 8(a) , 8(b) Figures 8(c) and 8(d) are schematic diagrams of the polarization mode and electrical connection of a MEMS piezoelectric generator provided in an embodiment of the present invention;
[0024] Figure 9(a) , 9(b) This invention provides a schematic diagram of the polarization method and electrical connection of a MEMS piezoelectric generator according to an embodiment of the present invention.
[0025] Figure 10(a) , 10(b) 10(c) is a schematic diagram of an array arrangement provided in an embodiment of the present invention;
[0026] Figure 11(a) , 11(b) 11(c) is a schematic diagram of an array arrangement provided in an embodiment of the present invention;
[0027] Figure 12(a) , 12(b) This is a schematic diagram of an array arrangement provided in an embodiment of the present invention;
[0028] Figure 13(a) , 13(b) 13(c), 13(d), 13(e), 13(f), 13(g), and 13(h) are schematic diagrams of an array arrangement provided in an embodiment of the present invention;
[0029] Figure 14(a) is a schematic diagram of a loudspeaker provided in an embodiment of the present invention;
[0030] Figure 14(b) , 14(c) A schematic diagram of simulation results provided for an embodiment of the present invention;
[0031] Figure 15(a) is a schematic diagram of a loudspeaker provided in an embodiment of the present invention;
[0032] Figure 15(b) , 15(c) A schematic diagram of simulation results provided for an embodiment of the present invention;
[0033] Figure 16 A flowchart illustrating a method for fabricating a MEMS piezoelectric sound generator according to an embodiment of the present invention;
[0034] Figure 17 A cross-sectional schematic diagram of a substrate with an insulating layer grown, provided as an embodiment of the present invention;
[0035] Figure 18 This is a schematic cross-sectional view of a bottom electrode layer after growth, provided in an embodiment of the present invention.
[0036] Figure 19 This is a cross-sectional schematic diagram of the intermediate layer and the top electrode layer after growth, provided in an embodiment of the present invention;
[0037] Figure 20 This is a graphical cross-sectional schematic diagram provided in an embodiment of the present invention;
[0038] Figure 21 This is a schematic cross-sectional view of a passivation layer after deposition and patterning, provided as an embodiment of the present invention;
[0039] Figure 22 This is a schematic cross-sectional view of a metal wire after deposition and patterning, provided in an embodiment of the present invention;
[0040] Figure 23 This is a schematic cross-sectional view of an SOI top silicon trench after etching, provided as an embodiment of the present invention.
[0041] Figure 24 This is a cross-sectional schematic diagram of a flexible thin film material coated according to an embodiment of the present invention. Detailed Implementation
[0042] The technical solution of the present invention will be clearly and completely described below with reference to the embodiments. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.
[0043] Most consumer electronics sound-generating devices use traditional electrodynamic mechanisms, consisting of magnets, voice coils, diaphragms, support structures, and housings. This operating principle limits the minimum height that the device can reach. A crucial factor in sound generation is the effective diaphragm radiation area; a larger area allows for more air output with the same thrust, resulting in a louder sound. A second factor is the movement of the diaphragm's radiation region: the greater the shift in the diaphragm's region, the louder the sound. To achieve small-sized, high-sound-pressure-level sound-generating devices and loudspeakers, the trend in MEMS sensors, loudspeakers, and transducers is to replace the entire system with silicone equivalents. Piezoelectric MEMS sound-generating devices, fabricated using MEMS processes, utilize piezoelectric thin-film materials as actuators. Piezoelectric MEMS loudspeakers, with their advantages of small size, low power consumption, low cost, and mass production capabilities, have become a research hotspot.
[0044] Silicon processing results in inherently thin form factors; the MEMS motors in loudspeakers are less than half a millimeter thick, an order of magnitude thinner than electrodynamic loudspeakers. MEMS loudspeakers benefit from the stabilizing effect of piezoelectric motors, which not only provide driving force but also make the motion more linear and controllable. The linear actuators in piezoelectric MEMS sound-generating devices have higher speed and precision than voice coils, resulting in higher bandwidth and more accurate high-frequency reproduction.
[0045] Related technologies provide a sound-generating unit and its manufacturing method, the sound-generating unit including a diaphragm and an actuating layer. The diaphragm includes a first diaphragm sub-section and a second diaphragm sub-section opposite to each other, and the actuating layer is disposed on the first diaphragm sub-section and the second diaphragm sub-section. The first diaphragm sub-section includes a first anchoring edge, which is fully or partially anchored, and all edges of the first diaphragm sub-section except the first anchoring edge are unanchored. The second diaphragm sub-section includes a second anchoring edge, which is fully or partially anchored, and all edges of the second diaphragm sub-section except the second anchoring edge are unanchored. However, this method, due to process limitations and stress constraints in the structure of each layer, results in significant harmonic distortion (THD) and limited sound pressure level (SPL) enhancement; the slotted cantilever beam structure is prone to air leakage.
[0046] Related technologies also provide a microelectromechanical sound transducer with a polymer coating, where a cured polymer is formed after the polymer has been cured, which has another advantage. The coating formed by the cured polymer and the piezoelectric component form a composite structure. The piezoelectric component can be formed, for example, from ceramic. Furthermore, if the piezoelectric component is relatively thin, its vibration performance is better. However, this increases the risk of piezoelectric component breakage. The piezoelectric component can be stabilized by the coating formed by the cured polymer, which retains elasticity and flexibility even after curing. The composite system formed by the coating made of the cured polymer and the piezoelectric component stabilizes the piezoelectric component. However, in this approach, the coating formed by the cured polymer only acts as a protective structure and does not reduce the quality of the vibrating diaphragm. The composite structure formed by the coating formed by the cured polymer and the piezoelectric component, due to process limitations and stress constraints in each layer, leads to significant harmonic distortion (THD) and limited sound pressure level (SPL) enhancement.
[0047] In summary, among related technologies, piezoelectric MEMS sound generators have low system damping and a high quality factor for device resonance. The displacement of the piezoelectric MEMS sound generator reaches its maximum at the resonant frequency, leading to resonance at that frequency with a large displacement, a high-amplitude spike, and a small frequency bandwidth. This deteriorates the sound pressure level (SPL) and total sound density (THD) frequency response curves, resulting in poor sound quality. In small-sized square or circular structures, due to the high symmetry of the structure, the excitation modes of the square or circular diaphragm are both odd and even modes. In the even-mode state, the vibrations of the diaphragm under excitation cancel each other out, resulting in a lower output SPL, which also affects the SPL frequency response curve. Therefore, this invention provides a piezoelectric MEMS sound generator and its fabrication method. This technology can be applied to applications requiring improved sound quality from piezoelectric MEMS sound generators.
[0048] To facilitate understanding of this embodiment, a MEMS piezoelectric generator disclosed in this embodiment of the invention will first be introduced. The MEMS piezoelectric generator includes: a substrate, on which first piezoelectric composite layers are symmetrically disposed at a set of designated edge positions opposite each other on the upper surface of the substrate; each first piezoelectric composite layer is a rectangular structure; the bottom central region of the substrate has a cavity, and at least a portion of each first piezoelectric composite layer is located in the upper region of the substrate corresponding to the cavity; in the upper region, in a designated area other than at least a portion of each first piezoelectric composite layer, a plurality of slotted structures are disposed, at least a portion of the slotted structures are covered with a flexible material, and the upper region with the flexible material forms the diaphragm structure of the MEMS piezoelectric generator; the diaphragm structure is a rectangular bridge structure; the first diaphragm edge of the diaphragm structure is an anchored edge, and the other diaphragm edges other than the first diaphragm edge are non-anchored edges; an edge slotted structure is disposed at each non-anchored edge, and the first diaphragm edge is determined according to the relative position of the first piezoelectric composite layer on the substrate.
[0049] The substrate material can also be SOI (Silicon-On-Insulator), silicon, glass, sapphire, etc., depending on the specific requirements. The upper surface of the substrate is typically covered with an insulating layer. The substrate usually has multiple edge locations; for example, if the upper surface of the substrate is rectangular, it includes two sets of opposite edge locations. The specified edge locations can be any set of edge locations; preferably, the specified edge locations are a set of edge locations corresponding to two opposite long sides of the rectangle. A first piezoelectric composite layer is symmetrically disposed at each of these specified edge locations, meaning that the first piezoelectric composite layer disposed at each of these specified edge locations is opposite to each other. Each of the first piezoelectric composite layers is a rectangular structure. The MEMS piezoelectric generator can perform electroacoustic conversion through the first piezoelectric composite layer. When a driving signal is applied to the first piezoelectric composite layer, the first piezoelectric composite layer can deform the diaphragm structure under the drive of the electrical signal, thereby generating sound waves and realizing the vibration sound generation of the MEMS piezoelectric generator. The size and shape of the cavity can be set according to actual needs. The cavity can be formed by etching on the back side of the substrate. By designing cavity structures of different sizes, the resonant frequency of the MEMS piezoelectric generator can be changed, so it can be applied to loudspeakers or ultrasonic transducers. Usually, different cavity sizes will result in different first-order resonant frequencies of the MEMS piezoelectric generator.
[0050] Projecting an orthographic projection from the cavity onto the upper surface of the substrate, the area corresponding to the projection is the upper region of the substrate. A portion of each first piezoelectric composite layer is located in this upper region. Within this upper region, a designated area excluding a portion of each first piezoelectric composite layer is provided with multiple slotted structures. This designated area may include: a central rectangular area and / or the edge of the substrate, etc. The shape and number of the slotted structures can be set according to actual needs. The flexible material can be a dry film, such as, but not limited to, one of the following materials: polyimide, parylene, polyurethane, PVI-3 (PVI stands for Poly Vinyl Isobutyl ether), photosensitive cover film Flexfiner SA, or other organic films. The thickness of the flexible material film layer is usually between 0.5μm and 30μm, preferably 5μm. The flexible material can not only cover the slotted structure, but also act as a diaphragm, and can also be used as an insulating layer material to cover metal interconnects, providing electrical insulation, waterproofing, and other functions. When a flexible material covers at least a portion of a slotted structure, the length and width dimensions of the covered portion are typically larger than the length and width dimensions of the slotted structure.
[0051] The aforementioned flexible materials typically need to possess the following properties: compatibility with MEMS processes, patternability, long-term operation, aging resistance, and good mechanical and temperature stability. Additionally, the flexible material needs to have a certain elongation, and the difference in thermal expansion coefficients between the flexible material and the substrate should minimize wafer bending.
[0052] The upper region of a substrate with flexible material forms the diaphragm structure of a MEMS piezoelectric generator. The diaphragm can be a rigid substrate or a flexible substrate, and the material can be monocrystalline silicon, polycrystalline silicon, glass, polymers (e.g., polyimide (PI), polyethylene terephthalate (PET), organic or inorganic compounds, any suitable material or combination thereof).
[0053] The aforementioned diaphragm structure is a rectangular bridge structure. The first edge of the diaphragm structure is the anchoring edge. For example, if the two long sides of the diaphragm structure are anchoring edges, then the two short sides of the diaphragm structure are non-anchoring edges. Each non-anchoring edge is provided with an edge slotting structure. The first diaphragm edge is determined according to the relative position of the first piezoelectric composite layer on the substrate. For example, if the first piezoelectric composite layer is on the left side of the substrate, then the left edge of the diaphragm structure is the anchoring edge; if the first piezoelectric composite layer is on the right side of the substrate, then the right edge of the diaphragm structure is the anchoring edge.
[0054] like Figure 1The diagram shows a schematic of a MEMS piezoelectric generator, illustrated using an SOI substrate as an example. The structure includes: SOI substrate silicon 01, a BOX layer silicon dioxide barrier layer 02, and SOI top silicon 03; an insulating layer 04 formed on the SOI top silicon 03, a seed layer 05 formed on the insulating layer 04, a bottom electrode layer 06, an intermediate electrode layer 07, and a top electrode layer 08 of the first piezoelectric composite layer, and a bottom piezoelectric layer 09 and a top piezoelectric layer 10 of the first piezoelectric composite layer; a groove 16 etched on the SOI top silicon 03 is a linear groove located above the hollow region of the device cavity 15. This groove 16 can be obtained using DRIE (Deep Reactive Ion Etching) technology. The width of the groove 16 is typically designed to be between 0.5 μm and 2000 μm, decoupling the device structure and releasing the process stress within each film layer, thereby achieving greater driving displacement and sound pressure level output. The flexible material 17 covers the area, with a width greater than the etched groove 16, to prevent sound leakage. 11 is the diaphragm of the device, composed of SOI top silicon O3 and a first piezoelectric composite layer, and is the sound-generating part of the MEMS piezoelectric generator. The insulating layer 14 provides electrical insulation and isolation protection. The solder pads 12 and 13 are connection points for the signal input terminals, and can be connected to the first piezoelectric composite layer of the MEMS piezoelectric generator via metal wires.
[0055] like Figure 2 The diagram shown is a structural schematic of a MEMS piezoelectric sound generator, wherein... Figure 1 Equivalent to Figure 2 The corresponding sectional view should be noted that the terms "left and right" refer to the two sides of the MEMS piezoelectric generator along the X-axis, "up and down" refer to the two sides along the Y-axis, and "inside and outside" refer to the two sides along the Z-axis. Moving downwards indicates that the MEMS piezoelectric generator has moved along the Y-axis.
[0056] like Figure 2As shown, the MEMS piezoelectric generator D10 includes a diaphragm structure, left and right first piezoelectric composite layers 10a and 10b, and a middle second piezoelectric composite layer 10c. These two first piezoelectric composite layers are rectangular and positioned on the diaphragm structure. The left and right first piezoelectric composite layers 10a and 10b are connected to and anchored to the device edges 30a and 30c, respectively, and fixed to the device substrate, extending beyond the back cavity edges 20a and 20c. The inner edges of the first piezoelectric composite layers 10a and 10b are 60a and 60b, which are parallel to each other and symmetrical about the Y-axis. The thin dashed lines 20a, 20b, 20c, and 20d in the figure form a rectangle, representing the back cavity region of the device, obtained through back etching or other methods, thereby causing the diaphragm structure to vibrate and shift on the device. The MEMS piezoelectric transmitter D10 has multiple slotted structures, namely the white dashed lines 40a, 40b, 40c, and 40d in the diagram. Slotted structures 40a and 40b are located on the upper and lower sides of the diaphragm structure, dividing the device at the edges 30b and 30d. The diaphragm structure can be a rectangular bridge structure, a rectangular cantilever beam structure, or a shape with slits or other suitable shapes. It can also have at least one or more straight lines or other pattern combinations. Slotted structures 40c and 40d are located on both sides of the second piezoelectric composite layer 10c in the middle of the diaphragm, and can have one or more straight lines or curved lines or other pattern combinations. Slotted structures 40c and 40d are covered with flexible materials 70a and 70b. Slotted structures 40a and 40b may not need to be covered. The length and width dimensions of the flexible material are usually larger than the length and width dimensions of the slotted structure, i.e., full coverage. Of course, in terms of length, it is also possible to not completely cover, or to use multiple segments of flexible material to partially cover slotted structures 40c and 40d. When the slotted structure is covered by a flexible material, the size of the slot can be very large, with dimensions such as length, width, and diameter up to 2000 μm.
[0057] The aforementioned MEMS piezoelectric generator, by incorporating a slotted structure, reduces the internal stress of each diaphragm layer caused by the manufacturing process. Using a flexible material to cover the slotted structure improves the flexibility of the diaphragm structure, reduces sound leakage at low frequencies, and increases the vibration amplitude and emitted sound pressure level. Replacing the denser silicon diaphragm with a low-density flexible material reduces the mass of the diaphragm structure. Furthermore, the rectangular bridge-type diaphragm structure allows for greater airflow. The flexible material increases system damping, which helps improve the sound pressure level (SPL) and total sound pressure level (THD) frequency response curves, thereby enhancing the sound quality of the MEMS piezoelectric generator.
[0058] Furthermore, the edge slot structures corresponding to the two opposite non-anchored edges are parallel to each other, and the dimensions of the edge slot structures are the same.
[0059] In actual implementation, such as Figure 2 As shown, the two short sides of the diaphragm structure are non-anchored edges, also known as free-moving edges. These free-moving edges are generally slotted to form free ends using manufacturing processes. The slotted structures 40a and 40b on the upper and lower sides correspond to the aforementioned edge slotting structures. The dimensions of the slotted structures 40a and 40b are generally the same and parallel to each other. The slotted structures 40a and 40b may also be incompletely slotted.
[0060] Both the top and bottom sides of the diaphragm structure contain slotted structures. For example, on the left side of the diaphragm structure, the slotted structures are formed on the three edges other than the anchoring edge. The three slotted structures corresponding to the other three edges constitute the free end of the left side of the diaphragm structure. The anchoring edge on the left side of the diaphragm structure is at the same position as the anchoring edge on the right side of the diaphragm structure and is fixed to the substrate of the device.
[0061] Furthermore, the diaphragm structure is parallel to the upper surface of the substrate, and at least a portion of the anchoring edge is fixed to the substrate.
[0062] The diaphragm structure is usually parallel to the upper surface of the substrate, and the anchoring edge can be fixed entirely or partially to the substrate.
[0063] Furthermore, at least one second piezoelectric composite layer is provided in the upper region of the substrate; a slotted structure is provided on each second piezoelectric composite layer, and / or, a slotted structure is provided in a designated region other than each second piezoelectric composite layer; the slotted structure is covered with a flexible material.
[0064] One or more second piezoelectric composite layers can be disposed in the middle of the upper region of the substrate. This can also be understood as one or more second piezoelectric composite layers being disposed in the middle of the diaphragm structure of the MEMS piezoelectric generator. Figure 1 and Figure 2 As shown, the second piezoelectric composite layer 10c in the middle is separated from the second piezoelectric composite layers 10a and 10b, and is a rectangular structure, and is disposed on the diaphragm structure; a slotted structure can be provided on each second piezoelectric composite layer, or a slotted structure can be provided around the perimeter of the second piezoelectric composite layer in a designated area, such as... Figure 2 The 40c and 40d values can be selected based on actual needs, and a flexible material is used to cover the slotted structure. The dimensions of this covering material are typically larger than the dimensions of the slotted structure itself. In practice, the second piezoelectric composite layer in the central region can be divided into two or more parts, with shapes such as circles, hexagons, octagons, or other irregular shapes. The slotted structure can release internal stress, for example... Figure 2In the process of manufacturing the diaphragm structure, the slotted structure can release the internal stress generated in regions 50a and 50b of the diaphragm structure, as well as the first and second piezoelectric composite layers. The width of the slotted structure should be small enough, and the slotted structure in the figure is generally less than 10μm wide.
[0065] In practice, the aforementioned slotted structure can run through the entire diaphragm structure, dividing it into two parts to form a cantilever beam structure, or it can leave a portion to form a connecting lock structure, so that the diaphragm structure vibrates uniformly under drive.
[0066] When the width of the slotted structure is relatively small, it needs to penetrate the diaphragm structure in the thickness direction, which is the thickness of the diaphragm structure. When the width of the slotted structure is greater than 5μm, it needs to be covered with a flexible material to prevent sound leakage. When the width of the slotted structure is less than 5μm, the diaphragm structure vibrates and produces sound. When the sound propagates in the narrow slot, heat loss and viscosity loss will cause sound wave attenuation. In this case, it is not necessary to cover with a flexible material, and it will not cause significant sound loss at low frequencies.
[0067] When the width of the slotted structure is relatively large, it extends through the diaphragm structure in the thickness direction, representing the diaphragm's thickness. When the width of the slotted structure is between 5μm and 2000μm, combining it with a rigid material to form a diaphragm structure can improve the diaphragm's flexibility and simultaneously seal off airflow, eliminating leakage areas in the MEMS piezoelectric generator. This reduces sound leakage at low frequencies and increases the vibration amplitude and emitted sound pressure level of the piezoelectric MEMS generator unit. Furthermore, a larger slotted structure can reduce the diaphragm's mass, which is beneficial for improving the sound pressure level curve and enhancing mid-frequency performance.
[0068] MEMS piezoelectric generators typically have a high quality factor Q, resulting in a sharp peak and narrow peak frequency response on their displacement-frequency or sound pressure level frequency curves after excitation. This embodiment utilizes a flexible material to construct a rigid-flexible diaphragm structure, which increases system damping and reduces the resonance quality factor Q, thereby flattening the sound pressure level curve and reducing total harmonic distortion (THD).
[0069] Furthermore, the aspect ratio of the diaphragm structure is greater than the preset value; as the aspect ratio of the diaphragm structure increases, the value of the first-order resonant frequency of the MEMS piezoelectric generator increases, and the difference between the resonant frequencies decreases.
[0070] In this embodiment, the diaphragm structure is a rectangular bridge structure. For example, the anchored edges on the left and right sides constitute the length of the diaphragm structure, while the non-anchored edges on the top and bottom sides constitute the width. The aspect ratio is greater than a preset threshold, such as greater than or equal to 3. The cavity size, diaphragm structure size, and diaphragm structure thickness of the MEMS piezoelectric generator are closely related to its resonant frequency. The length and width of the rectangular diaphragm structure both affect the resonant frequency of the MEMS piezoelectric generator; a smaller diaphragm width results in a higher resonant frequency. The diaphragm length affects the output sound pressure level of the device; MEMS piezoelectric generators with a large aspect ratio achieve higher resonant frequencies and higher sound pressure levels compared to those with a smaller aspect ratio. Figure 2 Taking the MEMS piezoelectric generator D10 as an example, the aspect ratio of the diaphragm structure of the MEMS piezoelectric generator D10 can be greater than 3 or other values. The larger the aspect ratio of the diaphragm structure, the higher the value of the first-order resonant frequency of the MEMS piezoelectric generator, and the smaller the difference between the resonant frequencies. When the quality factor Q of the MEMS piezoelectric generator D10 resonance decreases, mixed resonance can be achieved. By using multiple MEMS piezoelectric generators D10 to form an array structure, multiple relatively wide-bandgap smooth peaks can be mixed together to form a frequency response with a relatively flat resonant frequency, thereby improving the performance of the MEMS piezoelectric generator D10.
[0071] By applying a drive to the first piezoelectric composite layers 10a and 10b, the diaphragm structure is displaced and deflected, moving along the Z-axis, thereby pushing air to produce sound and converting mechanical acoustic energy. It should be noted that the audio drive signal applied to the first piezoelectric composite layer corresponds to the input drive signal, while the audio drive signal corresponds to the output sound wave signal. The audio drive signal is generally a sinusoidal signal of DC voltage plus AC voltage, such as 10VDV+10VP; or it can be driven by a bipolar signal. The diaphragm structure of the MEMS piezoelectric generator D10 is a rectangular bridge structure, such as... Figure 2 As shown, the length direction of the diaphragm structure is the anchored edge, and the width direction is the non-anchored edge. The width of the diaphragm structure significantly affects the first resonant frequency of the MEMS piezoelectric generator D10, while the length of the diaphragm structure has a smaller impact on the resonant frequency, but a greater impact on the amount of air pushed by the diaphragm under excitation. Therefore, the aspect ratio of MEMS piezoelectric generators is generally large in structural design.
[0072] Furthermore, the thickness range of the diaphragm structure is 0.1μm to 50μm; as the thickness of the diaphragm structure becomes thinner, the value of the first-order resonant frequency becomes smaller, and under the same piezoelectric drive, the deflection displacement generated by the diaphragm structure is greater, and the amount of air pushed out is greater.
[0073] In this embodiment, the thickness of the diaphragm structure ranges from 0.1 μm to 50 μm; the thickness can vary. Generally, it is preferred to be between 1 μm and 5 μm, which needs to be determined based on the dimensions and performance parameters of the MEMS piezoelectric generator design. For example, once the dimensions of the MEMS piezoelectric generator and the cavity are determined, if a lower first-order resonant frequency of the MEMS piezoelectric generator is required, a thinner diaphragm structure is usually chosen; if a higher first-order resonant frequency is required, a thicker diaphragm structure is usually chosen. The first-order resonant frequency of the MEMS piezoelectric generator is related not only to the stiffness of the diaphragm structure but also to its mass. When the cavity dimensions and other parameters of the MEMS piezoelectric generator are fixed, generally speaking, the thinner the diaphragm structure, the lower the first-order resonant frequency of the MEMS piezoelectric generator. Once the MEMS piezoelectric generator and its cavity dimensions are determined, the resonant frequency can be adjusted by changing the thickness of the diaphragm structure. The thinner the diaphragm structure, the lower the first-order resonant frequency and the lower the stiffness of the MEMS piezoelectric generator. Under the same piezoelectric drive, the greater the deflection displacement generated by the diaphragm structure, the greater the amount of air pushed out, and thus the higher the output sound pressure level.
[0074] Furthermore, the larger the cavity size, the smaller the value of the first-order resonant frequency; wherein the size includes at least one of the following: cavity area, cavity length, cavity width, cavity radius, and cavity diameter.
[0075] The shape of the cavity can be set according to actual needs. For example, from the top or bottom view of the MEMS piezoelectric generator, the shape of the cavity can be rectangular, circular or other shapes. Generally, the larger the size of the cavity, the lower the first resonant frequency of the MEMS piezoelectric generator. The size here can refer to the measured parameters such as cavity area, cavity length, cavity width, cavity radius or cavity diameter.
[0076] Furthermore, the neutral layer of the diaphragm structure is located at the center of the diaphragm structure.
[0077] The neutral layer of the entire diaphragm structure of a MEMS piezoelectric generator is designed at the center of the diaphragm structure. This design allows for opposing forces (tension and compression) on the upper and lower piezoelectric composite layers of the diaphragm. Through proper electrical connections and appropriate drive, the output sound pressure level of the device can be increased. The neutral layer mentioned above refers to a stress-neutral layer. For example, if the outer layer of the diaphragm structure is subjected to tensile stress while the inner layer is subjected to compressive stress, there is always a point where the stress is zero. This layer with zero stress is called the stress-neutral layer. Electrical connections require consideration of the number of piezoelectric layers and the polarization direction of each layer to ensure the maximum output sound pressure level of the piezoelectric MEMS generator. The drive is typically a combination of DC and AC voltage signals. Generally, the AC voltage does not exceed 30VpV, and the DC voltage does not exceed 15V.
[0078] Furthermore, each first piezoelectric composite layer and each second piezoelectric composite layer include, from bottom to top, a bottom electrode layer, an intermediate layer, and a top electrode layer; wherein, the intermediate layer is a piezoelectric layer, or, the intermediate layer is formed by overlapping and stacking multiple piezoelectric layers and multiple electrode layers; wherein, the layer above the bottom electrode layer and the layer below the top electrode layer are both piezoelectric layers.
[0079] Each of the first piezoelectric composite layers and each of the second piezoelectric composite layers can be a single piezoelectric layer structure, i.e., electrode layer / piezoelectric layer / electrode layer; it can be a double piezoelectric layer structure: electrode layer / piezoelectric layer / electrode layer / piezoelectric layer / electrode layer; and it can be a multi-piezoelectric layer structure: electrode layer / piezoelectric layer / electrode layer... / piezoelectric layer / electrode layer; the appropriate structure can be selected according to actual needs.
[0080] Figure 3(a), Figure 3(b), and Figure 3(c) show three structural schematics of a piezoelectric composite layer. In Figure 3(a), the piezoelectric composite layer is a single piezoelectric layer, consisting of a bottom electrode layer, a piezoelectric layer, and a top electrode layer from bottom to top. In Figure 3(b), the piezoelectric composite layer is a double piezoelectric layer, consisting of a bottom electrode layer, a piezoelectric layer, an electrode layer, a piezoelectric layer, and a top electrode layer from bottom to top. In Figure 3(c), the piezoelectric composite layer is a multi-piezoelectric layer structure, and the same logic applies to multi-piezoelectric layer structures. Depending on the number of piezoelectric layers and the polarization direction of different regions, various electrical connection methods exist. By comparison, the optimal connection method that maximizes the offset of the diaphragm structure of the MEMS piezoelectric generator and achieves the highest output sound pressure level can be obtained.
[0081] If the first piezoelectric composite layer and / or the second piezoelectric composite layer comprises multiple piezoelectric layers, each piezoelectric layer can be made of the same material or different materials, and the thicknesses of the different piezoelectric layers can be the same or different. The thickness range of the piezoelectric layers is typically between 0.1 μm and 25 μm, and the appropriate material or thickness can be selected according to actual needs. The material of the piezoelectric layer can be a single-crystal piezoelectric material or a polycrystalline material, such as single-crystal AlN, doped AlN, single-crystal PZT, doped PZT, ZnO, and other piezoelectric materials.
[0082] Similarly, if the first piezoelectric composite layer and / or the second piezoelectric composite layer include multiple electrode layers, each electrode layer can be made of the same material or different materials, and the thicknesses of the different electrode layers can be the same or different. The thickness range of the electrode layers is typically between 0.01 μm and 5 μm, and appropriate materials or thicknesses can be selected according to actual needs. The electrode layers can be made of single-crystal metal materials such as Mo, Pt, Al, and Cu, or alloy materials.
[0083] Figure 1 and Figure 2 The MEMS piezoelectric generator includes a diaphragm structure, which is a rectangular bridge structure comprising: first piezoelectric composite layers on the left and right sides of the diaphragm structure, and a second piezoelectric composite layer in the middle. Each first and second piezoelectric composite layer includes a double piezoelectric thin film structure consisting of a bottom electrode layer, a lower piezoelectric layer, a middle electrode layer, an upper piezoelectric layer, and a top electrode layer located on the upper surface of the diaphragm structure. One edge of the first piezoelectric composite layer unit on the left and right sides is anchored to the device, while the other edge is located on the diaphragm structure. The left and right sides of the diaphragm structure are anchored edges, while the top and bottom sides are free-moving edges, i.e., non-anchored edges. The anchored edges are completely or partially fixed to the device substrate, while the free-moving edges are generally formed by slotting them using process technology.
[0084] In actual implementation, besides Figure 1 The diaphragm structure in the MEMS piezoelectric generator can also be formed in other ways, as shown in Figure 4(a), which is a schematic diagram of a MEMS piezoelectric generator. The MEMS piezoelectric generator D11 is relative to... Figure 2In the MEMS piezoelectric generator D10, the second piezoelectric composite layer inside the diaphragm structure has three regions 10c, 10d, and 10e. Each second piezoelectric composite layer has a slotted structure 40c and 40d on the diaphragm structure near it, and these slotted structures 40c and 40d are covered by flexible materials 70a and 70b. In the figure, the three second piezoelectric composite layers 10c, 10d, and 10e can be equal in size (length), and their edges are parallel to each other, symmetrical about the horizontal axis (X) and the vertical axis (Y). Alternatively, the three second piezoelectric composite layers can be designed with unequal sizes, or any two of them can be equal, in other structural forms.
[0085] Figure 4(b) shows a schematic diagram of a MEMS piezoelectric generator. The MEMS piezoelectric generator D12 has two central second piezoelectric composite layers within its diaphragm structure. A diaphragm structure exists between the two second piezoelectric composite layers. L-shaped slotted structures 40a and 40b are etched onto the diaphragm and covered with flexible materials 70a and 70b. These slotted structures are equal in size (length) and have parallel edges. They are symmetrical about the horizontal X-axis and vertical Y-axis. The slotted structures are located on the diaphragm near the piezoelectric composite layers and are covered with flexible materials.
[0086] Figure 4(c) shows a schematic diagram of a MEMS piezoelectric generator. The second piezoelectric composite layer inside the diaphragm of the MEMS piezoelectric generator D13 is slotted, i.e., slotted structures 40c and 40d. Slotted structures 40c and 40d are not connected and do not divide the second piezoelectric composite layer. Flexible materials 70a and 70b are used to cover it. The slotted structures and the flexible material coverings shown in the figure have equal lengths and are symmetrical along the longitudinal axis Y. Alternatively, the lengths of the slotted structures and the flexible material coverings can be unequal and / or asymmetrical. In Figure 4(c), the slotted lines can also extend to the diaphragm structure, connecting with slotted structures 40a and 40b respectively, forming a single slotted structure that divides each of 10c into two regions. The slotted structure can also be composed of multiple line segments, and the length of the flexible material covering can be greater than and / or less than the length of the slotted structure.
[0087] Figure 4(d) shows a schematic diagram of a MEMS piezoelectric generator. Compared with MEMS piezoelectric generator D10, MEMS piezoelectric generator D14 does not have a second piezoelectric composite layer inside the diaphragm. The slots 40c, 40d, and 40e are located on the central diaphragm of the device and are covered by flexible materials 70a, 70b, and 70c. The slot gaps and the flexible material covering are located at the center of the diaphragm and are symmetrical about the horizontal axis X direction.
[0088] The aforementioned MEMS piezoelectric generator can have slots made in the second piezoelectric composite layer inside the diaphragm, as shown in Figure 4(c); or slots can be made in the diaphragm, as shown in Figure 4(d), and the location of the slots is not limited to those shown in the figures; it can form a flexible diaphragm and / or a vibrating thin film combining rigid and flexible materials.
[0089] The piezoelectric MEMS piezoelectric sound generating unit described above, when the width of the slotted structure is between 0.5μm and 5μm, its etched pattern can be a straight line, a circle, a square line, or other polygons and / or combinations thereof; when the width of the slotted structure is between 10μm and 200μm, its etched pattern can be a rectangle, a circle, a ring, a hexagon, or other polygons and / or combinations thereof, which can constitute a flexible diaphragm and / or a vibrating thin film composed of rigid and flexible materials.
[0090] Figure 4(e) shows a schematic diagram of a MEMS piezoelectric generator. Compared to MEMS piezoelectric generator D10, MEMS piezoelectric generator D15 has no slotted structures or flexible material covering on both sides of the second piezoelectric composite layer inside the diaphragm. However, there are two slotted structures 40c and 40d on the second piezoelectric composite layer 10c in the middle of the diaphragm, and the gaps are not covered by flexible material. The two slotted structures are of equal length, located on the diaphragm, and are rotationally symmetrical about the horizontal axis X. Alternatively, the slotted structures 40c and 40d can be designed asymmetrically with different lengths. The two slotted structures 40c and 40d on the second piezoelectric composite layer 10c can be one or more. One gap can extend to the upper and lower gaps 40a and 40b of the device, dividing the center of the device diaphragm into two cantilever beam structures, and the middle second piezoelectric composite layer 10c is divided into two regions.
[0091] Figure 4(f) shows a schematic diagram of a MEMS piezoelectric generator, D16. The second piezoelectric composite layers 10b, 10c, and 10d are located inside the diaphragm, and the slotted structures 40c and 40d are located inside the diaphragm and are symmetrical about the central horizontal line of the device. Compared to MEMS piezoelectric generator D15, the slotted structures are located in different positions within the diaphragm, and there are two slotted structures exhibiting central symmetry. Furthermore, the slotted structures are not covered by flexible materials. In practical implementation, the positions of the slotted structures inside the diaphragm can vary, and the number of slotted structures can be multiple. They can be centrally symmetrical or not, and the slotted structures can be fully or partially covered by flexible materials.
[0092] Figure 4(g) shows a schematic diagram of a MEMS piezoelectric generator. The diaphragm structure of the MEMS piezoelectric generator D17 contains two second piezoelectric composite layers, 10c and 10d, and there is no flexible material covering the slotted structure.
[0093] Figure 4(h) shows a schematic diagram of a MEMS piezoelectric generator. The diaphragm structure of MEMS piezoelectric generator D18 does not have a second piezoelectric composite layer, but it has three slotted structures 40c, 40d, and 40e. The shape of the slotted structure can be straight, circular, annular, or irregular, etc. The etching location, the number of etching slots, and the dimensional parameters of the etching slots (width, length, radius) can have various different structures or combinations thereof.
[0094] Figure 4(i) shows a schematic diagram of a MEMS piezoelectric generator, D19. Unlike MEMS piezoelectric generator D18, the slotted structure is inside the diaphragm, and there are two parallel slotted structures 40c and 40d of equal length. Both slotted structures 40c and 40d extend to slotted structures 40a and 40b, thus connecting to form a rectangular structure. Through MEMS technology, the rectangular part can be completely removed. At the same time, a flexible material 70a is used to cover the entire etched area. The size of the flexible material 70a is usually larger than the size of the etched rectangular slot. The left and right edges of the flexible material 70a exceed the slotted structures 40c and 40d, but do not cover the first piezoelectric composite layers 10a and 10b located on both sides in the middle of the diaphragm. Of course, during the design process, the flexible material 70a can cover the first piezoelectric composite layers 10a and 10b located on both sides of the middle of the diaphragm, so that the flexible material 70a is located on top of the piezoelectric composite layers 10a and 10b. Alternatively, it can be used for full-area sealing, covering the device frame 30a and 30b with the flexible material 70a, or multiple segments of flexible material can be used for equal or unequal coverage. The structural form of the flexible material 70a is diverse, and its structural size and distribution are not limited to device D19. The entire etched area is covered with flexible material, and the size of the flexible material is larger than the size of the removed area. When the device substrate cavity is released, a rigid-flexible diaphragm can be formed, and there is no air leakage inside the diaphragm when the device vibrates. Using flexible material for coverage, removing the high-density silicon diaphragm, and replacing it with a low-density flexible material as the diaphragm structure reduces the diaphragm's mass, which is beneficial for improving the sound pressure level curve and enhancing mid-frequency performance. The etched shape at the center of the diaphragm can be of various types, such as two rectangular frames, or circular, square, or polygonal structures. The number and position of the etched grooves can vary and are not limited to those shown in device D19.
[0095] Figure 4(j) shows a schematic diagram of a MEMS piezoelectric generator. Compared to the piezoelectric MEMS piezoelectric generator D19, the piezoelectric MEMS generator D20 has six rectangular strip structures 70b, 70c, 70d, 70e, 70f, and 70g made of flexible material inside its diaphragm. These six rectangular structures are of the same size and are regularly distributed within the diaphragm, exhibiting a symmetrical structure along the horizontal and vertical axes. One side of the six flexible rectangular strips is located above the frame 30a and 30c of the device D20, while the other side connects to the central flexible material 70a, forming a rectangular frame. The main function of the flexible material structure is to act as a reinforcing rib. Under piezoelectric actuation, it can increase the resonant frequency of the device without significantly reducing the maximum diaphragm offset, thereby widening the device's bandwidth. The reinforcing rib structure made of flexible material is not limited to this; its structure is diverse. Si material is relatively brittle, and diaphragms combining PZT and Si thin film layers, when used for anchoring in drivers, are prone to cracking and breakage. By using flexible dry film materials to create a rigid-flexible diaphragm, the dry film can reduce stress and absorb it through its own deformation when subjected to stress, thereby improving the device's shock resistance. Furthermore, when the device cavity structure is large, residual stress from MEMS processing can cause bulging or depressions in the diaphragm. This structure composed of flexible dry film materials can act as a reinforcing rib. Simultaneously, because the thermal expansion coefficients of flexible dry film materials differ from other materials, the stress distribution of the entire diaphragm can be adjusted, resulting in a smoother diaphragm structure. The piezoelectric composite layer can be divided by at least one slit, forming different piezoelectric composite layer regions around the perimeter of the diaphragm. The slit can reduce the internal stress of the piezoelectric composite film caused by the processing.
[0096] Figure 4(k) shows a schematic diagram of a MEMS piezoelectric generator. Compared to the piezoelectric MEMS piezoelectric generator D19, the piezoelectric MEMS generator D21 has three rectangular structures 40c, 40d, and 40e inside its diaphragm. These three rectangular structures are of the same size and are regularly distributed within the diaphragm, exhibiting a symmetrical structure along the horizontal and vertical axes. The rigid material of the rectangular structures 40c, 40d, and 40e on the diaphragm is removed. Flexible material 70a covers these areas and extends to the upper and lower edges 30b and 30d of the device. Alternatively, three flexible materials can be used to cover the three rectangular areas 40c, 40d, and 40e respectively, and these three flexible materials can be independent of each other. Of course, it can also be designed with multiple rectangular structures of the same size inside the diaphragm, regularly distributed within the diaphragm, and exhibiting a symmetrical structure along the horizontal and vertical axes. The rigid material of the rectangular structural pattern on the diaphragm is removed, and multiple rectangular areas where the rigid material was removed are covered with a flexible material. The size of the flexible material is larger than the rectangular structure, and they are not connected to each other. The internal pattern of the diaphragm of the piezoelectric MEMS piezoelectric sound unit D21 is a rectangular structure, but it can also be composed of one or more shapes such as square, circle, torus, hexagon, polygon, etc. The size and position of the pattern can be varied.
[0097] Other forms can also be used to form the diaphragm structure of the MEMS piezoelectric generator, as shown in Figure 4(m), Figure 4(n), Figure 4(o), Figure 4(p), Figure 4(q), and Figure 4(r). The shape, position, and size of the slotted structure can be selected according to actual needs, and no limitation is made here.
[0098] In the aforementioned piezoelectric MEMS piezoelectric sound-generating unit, if a slot is made in the second piezoelectric composite layer inside the diaphragm structure, when the width of the slot structure is between 0.5μm and 5μm, due to the small size, the sound will attenuate due to heat loss and viscous loss when the sound propagates in the narrow slot. Therefore, it is not necessary to use a flexible material for covering it. For device D18 in Figure 1, the slot structure is greater than 5μm, and a flexible material is used to cover it to prevent sound leakage. For device D20 in Figure 1, the width of the flexible material is greater than the slot structure, and it can and / or use a flexible material to cover all or part of the gap, and at the same time, it can cover the entire or part of the diaphragm.
[0099] MEMS piezoelectric generators are sound-generating devices that produce sound by shifting the diaphragm structure. When the applied driving signal frequency is significantly lower than the device's resonant frequency, the diaphragm structure shift can be directly controlled by the applied driving voltage signal. The amount of diaphragm structure shift is also related to the transverse piezoelectric coefficient of the piezoelectric film. When operating within the linear range of the diaphragm structure, the driving signal is much lower than the resonant frequency, and the diaphragm structure shift is proportional to the applied voltage and the transverse piezoelectric coefficient of the piezoelectric film.
[0100] In this embodiment, the mechanical resonant point of the MEMS piezoelectric generator can be designed within the audio range, or even beyond it (up to 20kHz), or even in the ultrasonic frequency band, by adjusting the diaphragm thickness and cavity size. When the mechanical resonant point is designed within the audible range of 20Hz-20kHz, and the first-order resonant frequency is 4-10kHz, the diaphragm displacement is large under piezoelectric signal drive, resulting in a high output sound pressure level in the low-frequency range, suitable for use in low-frequency loudspeakers. When the mechanical resonant point is designed beyond the audible range (greater than 20kHz), the first and third odd harmonics of the MEMS piezoelectric generator are outside the audible frequency range, resulting in lower nonlinearity and lower THD, suitable for use in high-frequency loudspeakers.
[0101] The aforementioned MEMS piezoelectric generator maintains structural symmetry, ensuring the consistency of vibration modes. Under drive, the rectangular structure only exhibits first, third, and fifth order odd vibration modes, without even-order mutually canceling vibration modes. This can broaden the bandwidth of the MEMS device and eliminate harmonic interference caused by even-order vibrations, thereby reducing THD.
[0102] The following uses a cross-sectional view of the MEMS piezoelectric generator D19 in Figure 4(i) as an example to provide a schematic diagram of the polarization mode and electrical connection of a MEMS piezoelectric generator as shown in Figure 5(a), Figure 5(b), Figure 5(c), and Figure 5(d). The MEMS piezoelectric generator D19 has first piezoelectric composite layers 10a and 10c on its left and right sides, but no second piezoelectric composite layer in the center of the diaphragm structure. As shown in Figures 5(a), 5(b), 5(c), and 5(d), the direction of the piezoelectric layer indicator arrows (upward or downward along the Z-axis) in piezoelectric composite layers 10a and 10c indicates the polarization direction of the device's piezoelectric layer. The positive and negative signs in the top electrode layer, middle electrode layer, and bottom electrode layer of piezoelectric composite layers 10a and 10c represent the positive and negative electrodes. As shown in Figure 5(a), the polarization direction of all the piezoelectric layers in the MEMS piezoelectric generator is consistent and upward. In terms of electrical connection, the middle electrode layer of each of the piezoelectric composite layers 10a and 10c is connected to the negative, and the top electrode layer and the bottom electrode layer are connected to the positive in parallel. In terms of electrical connection between piezoelectric composite layers 10a and 10c, the negative electrode is connected to the negative electrode, and the positive electrode is connected to the positive electrode. The connection method of the two piezoelectric composite layers 10a and 10c is a parallel structure.
[0103] Figure 5(b) , 5(c) In Figures 5(d), the polarization directions of the piezoelectric layers in piezoelectric composite layers 10a and 10c are different. In Figure 5(b), the polarization directions of both the upper and lower piezoelectric layers in piezoelectric composite layers 10a and 10c are downward. In Figure 5(c), the polarization direction of the bottom piezoelectric layer in piezoelectric composite layers 10a and 10c is upward, and the polarization direction of the upper piezoelectric layer is downward. In Figure 5(d), the polarization direction of the bottom piezoelectric layer in piezoelectric composite layers 10a and 10c is downward, and the polarization direction of the upper piezoelectric layer is upward. Electrically, in Figures 5(b), 5(c), and 5(d), the middle electrode of each piezoelectric composite layer 10a and 10c is connected to the negative electrode, and the top and bottom electrode layers are connected in parallel to the positive electrode. Electrically, the negative electrodes of piezoelectric composite layers 10a and 10c are connected to each other, and the positive electrodes are connected to each other. The connection method of the two piezoelectric composite layers 10a and 10c is a parallel structure. Figures 5(a), 5(b), 5(c), and 5(d) show four electrical connection methods with two-end interfaces, containing only positive and negative interfaces, or signal ports and ground ports. The impact of these four different polarization methods on device performance can be compared through simulation.
[0104] The following are simulation results of a MEMS piezoelectric generator, as shown in Figure 6(a), Figure 6(b), Figure 6(c), and Figure 6(d). These figures correspond to four displacement diagrams of the diaphragm structure of the MEMS piezoelectric generator under four different polarization modes, as shown in Figures 5(a), 5(b), 5(c), and 5(d). The maximum displacements obtained from the simulations are -11.3 μm, 11.3 μm, 28.8 μm, and -28.8 μm, respectively. Comparing the device displacement performance, it can be seen that when the middle electrode layer is grounded, the top electrode layer and the bottom electrode layer are connected in parallel, and the polarization directions of the upper and lower piezoelectric layers of the piezoelectric composite layer are opposite, that is, the maximum displacement can be obtained in the cases shown in Figures 5(c) and 5(d).
[0105] In Figures 5(a) and 5(b), the indicator arrows of the upper and lower piezoelectric layers in the piezoelectric composite layers 10a and 10c are all pointing upwards or downwards along the Z-axis. To achieve the same good displacement performance as in Figures 5(c) and 5(d), the electrical connection method of the piezoelectric composite layers 10a and 10c can be changed. Figure 7(a) shows a schematic diagram of the polarization method and electrical connection of a MEMS piezoelectric generator, and Figure 7(b) shows another schematic diagram of the polarization method and electrical connection of a MEMS piezoelectric generator. In terms of electrical connection, the middle electrode layer of each of the piezoelectric composite layers 10a and 10c is grounded, and the top and bottom electrode layers are connected to positive and negative respectively, or the top and bottom electrode layers are connected to negative and positive respectively. Then, the piezoelectric composite layers 10a and 10c are electrically connected with grounded, negative electrodes connected to negative electrodes, and positive electrodes connected to positive electrodes. The connection method between the two piezoelectric composite layers 10a and 10c is a parallel structure. Simulations show that the absolute value of the maximum displacement of the diaphragm structure is equal to 28.8 μm in both cases (Figure 7(a) and Figure 7(b), and the directions of the maximum displacement are opposite in Figure 7(a) and Figure 7(b). The electrical connection method in Figure 7(a) and Figure 7(b) is a three-terminal interface, with differential interfaces for positive, negative, and ground. Furthermore, the device performance is consistent with the electrical connection methods in Figure 5(c) and Figure 5(d).
[0106] The following is based on Figure 2Taking the MEMS piezoelectric generator D10 as an example, Figure 8(a), Figure 8(b), Figure 8(c), and Figure 8(d) provide a schematic diagram of the polarization and electrical connection of the MEMS piezoelectric generator. In Figures 8(a), 8(b), 8(c), and 8(d), the direction of the arrow indicates the polarization direction of the piezoelectric layer of the device. In Figures 8(a) and 8(b), all piezoelectric layers in the piezoelectric composite layers 10a, 10b, and 10c have the same polarization direction, and are all upward or downward along the Z-axis. The positive and negative signs in the top electrode layer, middle electrode layer, and bottom electrode layer of the piezoelectric composite layers 10a, 10b, and 10c represent the positive and negative electrodes. As shown in Figure 8(a), in terms of electrical connection, the middle layer electrodes of piezoelectric composite layers 10a and 10c are grounded, and the upper and lower electrode layers are connected in parallel with positive electrodes. Similarly, the middle layer electrode of piezoelectric composite layer 10b is grounded, and the upper and lower electrode layers are connected in parallel with positive electrodes. In Figures 8(a) and 8(b), the piezoelectric composite layers 10a and 10c are electrically connected to ground, with positive electrodes connected to positive electrodes, forming a parallel structure. In Figure 8(a), 10a, 10c, and 10b are electrically connected to ground, with positive electrodes connected to positive electrodes, forming a parallel structure. In Figure 8(b), the polarity of the upper and lower electrodes of piezoelectric composite layer 10b can be reversed, with the upper electrode layer connected to negative and the lower electrode layer connected to positive. In Figure 8(b), 10a, 10c, and 10b are electrically connected to ground, with positive electrodes connected to positive electrodes, forming a series structure.
[0107] In Figures 8(c) and 8(d), the polarization directions of all the upper and lower piezoelectric layers in piezoelectric composite layers 10a and 10c are opposite, while the polarization directions of all the upper and lower piezoelectric layers in 10b are the same. As shown in Figure 8(c), the polarization direction of the bottom piezoelectric layer in 10a and 10c is upward along the Z-axis, and the polarization direction of the top piezoelectric layer is downward along the Z-axis. The piezoelectric polarization of the upper and lower piezoelectric layers in piezoelectric composite layers 10a and 10c can be reversed, i.e., the polarization direction of the top piezoelectric layer is upward along the Z-axis, and the polarization direction of the bottom piezoelectric layer is downward along the Z-axis. In terms of electrical connection, the middle layer electrode of each of the piezoelectric composite layers 10a, 10b, and 10c is grounded, and the upper and lower electrode layers of 10a and 10c are connected in parallel. In Figures 8(c) and 8(d), 10a and 10c are electrically connected to ground, with positive electrodes connected to positive electrodes, and the two piezoelectric composite layers 10a and 10c are connected in parallel. In Figures 8(c) and 8(d), 10a, 10c, and 10b are electrically connected to ground, with positive electrodes connected to positive electrodes, and the connection between 10a, 10b, and 10c is also parallel. In Figure 8(c), the polarity of the upper and lower electrodes of piezoelectric composite layer 10b can be opposite, both being negative; in Figure 8(d), the polarity of the upper and lower electrodes of piezoelectric composite layer 10b can also be opposite, both being negative. Simulations show that the diaphragm structure achieves the optimal offset under the polarization direction and electrode connection shown in Figure 8(d).
[0108] Figure 9(a) shows a schematic diagram of the polarization and electrical connection of a MEMS piezoelectric generator, and Figure 9(b) shows a schematic diagram of the polarization and electrical connection of a MEMS piezoelectric generator. The indicator arrows of the upper and lower piezoelectric layers in piezoelectric composite layers 10a, 10b, and 10c are all pointing upwards or downwards along the Z-axis. In Figure 9(a), the indicator arrows of the upper and lower piezoelectric layers in piezoelectric composite layers 10a and 10c are pointing upwards along the Z-axis, 10b is pointing upwards, or the arrows of 10a, 10b, and 10c are all pointing in opposite directions. The direction of the indicator arrows is the polarization direction of the piezoelectric layer of the device. In order to achieve the optimal maximum displacement of the device performance, the electrical connection of device D10 is as shown in Figures 9(a) and 9(b). In Figure 9(a), the polarization direction of each voltage layer is upwards or downwards. In terms of electrical connection, the middle electrode of each piezoelectric composite layer 10a and 10c is grounded, and the upper and lower electrode layers are connected to positive and negative, or the upper and lower electrode layers are connected to negative and positive. The piezoelectric composite layer 10b is exactly the opposite of 10a and 10c. Electrically, piezoelectric composite layers 10a and 10c are connected in parallel with their negative electrodes connected to each other and their positive electrodes connected to each other. The connection between the two piezoelectric composite layers 10a and 10c is a parallel structure. However, the connection between piezoelectric composite layers 10a and 10c and unit 10b is a series structure with their negative electrodes connected to their positive electrodes and their positive electrodes connected to their negative electrodes. In Figure 9(b), the arrows indicating the upper and lower piezoelectric layers in piezoelectric composite layers 10a and 10c point downwards along the Z-axis, 10b upwards, or the arrows for 10a, 10b, and 10c all point in opposite directions. Electrically, piezoelectric composite layers 10a, 10b, and 10c are connected in parallel with their negative electrodes connected to each other and their positive electrodes connected to each other. When the arrows of the piezoelectric composite layers 10a, 10b, and 10c all point in opposite directions and the polarization directions change, the connection between the three piezoelectric composite layers 10a, 10b, and 10c remains a parallel structure, but the magnitudes of the displacements are equal and the directions of the offsets are opposite.
[0109] The positive and negative signs in the top, middle, and bottom electrode layers of the aforementioned piezoelectric composite layer indicate the positive and negative electrodes. When the polarities of the top and bottom electrode layers of the same piezoelectric composite layer are the same, the top and bottom electrodes are connected in parallel to the electrical signal terminal, and the middle electrode layer is grounded. Of course, it can also be reversed that the top and bottom electrode layers are connected in parallel to ground, and the middle electrode layer is connected to the signal terminal. At the same time, when there are two or more piezoelectric composite layers, or when there are two or more piezoelectric composite layers in the diaphragm structure, the performance of the device is related to the polarization direction of the piezoelectric layers in each region and the electrical connection between each unit and each electrode layer. Only when the polarization direction of the piezoelectric layers and the electrical connection method are appropriate will the acoustic performance output sound pressure level (SPL) of the device be optimal.
[0110] The present invention provides a loudspeaker, including at least one MEMS piezoelectric generator as described above, wherein each MEMS piezoelectric generator is arranged in a preset array.
[0111] To generate sound, 1) the larger the effective radiation area, the higher the sound pressure level. 2) the greater the displacement of the diaphragm radiation area, the higher the sound pressure level. When the output sound pressure level (SPL) of a single MEMS piezoelectric generator speaker device is limited under excitation, multiple MEMS piezoelectric generators can be distributed in an array structure to increase the area of the speaker's sound generation, thereby improving the device's sound pressure level output. Figure 10(a) shows a schematic diagram of one array arrangement, Figure 10(b) shows a schematic diagram of another array arrangement, and Figure 10(c) shows a schematic diagram of yet another array arrangement.
[0112] Figure 10(a) shows MEMS piezoelectric generators with the same structure. The unit devices in the array have the same size parameters, structural shape, and performance. The array structure is linear, with linear arrangement along the horizontal and vertical axes. Taking MEMS piezoelectric generator D10 as an example, it can be arranged in the horizontal axis X direction as two units D10-D10, three units D10-D10-D10, and many other unit arrangements; it can be arranged in the vertical axis Y direction as one unit D10, four units D10-D10-D10-D10, and many other unit arrangements; it can also be arranged linearly along the horizontal and vertical axes, using devices D10 to form array structures such as 1x1, 2x2, 3x3, 2x3, 3x2, and 4x4. The array structure can use MEMS piezoelectric generator D10, or other MEMS piezoelectric generators such as MEMS piezoelectric generator D11, MEMS piezoelectric generator D12, etc., to form an array structure with multiple identical devices.
[0113] The array structure layout in Figure 10(b) has a linear arrangement along the horizontal and vertical axes. In the horizontal axis X direction, the MEMS piezoelectric generators D11 are arranged as one or more identical units, with the devices in the horizontal axis X direction being the same. In the vertical axis Y direction, the MEMS piezoelectric generators D12 are arranged as one or more identical units, with the devices in the vertical axis Y direction being different. The array can be arranged linearly along both the horizontal and vertical axes simultaneously, using MEMS piezoelectric generators D11 and D12 in various array structures such as 2x2, 3x3, 4x4, 2x3, and 3x2. Other MEMS piezoelectric generators, such as MEMS piezoelectric generators D14 and / or MEMS piezoelectric generators D15, can also be used in this array structure.
[0114] The array structure layout in Figure 10(c) has a linear arrangement along the horizontal and vertical axes. In the horizontal axis X direction, MEMS piezoelectric generators D14 are arranged in single or multiple units, and the MEMS piezoelectric generators in the horizontal axis X direction are different. In the vertical axis Y direction, MEMS piezoelectric generators D13 are arranged in single or multiple units, and the MEMS piezoelectric generators in the vertical axis Y direction are different. It can also be arranged linearly along both the horizontal and vertical axes at the same time, using MEMS piezoelectric generators D14 and D16, and MEMS piezoelectric generators D13 and D15 in the horizontal axis X direction, arranged in various different array structures such as 2x2, 3x3, 4x4, 2x3, and 3x2. It should be noted that the MEMS piezoelectric generators in the array can be other MEMS piezoelectric generators, such as MEMS piezoelectric generators D17 and / or MEMS piezoelectric generators D20, etc.
[0115] Of course, other array arrangements can also be selected according to actual needs, as shown in Figure 11(a), Figure 11(b), Figure 11(c), Figure 12(a), and Figure 12(b). Figure 13(a) , 13(b) The array layout diagrams shown in 13(c), 13(d), 13(e), 13(f), 13(g), and 13(h) can be used to select a suitable layout method according to actual needs, and no limitation is made here.
[0116] In this embodiment, when used as a loudspeaker, depending on the magnitude of the emitted sound pressure level, the loudspeaker can be a single MEMS piezoelectric generator or multiple MEMS piezoelectric generators arranged in a preset array can be driven by electrical parallel connection to increase the output sound pressure level, wherein the diaphragm structures of the multiple MEMS piezoelectric generators are coplanar.
[0117] When used as a loudspeaker, there are various electrical connection methods depending on the number of piezoelectric layers and the polarization direction of the piezoelectric layers in different regions. By comparison, the optimal connection method that maximizes the diaphragm offset and outputs the highest sound pressure level can be obtained.
[0118] If the polarization direction of the piezoelectric layer in all MEMS piezoelectric generators on the upper side of the diaphragm structure is the same, then the electric fields of the piezoelectric layers in the inner and outer composite layers of the spring structure are opposite, the inner and outer electrodes are electrically separated, and the electrode layers are connected in series; if the polarization direction of the piezoelectric layer in all MEMS piezoelectric generators on the upper side of the diaphragm structure is opposite, then the electric fields of the piezoelectric layers in the inner and outer composite layers of the spring structure are the same, the inner and outer electrodes are electrically separated, and the electrode layers are connected in parallel.
[0119] The MEMS piezoelectric transmitters and speakers described in this invention can be used as MEMS actuators, specifically as piezoelectric MEMS drivers, piezoelectric MEMS micropumps, piezoelectric MEMS micromirrors, piezoelectric MEMS switches, piezoelectric MEMS inkjet printheads, etc. Conversely, they can also be used as MEMS transducers and sensors, specifically as piezoelectric MEMS microphones, piezoelectric MEMS pressure gauges, piezoelectric MEMS ultrasonic transducers, piezoelectric MEMS accelerometers, etc.
[0120] The structure of the above-mentioned loudspeakers is verified below. Figure 14(a) shows a schematic diagram of a loudspeaker, which is a MEMS loudspeaker device A with an array structure composed of four square units. Figure 15(a) shows a schematic diagram of a loudspeaker, which is a MEMS loudspeaker device B with an array structure composed of three rectangular units. MEMS loudspeaker devices A and B with the same size (length, width and thickness of each diaphragm) are manufactured under the same process conditions. The individual units of devices A and B are simulated under a 15V voltage drive to obtain the resonant frequency of the corresponding structure and the maximum vibration displacement of the diaphragm. Figures 14(b) and 14(c) show the simulation results for the resonant frequency and diaphragm displacement of device A; Figures 15(b) and 15(c) show the simulation results for the resonant frequency and diaphragm displacement of device B. From the figures, it can be seen that the resonant frequencies of the unit structures of MEMS speaker A and MEMS speaker B are 9.79kHz and 11.8kHz, respectively, and their maximum displacements are 48.2µm and 49.8µm, respectively. Integrating the diaphragm displacements, the air volumes pushed by the corresponding MEMS speaker A and MEMS speaker B are 0.435mm³ and 0.519mm³, respectively. Comparing MEMS speaker A and MEMS speaker B, the simulated resonant frequency of the MEMS speaker B unit is higher than that of MEMS speaker A, and the maximum diaphragm displacement under voltage drive is also larger. This is because a rectangular structure is superior to a square structure, pushing more air, i.e., a higher emitted sound pressure level of the acoustic transducer.
[0121] The aforementioned MEMS piezoelectric generator utilizes a gap for mechanical decoupling. When the gap width is between 0.5 and 5 μm, it not only reduces the internal stress in each layer of the vibrating diaphragm caused by the manufacturing process, but also improves the diaphragm's flexibility by using a flexible material for covering, reducing sound leakage at low frequencies and increasing the vibration amplitude and emitted sound pressure level of the piezoelectric MEMS generator. For cantilever beam structures, flexible materials can be used to create springs that connect to form a unified structure, ensuring consistent diaphragm posture during vibration. When the slot width is between 5 μm and 200 μm, replacing the high-density silicon diaphragm with a low-density flexible material reduces the diaphragm's mass, which helps improve the sound pressure level curve and enhance mid-frequency performance.
[0122] The aforementioned MEMS piezoelectric generator has a rectangular structure. Compared to circular or square structures, it lacks even modes in its response spectrum. Multiple modes are excited within a narrower frequency range, and the excited modes are all odd modes. These multiple modes are combined, thus significantly widening the frequency bandwidth. Furthermore, within the same area, the rectangular array structure exhibits higher performance and can improve the sound pressure level (SPL) of the sound-generating device.
[0123] This scheme is based on a double-layer piezoelectric PZT film. By rationally polarizing the piezoelectric layer and electrically connecting different regions, the dual driving electrodes (inner and outer electrodes) are used in a piston mode with a 180° antiphase driving structure to improve the emitted sound pressure level of MEMS piezoelectric generators and loudspeakers.
[0124] This embodiment employs a rigid-flexible diaphragm structure, using flexible material to cover the slotted structure, reducing low-frequency sound leakage and increasing the sound pressure level output at low frequencies. It also increases the damping of the diaphragm system, lowering the quality factor (Q), thereby reducing or minimizing resonance over a wider frequency range. This reduces the nonlinearity caused by large diaphragm offset at the device's resonant frequency, thus lowering total harmonic distortion (THD) and intermodulation distortion (IM). Furthermore, a double-layer piezoelectric thin-film structure with a rectangular cantilever beam or bridge-like structure fixed at both ends is designed, along with an array structure composed of multiple units to improve the output sound pressure level of the MEMS piezoelectric sound unit and the loudspeaker.
[0125] In this invention, the MEMS piezoelectric generator and loudspeaker perform electroacoustic conversion through a piezoelectric composite layer. Applying an electrical signal to the piezoelectric composite layer causes deformation, which in turn causes the diaphragm to vibrate, thus producing sound. In some embodiments, the sound-generating device can be a miniature loudspeaker, an ultrasonic transducer, or other suitable device to convert the electrical signal into sound waves. For the same area and resonant frequency, a rectangular structure pushes out more air than square, circular, or hexagonal structures, making it more efficient. The modes excited by cantilever beam or bridge-type rectangular structures are all odd modes. The larger the aspect ratio of the device, the smaller the spacing between adjacent resonant frequencies, increasing system damping, reducing the device's resonance quality factor, and causing the correlation peaks of different modes to merge, resulting in an ultra-wide bandwidth.
[0126] This invention also provides a method for fabricating a MEMS piezoelectric sound generator, such as... Figure 16 As shown, the method includes the following steps:
[0127] Step S1601: Thermally oxidize and grow insulating layers on the upper and lower surfaces of the preset substrate, respectively;
[0128] The aforementioned pre-defined substrate can be an SOI substrate, a silicon substrate, glass, sapphire, etc. Taking an SOI substrate as an example, this SOI substrate typically has an insulating buried layer, also known as a BOX layer. The BOX layer divides the substrate into two parts: the part above the BOX layer corresponds to the aforementioned top-layer silicon of the SOI, and the part below the BOX layer corresponds to the aforementioned base silicon of the SOI. This BOX layer can reduce parasitic junction capacitance. Insulating layers can be thermally grown on the upper and lower surfaces of the SOI substrate, with a thickness between 0.1 and 15 μm, and can be insulating materials such as silicon nitride or aluminum oxide. Figure 17 The diagram shows a cross-sectional view of a substrate with an insulating layer, where the upper and lower black areas are the insulating layers.
[0129] Step S1602: On the insulating layer on the upper surface of the substrate, a seed layer, a bottom electrode layer, an intermediate layer and a top electrode layer are deposited sequentially from bottom to top to obtain a first device; wherein, the intermediate layer is a piezoelectric layer, or the intermediate layer is formed by stacking multiple piezoelectric layers and multiple electrode layers; wherein, the layer above the bottom electrode layer and the layer below the top electrode layer are both piezoelectric layers.
[0130] The bottom electrode layer, bottom piezoelectric layer, middle electrode layer, top piezoelectric layer and top electrode layer are grown. For example, the two piezoelectric layers of the piezoelectric MEMS generation unit D10 are single crystal PZT thin films. In this case, the thickness of each PZT is 1.5 μm.
[0131] The material of the piezoelectric layer can be selected from, but is not limited to, one or a combination of the following materials: polycrystalline or single-crystal piezoelectric thin films such as ZnO, AlN, PZT, PVDF, or doped piezoelectric thin films, such as AlN doped with phthalic acid; the thickness of the piezoelectric layer is between 0.1 μm and 25 μm, and the thicknesses of the two piezoelectric thin films can be the same or different.
[0132] A seed layer is beneficial for the high-quality growth of the piezoelectric layer. The materials for the bottom electrode layer, middle electrode layer, and top electrode layer can be selected from, but are not limited to, one or a combination of the following materials: single-crystal or polycrystalline metal thin films such as aluminum, copper, gold, platinum, molybdenum, chromium, and titanium; conductive metal films such as lanthanum nickel oxide (LNO) and SRO; or composite metal layers, such as gold / chromium composite layers. Preferably, the thickness of the Pt electrode is between 0.01 μm and 5 μm. The thickness of each electrode layer film can be the same or different; in this case, the Pt thickness is 0.15 μm.
[0133] like Figure 18 The diagram shown is a cross-sectional view after the growth of the bottom electrode layer, as follows: Figure 19 The diagram shown is a cross-sectional view after the growth of the intermediate layer and the top electrode layer. Figure 19 The intermediate layer is illustrated using two piezoelectric layers as an example.
[0134] Step S1603: The top electrode layer, intermediate layer and bottom electrode layer in the first element are sequentially patterned to form a symmetrical first piezoelectric composite layer at a set of specified edge positions opposite each other on the upper surface of the substrate, so as to obtain the patterned second element.
[0135] By employing key processes such as wet etching and dry etching, the PZT piezoelectric film is etched at an angle, which is beneficial for the step coverage of the passivation layer. The etching angle of the PZT piezoelectric film is 30°-60°, and the over-etching amount of the middle electrode and the bottom electrode is <30%. The roughness of the PZT sidewall is as small as possible. The goal is that after the passivation layer is deposited, there is no delamination between the sliced PZT and the passivation layer.
[0136] The electrode layer and piezoelectric layer in the first element are patterned. After patterning the top electrode layer, top piezoelectric layer, middle electrode layer, bottom piezoelectric layer, and bottom electrode layer, the overlay dimension between each layer is less than 3µm. For example... Figure 20 The figure shown is a graphical cross-sectional schematic diagram. Figure 19 The cross-sectional view is obtained by sequentially graphically processing the top electrode layer, top piezoelectric layer, middle electrode layer, bottom piezoelectric layer and bottom electrode layer.
[0137] The excess piezoelectric and electrode layers in the vibration region are completely removed to maintain the symmetry of the structure and ensure the consistency of the vibration modes. Under driving, the rectangular structure only has odd-order vibration modes such as first, third, and fifth order, and no even-order vibration modes that cancel each other out.
[0138] Step S1604: Deposit a passivation layer on the second element to isolate the electrical connection of each top electrode layer, and pattern the passivation layer to form a pad area to bring out the bottom electrode layer, middle electrode layer and top electrode layer of each first piezoelectric composite layer to obtain the third element.
[0139] The passivation layer isolates the electrical connections between the various electrode layers, providing insulation and protection. A patterned passivation layer leads to the bottom, middle, and top electrode layers, used for electrical connections between different piezoelectric composite layers and for connecting pads (PADs). In this embodiment, the passivation layer needs to have good step coverage to ensure tight adhesion to each film layer. Materials can be selected from, but are not limited to, one or a combination of the following: silicon dioxide, aluminum nitride, PI, alumina, and other oxide insulating materials, or non-conductive organic compounds, with a thickness ranging from 0.05 μm to 5 μm. Figure 21 The diagram shows a passivation layer deposition and a schematic cross-section after patterning.
[0140] Step S1605: Deposit a metal layer in each pad region of the third component to form a pad, thereby obtaining the fourth component;
[0141] like Figure 22 The diagram shows a cross-sectional view of a metal wire after deposition and patterning. In this embodiment, a lift-off process can be used for metal wire deposition and patterning, leading the top and bottom electrode layers to the bonding pads (PADs) and connecting the piezoelectric composite layers of each region, such as parallel or series connections between units. Materials can be selected from, but are not limited to, one or a combination of the following: gold, copper, aluminum, and other metallic materials, or conductive alloy materials, etc., with a thickness ranging from 0.1 to 3 μm.
[0142] Step S1606: Etch a designated area on the upper surface of the fourth element to form multiple groove structures, and cover at least a portion of the groove structures with a flexible material to obtain the fifth element.
[0143] like Figure 23 The diagram shows a cross-sectional view of an SOI top-layer silicon trench after etching. In this embodiment, the SOI top-layer silicon etching uses the DRIE process, which has a good aspect ratio and can etch a specified area of the Si layer on the upper surface of the fourth element's substrate. The etched trench shape can be an inner and outer ring, or a long slot, but it can also be an etched area layer of other shapes, including square, rectangular, or polygonal, etc. The etching thickness can be between 0.5μm and 35μm, and the width of the ring in the circular or square annular trench is between 5μm and 2000μm, etc. Figure 24 The diagram shows a cross-sectional view of a material coated with a flexible thin film, with the slotted gaps covered by the flexible thin film material.
[0144] In step S1607, the bottom surface of the substrate of the fifth element is thinned and the cavity is etched to obtain the MEMS piezoelectric generator; wherein the cavity obtained by etching is located in the central region of the bottom of the substrate.
[0145] In this embodiment, wafer thinning and DRIE etching of the back cavity Si layer and BOX layer can be performed. Specifically, DRIE etching of the back cavity and SOI BOX layer can be used. Wafer thinning to 300μm using CMP (Chemical-Mechanical Planarization) facilitates device thinning. Double-sided exposure technology is used for DRIE etching of the back cavity and SOI BOX layer, thereby obtaining a MEMS piezoelectric generator with a cavity and diaphragm structure, such as... Figure 1 As shown.
[0146] The etching precision of the DRIE back cavity has a significant impact on device performance, especially variations in cavity width. When the cavity etching width exceeds the original design, it reduces the device's resonant frequency; excessively wide etching can even lead to diaphragm breakage. Therefore, the accuracy of the alignment marks, as well as the precision, completeness, and absence of over-etching, require strict process control. The required back cavity etching angle is 90°±1.5°, with no residue and no over-etching.
[0147] The fabrication method of the aforementioned MEMS piezoelectric generator includes: providing an SOI wafer, comprising: a substrate silicon layer, a Box layer (silicon dioxide), and a device silicon layer. A piezoelectric composite layer is deposited on the wafer, and patterned using an etching process to form piezoelectric composite layers in different regions; a passivation layer is deposited to electrically isolate and protect the piezoelectric composite layers in each region, leaving electrode connection areas for electrical connection by metal interconnects; the device silicon layer is etched using an etching process, etching through and onto the diaphragm to form a slotted structure. A flexible dry film material is vacuum laminated, and a flexible thin film is patterned using MEMS techniques, covering the slotted structure; DRIE etching is performed on the back of the device to form the cavity structure of the generator; the process stops at the Box layer, and the Box layer is wet-etched to release the cavity diaphragm structure.
[0148] The aforementioned method for fabricating a MEMS piezoelectric generator reduces internal stress in each diaphragm layer due to manufacturing processes by incorporating a slotted structure. Covering the slotted structure with a flexible material improves the diaphragm's flexibility, reduces sound leakage at low frequencies, and increases the sound pressure level output at low frequencies. Designing a double-layered piezoelectric thin-film rectangular bridge unit structure reinforced at both ends, and an array of multiple units, allows for greater airflow, increasing the vibration amplitude and emitted sound pressure level of the MEMS piezoelectric generator. Replacing the denser silicon diaphragm with a low-density flexible material reduces the diaphragm's mass, and the combination of rigidity and flexibility increases the damping of the diaphragm system, lowering the Q-factor and thus reducing resonance over a wider frequency range. Reducing the nonlinearity caused by large diaphragm offset at the device's resonant frequency lowers total harmonic distortion (THD) and intermodulation distortion (IM), which in turn improves the SPL and THD frequency response curves, thereby enhancing the sound quality of the MEMS piezoelectric generator.
[0149] This embodiment mainly improves the following aspects: (1) The structural form of the MEMS piezoelectric generator, such as cantilever beam, cantilever beam with spring connection or bridge structure, distribution of piezoelectric composite layer, different shapes, sizes and positions of the opening gap, and rectangular device structure covered with flexible material, with different shapes, sizes and positions of the flexible material covering. (2) The process fabrication method of flexible dry film MEMS piezoelectric device. (3) The polarization method based on double-layer piezoelectric PZT film and the electrical connection method of different piezoelectric composite layers. (4) The structure of MEMS piezoelectric loudspeaker array, in which sound generating units with different resonant frequencies can be set in the array structure, so that multiple relatively wide smooth peaks are mixed together and form a frequency response with a relatively flat resonant frequency.
[0150] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, and not to limit them; although the present invention has been described in detail with reference to the foregoing embodiments, those skilled in the art should understand that modifications can still be made to the technical solutions described in the foregoing embodiments, or equivalent substitutions can be made to some or all of the technical features; and these modifications or substitutions do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.
Claims
1. A MEMS piezoelectric sound generator, characterized in that, include: A substrate, wherein a first piezoelectric composite layer is symmetrically disposed at a set of designated edge positions opposite each other on the upper surface of the substrate; Each of the first piezoelectric composite layers is a rectangular structure; The substrate has a cavity in the bottom central region, and at least a portion of each of the first piezoelectric composite layers is located in the upper region of the substrate corresponding to the cavity; In the upper region, a plurality of slotted structures are provided in a designated area excluding at least a portion of each of the first piezoelectric composite layers. At least a portion of the slotted structures are covered with a flexible material. The upper region with the flexible material forms the diaphragm structure of the MEMS piezoelectric transmitter. The diaphragm structure is a rectangular bridge structure. The first diaphragm edge of the diaphragm structure is an anchored edge, and the other diaphragm edges are non-anchored edges. An edge slotted structure is provided at each of the non-anchored edges. The first diaphragm edge is determined according to the relative position of the first piezoelectric composite layer on the substrate. Wherein, if the first piezoelectric composite layer is located on the left side of the substrate, the left diaphragm edge of the diaphragm structure is an anchored edge; if the first piezoelectric composite layer is located on the right side of the substrate, the right diaphragm edge of the diaphragm structure is an anchored edge. The length and width dimensions covered by the flexible material are larger than the length and width dimensions of the slotted structure. The upper region of the substrate has at least one second piezoelectric composite layer; each second piezoelectric composite layer has a slotted structure; the slotted structure is covered with a flexible material; the second piezoelectric composite layer is divided into two or more parts, each part having the shape of a circle, hexagon, octagon or irregular graphic structure.
2. The MEMS piezoelectric sound generator according to claim 1, characterized in that, The edge slot structures corresponding to the two opposite non-anchored edges are parallel to each other, and the dimensions of the edge slot structures are the same.
3. The MEMS piezoelectric sound generator according to claim 1, characterized in that, The diaphragm structure is parallel to the upper surface of the substrate, and at least a portion of the anchoring edge is fixed to the substrate.
4. The MEMS piezoelectric sound generator according to claim 1, characterized in that, A slotted structure is provided in the designated area, except for each of the second piezoelectric composite layers.
5. The MEMS piezoelectric sound generator according to claim 1, characterized in that, The aspect ratio of the diaphragm structure is greater than a preset value; As the aspect ratio of the diaphragm structure increases, the first-order resonant frequency of the MEMS piezoelectric generator increases, and the difference between the resonant frequencies decreases.
6. The MEMS piezoelectric sound generator according to claim 5, characterized in that, The thickness of the diaphragm structure ranges from 0.1 μm to 50 μm. As the thickness of the diaphragm structure decreases, the value of the first-order resonant frequency decreases. Under the same piezoelectric drive, the deflection displacement generated by the diaphragm structure is greater, and the amount of air pushed out is greater.
7. The MEMS piezoelectric sound generator according to claim 5, characterized in that, The larger the size of the cavity, the smaller the value of the first-order resonant frequency; wherein the size includes at least one of the following: cavity area, cavity length, cavity width, cavity radius, and cavity diameter.
8. The MEMS piezoelectric sound generator according to claim 1, characterized in that, The neutral layer of the diaphragm structure is located at the center of the diaphragm structure.
9. The MEMS piezoelectric sound generator according to claim 4, characterized in that, Each of the first piezoelectric composite layers and each of the second piezoelectric composite layers comprises, from bottom to top, a bottom electrode layer, an intermediate layer, and a top electrode layer; wherein, the intermediate layer is a piezoelectric layer, or, the intermediate layer is formed by overlapping and stacking multiple piezoelectric layers and multiple electrode layers; wherein, the layer above the bottom electrode layer and the layer below the top electrode layer are both piezoelectric layers.
10. A method for fabricating a MEMS piezoelectric generator, the method being used to fabricate the MEMS piezoelectric generator according to any one of claims 1-9; characterized in that, The method includes: Insulating layers are thermally oxidized to grow on the upper and lower surfaces of the preset substrate, respectively; A seed layer, a bottom electrode layer, an intermediate layer, and a top electrode layer are deposited sequentially from bottom to top on an insulating layer on the upper surface of the substrate to obtain a first element; wherein the intermediate layer is a piezoelectric layer, or the intermediate layer is formed by stacking multiple piezoelectric layers and multiple electrode layers; wherein the layer above the bottom electrode layer and the layer below the top electrode layer are both piezoelectric layers. The top electrode layer, the intermediate layer and the bottom electrode layer in the first element are sequentially patterned to form a symmetrical first piezoelectric composite layer at a set of specified edge positions opposite each other on the upper surface of the substrate, thus obtaining the patterned second element. A passivation layer is deposited on the second element to isolate the electrical connections of each of the top electrode layers, and the passivation layer is patterned to form pad areas to bring out the bottom electrode layer, middle electrode layer and top electrode layer of each of the first piezoelectric composite layers, thus obtaining the third element. A metal layer is deposited on each of the pad regions in the third element to form a pad, thereby obtaining the fourth element; A designated area on the upper surface of the fourth element is etched to form multiple slotted structures, and at least a portion of the slotted structures are covered with a flexible material to obtain the fifth element. The bottom surface of the substrate of the fifth element is thinned and etched with cavities to obtain a MEMS piezoelectric generator; wherein the etched cavity is located in the bottom center region of the substrate; at least a portion of each of the first piezoelectric composite layers is located in the upper region of the substrate corresponding to the cavity; the upper region having a flexible material forms the diaphragm structure of the MEMS piezoelectric generator; the first diaphragm edge of the diaphragm structure is an anchoring edge, and the first diaphragm edge is determined according to the relative position of the first piezoelectric composite layer on the substrate; wherein, if the first piezoelectric composite layer is located on the left side of the substrate, the left diaphragm edge of the diaphragm structure is the anchoring edge, and if the first piezoelectric composite layer is located on the right side of the substrate, the right diaphragm edge of the diaphragm structure is the anchoring edge; the length and width dimensions covered by the flexible material are larger than the length and width dimensions of the slotted structure.
Citation Information
Patent Citations
Sound emitting unit and manufacturing method thereof
CN115334441A
Piezoelectric MEMS (Micro Electro Mechanical System) sounder, loudspeaker and sounder manufacturing method
CN116887153A
Piezoelectric MEMS transducer and operation method and preparation method thereof
CN116887154A
MEMS piezoelectric sounder and loudspeaker
CN222547621U