Core-shell structure polymer, aqueous primer slurry, secondary battery, and electric device
Patent Information
- Application Number
- CN202280092954.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2022-11-04
- Publication Date
- 2024-10-15
AI Technical Summary
In the existing secondary battery pole plate primer coating process, the aqueous primer slurry has high viscosity and poor filterability, resulting in low production efficiency and narrow process window, making it difficult to meet production needs.
Develop a core-shell structure polymer that polymerizes vinylidene fluoride, acrylic acid, and styrene monomers to form a core with high thermal stability and a cohesive shell to reduce slurry viscosity, improve filterability, and broaden the process window to optimize the base coating production process.
It significantly improves the filterability and dispersibility of the water-based primer slurry, reduces the diaphragm resistance of the pole piece, enhances the adhesive force and dynamic performance of the pole piece, and improves production efficiency.
Smart Images

Figure CN118786157A_ABST
Abstract
Description
Core-shell polymers, water-based primer slurries, secondary batteries, electrical devices Technical Field
[0001] The present application relates to the technical field of secondary batteries, and in particular to a core-shell polymer, a preparation method, an aqueous primer slurry, a secondary battery, and an electrical device. Background Art
[0002] During the production of secondary battery electrodes, a primer is applied between the current collector and the active material layer. This provides electrical conductivity between the active material layer and the current collector, thereby reducing the contact resistance between the two. This primer is typically prepared by applying a primer slurry composed of a binder, a conductive agent, and additives to the current collector surface. However, existing primer slurries suffer from a short processing window, poor filterability, and the tendency for precipitation to clog pipelines, severely impacting electrode production efficiency. Therefore, the development of a binder to improve the slurry's processing performance is urgently needed.
[0003] Summary of the Invention
[0004] The present application is made in view of the above-mentioned problems, and its purpose is to provide a core-shell structure polymer and an aqueous primer slurry containing the core-shell structure polymer, so as to optimize the process window for preparing the aqueous primer slurry and improve the production efficiency of the aqueous primer slurry.
[0005] The first aspect of the present application provides a core-shell structure polymer, comprising a core portion and a shell portion at least partially covering the core portion, wherein the core portion comprises a structural unit derived from a monomer represented by Formula I, and the shell portion comprises a structural unit derived from a monomer represented by Formula I, a structural unit derived from a monomer represented by Formula II, and a structural unit derived from a monomer represented by Formula III.
[0006]
[0007] wherein R1, R2, and R3 are each independently selected from hydrogen, fluorine, chlorine, or a C 1-3 Alkyl, R4, R5, R6, R7, R8, R9 are each independently selected from hydrogen, substituted or unsubstituted C 1-5 Ar is an alkyl group, and Ar is a substituted or unsubstituted aromatic group.
[0008] The core-shell structure polymer provided in this application can reduce the viscosity of the slurry, improve the filterability of the slurry, significantly broaden the process window of the slurry, and improve the processability of the slurry, so that the slurry can meet the production requirements of the primer without adding a dispersant, which is beneficial to optimizing the production process of the primer and improving its production efficiency.
[0009] In any embodiment, R1 is fluorine, R2 and R3 are each independently selected from hydrogen, fluorine, chlorine or trifluoromethyl, and R4, R5, R6, R7, R8 and R9 are each independently selected from hydrogen or methyl.
[0010] In any embodiment, the mass content of the core portion is 40% to 50% based on the mass of the core-shell structure polymer.
[0011] By controlling the mass content of the core within an appropriate range, the core-shell structure polymer can take into account both the viscosity of the slurry and the adhesion of the electrode, and comprehensively improve the processing performance and usage performance of the water-based primer slurry.
[0012] In any embodiment, the mass content of the structural unit derived from the monomer represented by Formula II is 10% to 40%, based on the mass of the core-shell structure polymer.
[0013] By controlling the mass content of the structural unit derived from the monomer represented by Formula II within an appropriate range, it is possible to balance the viscosity of the slurry and the adhesion of the electrode, thereby comprehensively improving the processing performance and use performance of the slurry.
[0014] In any embodiment, the mass content of the structural unit derived from the monomer represented by formula III is 10% to 40%, based on the mass of the core-shell structure polymer.
[0015] By controlling the mass content of the structural unit derived from the monomer represented by Formula III within an appropriate range, it is possible to balance the viscosity of the slurry and the adhesion of the electrode, thereby comprehensively improving the processing performance and use performance of the slurry.
[0016] In any embodiment, the core-shell structure polymer has a weight average molecular weight of 300,000 to 500,000.
[0017] By controlling the weight-average molecular weight of the core-shell structure polymer within an appropriate range, both the electrode adhesion and the membrane resistance can be taken into account, thereby comprehensively improving the electrode adhesion and dynamic performance.
[0018] In any embodiment, the core-shell structured polymer has a Dv50 particle size of 100 nm to 10 μm.
[0019] In any embodiment, the monomer represented by formula I is selected from one or more of vinylidene fluoride, tetrafluoroethylene, chlorotrifluoroethylene, and hexafluoropropylene.
[0020] In any embodiment, the monomer represented by formula II is selected from one or both of acrylic acid and methacrylic acid.
[0021] In any embodiment, the monomer represented by formula III is selected from one or both of styrene and 4-methylstyrene.
[0022] The second aspect of the present application provides a method for preparing a core-shell structure polymer, the preparation method comprising the following steps: polymerizing the monomer represented by formula I under polymerizable conditions to prepare the core portion of the core-shell structure polymer; polymerizing the monomer represented by formula I, the monomer represented by formula II, and the monomer represented by formula III to prepare the shell portion of the core-shell structure polymer, wherein the shell portion at least partially covers the core portion;
[0023]
[0024] wherein R1, R2, and R3 are each independently selected from hydrogen, fluorine, chlorine, or a C 1-3 Alkyl, R4, R5, R6, R7, R8, R9 are each independently selected from hydrogen, substituted or unsubstituted C 1-5 Ar is an alkyl group, and Ar is a substituted or unsubstituted aromatic group.
[0025] The core-shell structure polymer prepared by this method can reduce the viscosity of the slurry, improve the filterability of the slurry, significantly broaden the process window of the slurry, and improve the processability of the slurry, so that the slurry can meet the production requirements of the primer without adding a dispersant, which is conducive to optimizing the production process of the primer and improving its production efficiency.
[0026] In any embodiment, R1 is fluorine, R2 and R3 are each independently selected from one or more of hydrogen, fluorine, chlorine, and trifluoromethyl, and R4, R5, R6, R7, R8, and R9 are each independently selected from one or two of hydrogen and methyl.
[0027] In any embodiment, the mass content of the core portion is 40% to 50% based on the mass of the core-shell structure polymer.
[0028] In any embodiment, the mass content of the monomer represented by formula II is 10% to 40%, based on the total mass of the monomer represented by formula I, the monomer represented by formula II, and the monomer represented by formula III.
[0029] In any embodiment, the mass content of the monomer represented by formula III is 10% to 40%, based on the total mass of the monomer represented by formula I, the monomer represented by formula II, and the monomer represented by formula III.
[0030] In any embodiment, the preparation method comprises a first stage polymerization and a second stage polymerization,
[0031] First stage polymerization: providing an initiator, a first emulsifier, at least one monomer represented by formula I and an aqueous medium to carry out a first stage polymerization reaction to obtain a core portion, and continuously feeding the monomer represented by formula I during the first stage polymerization reaction;
[0032] Second stage polymerization: After a period of reaction, an initiator, a second emulsifier, at least one monomer represented by formula II and a monomer represented by formula III, and an aqueous medium are added to the reaction vessel to carry out a second stage polymerization reaction to obtain a core-shell structure polymer, and the monomer represented by formula I is continuously input during the second stage polymerization reaction.
[0033] The method provided in the present application is to form a fluorine-containing core portion by first continuously feeding the monomer shown in formula I, so that the core portion has high thermal stability; and then the monomer shown in formula I, the monomer shown in formula II and the monomer shown in formula III are introduced to form a core-shell structure polymer. In the emulsion system, a core-shell structure polymer is obtained by polymerizing monomers with different hydrophilicities in a step-by-step manner. The core-shell structure polymer exists in the form of a core-shell structure in an aqueous medium. Compared with the non-core-shell structure polymer prepared by simultaneously passing all the monomers into the reaction vessel, the stability and dispersibility of the core-shell structure polymer are greatly improved, the filterability and dispersibility of the water-based primer slurry are improved, the membrane resistance of the electrode is reduced, and the process window of the slurry is further widened, which helps to improve the production efficiency of the water-based primer. At the same time, since the structural units derived from the monomer shown in formula II are all distributed in the shell portion, the carboxyl group of the shell portion can improve the adhesion of the core-shell structure polymer, thereby improving the adhesion of the electrode. In addition, when the monomers represented by formula II and formula III are fed into the reaction vessel for the second stage polymerization, the monomer represented by formula I is continued to be fed into the reaction vessel to increase the compatibility of the core and shell parts and improve the stability of the core-shell structure polymer.
[0034] In any embodiment, the second stage polymerization comprises:
[0035] After adding the initiator into the reaction container, a premixed solution comprising a second emulsifier, at least one monomer represented by formula II, a monomer represented by formula III and an aqueous medium is added.
[0036] In any embodiment, the mass of the monomer of formula I introduced in the first stage polymerization is 70% to 85% of the total mass of the monomer of formula I supplied in the polymerization reaction, and the mass of the monomer of formula I introduced in the second stage polymerization reaction is 15% to 30% of the total mass of the monomer of formula I supplied in the polymerization reaction.
[0037] In any embodiment, the initiator provided in the first stage polymerization and the initiator provided in the second stage polymerization are both persulfate, the mass percentage of the initiator provided in the first stage polymerization is 0.05% to 0.075%, and the mass percentage of the initiator provided in the second stage polymerization is 0.05% to 0.075%, based on the total mass of the monomer represented by formula I, the monomer represented by formula II, and the monomer represented by formula III.
[0038] In any embodiment, the mass percentage of the first emulsifier is 0.28% to 0.42%, based on the total mass of the monomer represented by formula I, the monomer represented by formula II, and the monomer represented by formula III.
[0039] In any embodiment, the mass percentage of the second emulsifier is 0.8% to 1.2%, based on the total mass of the monomer represented by formula I, the monomer represented by formula II, and the monomer represented by formula III.
[0040] In any embodiment, the mass percentage of the aqueous medium provided in the first stage polymerization is 200% to 500%, and the mass percentage of the aqueous medium provided in the second stage polymerization is 100% to 200%, based on the total mass of the monomer represented by formula I, the monomer represented by formula II, and the monomer represented by formula III.
[0041] In any embodiment, the reaction pressure of the first stage polymerization is 5.5 MPa to 7.5 MPa, and the reaction temperature is 75° C. to 85° C.
[0042] In any embodiment, the reaction pressure of the second polymerization is 4.5 MPa to 6.5 MPa, and the reaction temperature is 86° C. to 95° C.
[0043] In any embodiment, the initiator may be selected from one or both of potassium persulfate and ammonium persulfate.
[0044] In any embodiment, the first emulsifier is an alkali metal perfluorooctanoate.
[0045] In any embodiment, the second emulsifier is one or both of polyoxyethylene-4-phenol ether ammonium sulfate and nonylphenol polyoxyethylene ether ammonium sulfate.
[0046] The third aspect of the present application provides an emulsion-type adhesive, which comprises the core-shell structure polymer described in the first aspect.
[0047] The emulsion-type binder is a direct product of the preparation method of the core-shell structure polymer of the second aspect, and can be directly used as a binder for water-based primer slurry, thereby reducing production costs and improving production efficiency.
[0048] The fourth aspect of the present application provides the use of the core-shell structure polymer described in the first aspect in a secondary battery.
[0049] The fifth aspect of the present application provides an aqueous primer slurry, comprising a binder, a conductive agent and an aqueous medium, wherein the binder comprises the core-shell structure polymer described in the first aspect.
[0050] Compared with non-core-shell structured polymers, core-shell structured polymers have improved stability and dispersibility, which improves the filterability and dispersibility of water-based primer slurry and reduces the diaphragm resistance of the electrode.
[0051] In any embodiment, the core-shell structure polymer is added to the aqueous base coating slurry in the form of an emulsion containing the core-shell structure polymer.
[0052] The core-shell structure polymer prepared by the preparation method described in the second aspect above is in the form of an emulsion and can be directly added to an aqueous primer slurry for use, thereby reducing production costs and improving production efficiency.
[0053] In any embodiment, the mass ratio of the conductive agent to the binder is 0.8:1 to 1:1.
[0054] By controlling the mass ratio of the conductive agent to the binder within an appropriate range, the bonding strength of the slurry electrode and the diaphragm resistance can be taken into account, and the bonding performance and dynamic performance of the electrode can be comprehensively improved.
[0055] In any embodiment, when the solid content of the aqueous primer slurry is 10% to 20%, the viscosity of the aqueous primer slurry is 300 mPa·s to 900 mPa·s.
[0056] Controlling the solid content of the water-based primer slurry within an appropriate range can take into account both the viscosity of the slurry and the adhesion of the electrode, and comprehensively improve the processing performance and performance of the slurry.
[0057] The viscosity of the aqueous primer slurry with a solid content of 10% to 20% is 300mPa·s to 900mPa·s, which means that the aqueous primer slurry prepared from the core-shell structure polymer does not need to add additional dispersants or thickeners to improve processing performance, which helps to improve production efficiency and optimize the production process.
[0058] A sixth aspect of the present application provides a method for preparing a water-based primer layer, comprising the following steps:
[0059] Using a gravure coater, coating the aqueous primer slurry described in the fifth aspect on the surface of the current collector;
[0060] After drying, a water-based primer layer is obtained, and the thickness of the water-based primer layer is 1 μm to 3 μm.
[0061] The preparation method of the water-based primer layer disclosed in the present application can improve the bonding force of the electrode sheet and reduce the membrane resistance of the electrode sheet.
[0062] The seventh aspect of the present application provides a secondary battery comprising a positive electrode sheet, a separator, a negative electrode sheet, and an electrolyte, wherein the positive electrode sheet and / or the negative electrode sheet comprises a water-based primer layer prepared by the preparation method described in the sixth aspect of the present application.
[0063] In any embodiment, the secondary battery includes at least one of a lithium ion battery, a sodium ion battery, a magnesium ion battery, and a potassium ion battery.
[0064] An eighth aspect of the present application provides a battery module including the secondary battery according to the seventh aspect of the present application.
[0065] A ninth aspect of the present application provides a battery pack comprising the secondary battery of the seventh aspect of the present application or the battery module of the eighth aspect of the present application.
[0066] The tenth aspect of the present application provides an electrical device comprising at least one selected from the secondary battery of the seventh aspect of the present application, the battery module of the eighth aspect of the present application, or the battery pack of the ninth aspect of the present application. BRIEF DESCRIPTION OF THE DRAWINGS
[0067] FIG1 is a schematic structural diagram of a core-shell polymer according to an embodiment of the present invention;
[0068] FIG2 is a schematic diagram of a secondary battery according to an embodiment of the present application;
[0069] FIG3 is an exploded view of the secondary battery according to one embodiment of the present application shown in FIG2 ;
[0070] FIG4 is a schematic diagram of a battery module according to an embodiment of the present application;
[0071] FIG5 is a schematic diagram of a battery pack according to an embodiment of the present application;
[0072] FIG6 is an exploded view of the battery pack shown in FIG5 according to an embodiment of the present application;
[0073] FIG. 7 is a schematic diagram of an electric device using a secondary battery as a power source according to an embodiment of the present application.
[0074] Reference numerals:
[0075] 1 battery pack; 2 upper case; 3 lower case; 4 battery module; 5 secondary battery; 51 shell; 52 electrode assembly; 53 cover; 6 core-shell structure polymer; 61 core; 62 shell. DETAILED DESCRIPTION
[0076] Below, the embodiments of the binder, preparation method, electrode, battery, and electrical device of the present application are described in detail with appropriate reference to the accompanying drawings. However, there may be cases where unnecessary detailed descriptions are omitted. For example, there may be cases where detailed descriptions of well-known matters and repeated descriptions of actually the same structures are omitted. This is to avoid the following description from becoming unnecessarily lengthy and to facilitate understanding by those skilled in the art. In addition, the drawings and the following description are provided to enable those skilled in the art to fully understand the present application and are not intended to limit the subject matter described in the claims.
[0077] " range " disclosed in the present application is limited in the form of lower limit and upper limit, and given range is limited by selecting a lower limit and an upper limit, and the selected lower limit and upper limit define the boundary of special range. The scope limited in this way can be to include end value or not include end value, and can be arbitrarily combined, that is, any lower limit can form a range with any upper limit combination. For example, if the scope of 60-120 and 80-110 is listed for specific parameters, it is understood that the scope of 60-110 and 80-120 is also expected. In addition, if the minimum range value 1 and 2 are listed, and if the maximum range value 3,4 and 5 are listed, then the following range can all be expected: 1-3, 1-4, 1-5, 2-3, 2-4 and 2-5. In this application, unless otherwise specified, the numerical range " ab " represents the abbreviation of any real number combination between a and b, wherein a and b are all real numbers. For example, a numerical range of "0-5" indicates that all real numbers between "0-5" are listed herein, and "0-5" is simply an abbreviation for these numerical combinations. Furthermore, when a parameter is expressed as an integer ≥ 2, this is equivalent to disclosing that the parameter is, for example, an integer of 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc.
[0078] Unless otherwise specified, all embodiments and optional embodiments of the present application can be combined with each other to form a new technical solution.
[0079] Unless otherwise specified, all technical features and optional technical features of this application can be combined with each other to form a new technical solution.
[0080] Unless otherwise specified, all steps of the present application may be performed sequentially or randomly, preferably sequentially. For example, the method includes steps (a) and (b), indicating that the method may include steps (a) and (b) performed sequentially, or may include steps (b) and (a) performed sequentially. For example, the method may further include step (c), indicating that step (c) may be added to the method in any order, for example, the method may include steps (a), (b) and (c), or may include steps (a), (c) and (b), or may include steps (c), (a) and (b), etc.
[0081] Unless otherwise specified, the terms "include" and "comprising" used in this application may be open-ended or closed-ended. For example, "include" and "comprising" may mean that other components not listed may also be included or that only the listed components are included.
[0082] Unless otherwise specified, the term "or" is used in this application to be inclusive. For example, the phrase "A or B" means "A, B, or both A and B." More specifically, the condition "A or B" is satisfied if any of the following conditions are met: A is true (or exists) and B is false (or does not exist); A is false (or does not exist) and B is true (or exists); or both A and B are true (or exist).
[0083] The conductivity of the electrode is one of the most important research topics in secondary batteries. During the preparation process of the secondary battery electrode, a primer layer is applied between the current collector and the active material layer to provide electrical conduction between the active material layer and the current collector, thereby reducing the contact resistance between the active material layer and the current collector, making the electrode have good electronic conductivity and ionic conductivity, and improving the dynamic performance of the battery. In the prior art, binders and conductive agents are generally used to prepare the primer layer. Traditional polyvinylidene fluoride binders will make the slurry have high viscosity and poor filterability, making it difficult to apply evenly. Therefore, a dispersant needs to be added during the slurry preparation process to improve the processing performance of the slurry. This will undoubtedly increase the processing difficulty of the slurry, affect production efficiency and lead to poor stability of the slurry between batches. Based on the above technical problems, the present application has developed a binder that gives the water-based primer slurry a suitable viscosity and excellent filterability to improve the production efficiency and production quality of the primer layer.
[0084] [Core-shell polymer]
[0085] Based on this, the present application provides a core-shell structure polymer, comprising a core portion and a shell portion at least partially covering the core portion, wherein the core portion comprises a structural unit derived from a monomer represented by Formula I, and the shell portion comprises a structural unit derived from a monomer represented by Formula I, a structural unit derived from a monomer represented by Formula II, and a structural unit derived from a monomer represented by Formula III.
[0086]
[0087] wherein R1, R2, and R3 are each independently selected from hydrogen, fluorine, chlorine, or a C 1-3 Alkyl, R4, R5, R6, R7, R8, R9 are each independently selected from hydrogen, substituted or unsubstituted C 1-5 Ar is an alkyl group, and Ar is a substituted or unsubstituted aromatic group.
[0088] As used herein, the term "polymer" includes, on the one hand, a collection of chemically homogeneous macromolecules prepared by polymerization, but differing in degree of polymerization, molar mass, and chain length. The term also includes derivatives of such collections of macromolecules formed by polymerization, i.e., products that can be obtained by reaction of functional groups in the aforementioned macromolecules, such as addition or substitution, and can be chemically homogeneous or chemically heterogeneous.
[0089] As used herein, the term "trifluoromethyl" refers to a -CF3 group.
[0090] In this article, the term “C 1-5 "Alkyl" refers to a straight or branched hydrocarbon chain radical consisting solely of carbon and hydrogen atoms, with no unsaturation present, having from one to five carbon atoms, and attached to the remainder of the molecule by a single bond. 1-3 "Alkyl" should be interpreted accordingly. C 1-5 Examples of alkyl groups include, but are not limited to, methyl, ethyl, n-propyl, 1-methylethyl (isopropyl), butyl, and pentyl. In some embodiments, C 1-3 Alkyl is -CF3, -CH3CH2F or -CH2FCH2F.
[0091] As used herein, the term "substituted" refers to a compound or chemical moiety in which at least one hydrogen atom is replaced by another chemical moiety, wherein the substituents are each independently selected from the group consisting of hydroxyl, thiol, amino, cyano, nitro, aldehyde, halogen, alkenyl, alkynyl, aryl, heteroaryl, C 1-6 Alkyl, C 1-6 Alkoxy.
[0092] As used herein, the term "aromatic group" refers to a functional group or substituent derived from a simple aromatic ring, such as phenyl, o-tolyl, 1-naphthyl (or α-naphthyl).
[0093] In some embodiments, R1 is fluorine, R2 and R3 are each independently selected from one or more of hydrogen, fluorine, chlorine, and trifluoromethyl, and R4, R5, R6, R7, R8, and R9 are each independently selected from one or two of hydrogen and methyl.
[0094] In some embodiments, the monomer represented by formula I is selected from one or more of vinylidene fluoride, tetrafluoroethylene, chlorotrifluoroethylene, and hexafluoropropylene.
[0095] In some embodiments, the monomer represented by Formula II is selected from one or both of acrylic acid and methacrylic acid.
[0096] In some embodiments, the monomer represented by formula III is selected from one or both of styrene and 4-methylstyrene.
[0097] Figure 1 is a schematic structural diagram of a core-shell structure polymer in one embodiment of the present application, wherein the core-shell structure polymer 6 includes a core portion 61 and a shell portion 62, wherein the shell portion 62 covers the surface of the core portion 61, and the core portion 61 includes a structural unit derived from a monomer shown in Formula I, and the core portion 61 includes a fluorine-containing structural unit, which can increase the thermal stability of the structure; the shell portion includes a structural unit derived from a monomer shown in Formula I, a structural unit derived from a monomer shown in Formula II, and a structural unit derived from a monomer shown in Formula III, and the shell portion includes a carboxyl group, which can improve the bonding performance of the structure. Compared to traditional polyvinylidene fluoride, the core-shell structure polymer has a fluorine-containing unit located in the core portion and a non-fluorine unit located in the shell portion, which reduces the contact area between the fluorine-containing structural unit and the solvent, thereby reducing the viscosity of the slurry, stabilizing the slurry, and alleviating the sedimentation of the slurry, and effectively improving the filterability of the slurry.
[0098] The core-shell structure polymer provided in this application can reduce the viscosity of the slurry, improve the filterability of the slurry, significantly broaden the process window of the slurry, and improve the processability of the slurry, so that the slurry can meet the production requirements of the water-based primer without adding a dispersant, which is conducive to optimizing the production process of the water-based primer and improving its production efficiency.
[0099] In this article, the term "process window" refers to the process range that can ensure product quality, including but not limited to temperature range, pressure range, storage time length, etc. It can be understood that the wider the process window, the lower the requirement for process accuracy.
[0100] In some embodiments, the mass content of the core portion is 40% to 50% based on the mass of the core-shell polymer. In some embodiments, the mass content of the core portion can be any one of 40%, 45%, and 50% based on the mass of the core-shell polymer.
[0101] Controlling the mass content of the core within an appropriate range allows the slurry to have an appropriate viscosity. This not only allows the electrode to have good adhesion, but also allows for subsequent coating processing and coating drying, thereby comprehensively improving the processing and performance of the slurry.
[0102] In some embodiments, the mass content of the structural unit derived from the monomer represented by Formula II is 10% to 40%, based on the mass of the core-shell structure polymer. In some embodiments, the mass content of the structural unit derived from the monomer represented by Formula II can be any one of 10%, 20%, 30%, and 40%, based on the mass of the core-shell structure polymer.
[0103] The mass content of the structural unit derived from the monomer represented by Formula II is controlled within an appropriate range so that the slurry has an appropriate viscosity. On the one hand, this allows the electrode to have good adhesion, and on the other hand, it can also take into account the subsequent coating processing and coating drying work, thereby comprehensively improving the processing performance and use performance of the slurry.
[0104] In some embodiments, the mass content of the structural unit derived from the monomer represented by formula III is 10% to 40%, based on the mass of the core-shell structure polymer. In some embodiments, the mass content of the structural unit derived from the monomer represented by formula III can be any one of 10%, 20%, 30%, and 40%, based on the mass of the core-shell structure polymer.
[0105] The mass content of the structural unit derived from the monomer represented by Formula III is controlled within an appropriate range so that the slurry has an appropriate viscosity. On the one hand, it enables the electrode to have good adhesion, and on the other hand, it can also take into account the subsequent coating processing and coating drying work, thereby comprehensively improving the processing performance and use performance of the slurry.
[0106] In some embodiments, the weight average molecular weight of the core-shell structure polymer is 300,000 to 500,000. In some embodiments, the weight average molecular weight of the core-shell structure polymer can be any one of 300,000, 400,000, and 500,000.
[0107] As used herein, the term "weight average molecular weight" refers to the sum of the weight fractions of molecules of different molecular weights in a polymer multiplied by their corresponding molecular weights.
[0108] In the present application, the weight-average molecular weight of the polymer can be tested using methods known in the art, such as gel chromatography, such as using a Waters 2695Isocratic HPLC gel chromatograph (differential refractive index detector 2141). In some embodiments, the testing method is to use a polystyrene solution sample with a mass fraction of 3.0% as a reference and select a matching chromatographic column (oily: Styragel HT5DMF7.8*300mm+Styragel HT4). Use purified N-methylpyrrolidone (NMP) solvent to prepare a 3.0% core-shell structure polymer glue, and let the prepared solution stand for one day for use. During the test, first use a syringe to draw tetrahydrofuran, rinse, and repeat several times. Then draw 5 ml of the experimental solution, expel the air in the syringe, and wipe the needle tip dry. Finally, slowly inject the sample solution into the injection port. After the reading stabilizes, obtain data and read the weight-average molecular weight.
[0109] Controlling the weight average molecular weight of the core-shell structure polymer within an appropriate range is beneficial to the dispersion of the core-shell structure polymer in the aqueous primer slurry, making it less likely to agglomerate with the conductive agent, thereby improving the dispersibility of the conductive agent and reducing the diaphragm resistance of the electrode; at the same time, the core-shell structure polymer with a weight average molecular weight within an appropriate range can form a three-dimensional network bonding structure, playing an effective bonding role.
[0110] In summary, controlling the weight-average molecular weight of the core-shell structure polymer within an appropriate range can take into account both the adhesion of the electrode and the membrane resistance, and comprehensively improve the adhesion and dynamic properties of the electrode.
[0111] In some embodiments, the Dv50 particle size of the core-shell structure polymer is 100 nm to 10 μm. In some embodiments, the Dv50 particle size of the core-shell structure polymer can be any one of 100 nm to 1000 nm, 500 nm to 1000 nm, and 500 nm to 10 μm.
[0112] In this article, the term "Dv50 particle size" refers to the particle size corresponding to when the cumulative particle size distribution number of particles reaches 50% in the particle size distribution curve. Its physical meaning is that particles with a particle size smaller than (or larger than) it account for 50%.
[0113] In one embodiment of the present application, a method for preparing a core-shell structure polymer is provided, the preparation method comprising the following steps:
[0114] The core portion of the core-shell structure polymer is prepared by polymerizing the monomer represented by formula I under polymerizable conditions, and the shell portion of the core-shell structure polymer is prepared by polymerizing the monomer represented by formula I, the monomer represented by formula II, and the monomer represented by formula III, wherein the shell portion at least partially covers the core portion.
[0115]
[0116] wherein R1, R2, and R3 are each independently selected from hydrogen, fluorine, chlorine, or a C 1-3 Alkyl, R4, R5, R6, R7, R8, R9 are each independently selected from hydrogen, substituted or unsubstituted C 1-5 Ar is an alkyl group, and Ar is a substituted or unsubstituted aromatic group.
[0117] As used herein, the term "polymerizable conditions" refers to those conditions including temperature, pressure, reactant concentrations, optional solvents / diluents, reactant mixing / addition parameters selected by one skilled in the art, and other conditions that facilitate the reaction of one or more monomers within at least one polymerization reactor.
[0118] The core-shell structure polymer prepared by this method can reduce the viscosity of the slurry, improve the filterability of the slurry, significantly broaden the process window of the slurry, and improve the processability of the slurry, so that the slurry can meet the production requirements of water-based primer without adding dispersants, which is conducive to optimizing the production process of water-based primer and improving its production efficiency.
[0119] In some embodiments, R1 is fluorine, R2 and R3 are each independently selected from hydrogen, fluorine, chlorine or trifluoromethyl, and R4, R5, R6, R7, R8 and R9 are each independently selected from hydrogen or methyl.
[0120] In some embodiments, the mass content of the core portion is 40% to 50%, based on the mass of the core-shell structure polymer. In some embodiments, the mass content of the core portion can be any one of 40%, 45%, and 50%.
[0121] In some embodiments, the weight content of the monomer represented by Formula II is 10% to 40%, based on the total weight of the monomer represented by Formula I, the monomer represented by Formula II, and the monomer represented by Formula III. In some embodiments, the weight content of the monomer represented by Formula II can be any one of 10%, 20%, 30%, and 40%, based on the total weight of the monomer represented by Formula I, the monomer represented by Formula II, and the monomer represented by Formula III.
[0122] In some embodiments, the mass content of the monomer represented by formula III can be any one of 10%, 20%, 30%, and 40%, based on the total mass of the monomer represented by formula I, the monomer represented by formula II, and the monomer represented by formula III.
[0123] In some embodiments, the preparation method includes a first stage polymerization and a second stage polymerization,
[0124] First stage polymerization: providing an initiator, a first emulsifier, at least one monomer represented by formula I and an aqueous medium to carry out a first stage polymerization reaction to obtain a core portion, and continuously feeding the monomer represented by formula I during the first stage polymerization reaction;
[0125] Second stage polymerization: After a period of reaction, an initiator, a second emulsifier, at least one monomer represented by formula II and a monomer represented by formula III, and an aqueous medium are added to the reaction vessel to carry out a second stage polymerization reaction to obtain a core-shell structure polymer, and the monomer represented by formula I is continuously input during the second stage polymerization reaction.
[0126] The method provided by the present application is to form a fluorine-containing core by first continuously feeding the monomer shown in formula I so that the core has high thermal stability; and then the monomer shown in formula I, the monomer shown in formula II and the monomer shown in formula III are introduced to form a core-shell structure polymer. In the emulsion system, the hydrophobic monomer shown in formula I is first added to carry out the first stage of polymerization to form the core, and then the hydrophilic monomer shown in formula II, the monomer shown in formula III and the monomer shown in formula I are added to carry out the second stage of polymerization to form the shell. The generated core-shell structure polymer exists in the form of a core-shell structure in the aqueous medium. Compared with the non-core-shell structure polymer prepared by simultaneously passing all the monomers into the reaction vessel, the stability and dispersibility of the core-shell structure polymer are greatly improved, the filterability and dispersibility of the water-based primer slurry are improved, the membrane resistance of the electrode is reduced, and the process window of the slurry is further widened, which helps to improve the production efficiency of the water-based primer. At the same time, since the structural units derived from the monomer shown in formula II are all distributed in the shell, the carboxyl group of the shell can improve the adhesion of the electrode. In addition, when the monomers represented by formula II and formula III are fed into the reaction vessel for the second stage polymerization, the monomer represented by formula I is continued to be fed into the reaction vessel to increase the compatibility of the core and shell parts and improve the stability of the core-shell structure polymer.
[0127] As used herein, the term "hydrophobicity" refers to the physical property of a molecule that repels water.
[0128] As used herein, the term "hydrophilicity" refers to the physical property of a molecule that allows it to form transient bonds with water via hydrogen bonds.
[0129] In some embodiments, the mass of the monomer of formula I introduced in the first stage polymerization is 70% to 85% of the total mass of the monomer of formula I supplied in the polymerization reaction, and the mass of the monomer of formula I introduced in the second stage polymerization reaction is 15% to 30% of the total mass of the monomer of formula I supplied in the polymerization reaction.
[0130] In some embodiments, the second stage polymerization comprises: adding an initiator into a reaction vessel, and then adding a premixed solution comprising a second emulsifier, at least one monomer represented by Formula II or a monomer represented by Formula III, and an aqueous medium.
[0131] In some embodiments, the initiator provided in the first stage polymerization and the initiator provided in the second stage polymerization are persulfates, the mass percentage of the initiator provided in the first stage polymerization is 0.05% to 0.075%, and the mass percentage of the initiator provided in the second stage polymerization is 0.05% to 0.075%, based on the total mass of the monomer represented by formula I, the monomer represented by formula II, and the monomer represented by formula III.
[0132] In some embodiments, the mass percentage of the first emulsifier is 0.28% to 0.42%, based on the total mass of the monomer represented by formula I, the monomer represented by formula II, and the monomer represented by formula III.
[0133] In some embodiments, the mass percentage of the second emulsifier is 0.8% to 1.2%, based on the total mass of the monomer represented by formula I, the monomer represented by formula II, and the monomer represented by formula III.
[0134] In some embodiments, the mass percentage of the aqueous medium provided in the first stage polymerization is 200% to 500%, and the mass percentage of the aqueous medium provided in the second stage polymerization is 100% to 200%, based on the total mass of the monomer represented by formula I, the monomer represented by formula II, and the monomer represented by formula III.
[0135] In some embodiments, the aqueous medium provided in the first stage polymerization and the aqueous medium provided in the second stage polymerization are deionized water.
[0136] In some embodiments, the reaction pressure of the first stage polymerization is 5.5 MPa to 7.5 MPa, and the reaction temperature is 75° C. to 85° C.
[0137] In some embodiments, the reaction pressure of the second polymerization is 4.5 MPa to 6.5 MPa, and the reaction temperature is 86° C. to 95° C.
[0138] In some embodiments, the initiator may be selected from one or more of potassium persulfate and ammonium persulfate.
[0139] Ammonium persulfate or potassium persulfate can be effectively decomposed above 60°C to generate free radical ions or ionic free radicals, and are suitable as initiators for emulsion polymerization.
[0140] In some embodiments, the first emulsifier is an alkali metal salt of perfluorooctanoic acid, optionally a sodium salt of perfluorooctanoic acid.
[0141] Alkali metal perfluorooctanoate is often used as an emulsifier or dispersant in the polymerization reaction of fluorinated monomers.
[0142] In some embodiments, the second emulsifier is one or both of polyoxyethylene-4-phenol ether ammonium sulfate and nonylphenol polyoxyethylene ether ammonium sulfate.
[0143] Polyoxyethylene-4-phenol ether ammonium sulfate and nonylphenol polyoxyethylene ether ammonium sulfate are both anionic-nonionic emulsifiers, which have both anionic and nonionic properties. They can be used alone in emulsion polymerization and do not need to be used in combination with other emulsifiers.
[0144] In one embodiment of the present application, an emulsion-type adhesive is provided, wherein the emulsion-type adhesive comprises the core-shell structure polymer according to any embodiment.
[0145] The emulsion-type binder is a direct product of the preparation method of the core-shell structure polymer in any embodiment, and can be directly used as a binder for water-based primer slurry, thereby reducing production costs and improving production efficiency.
[0146] In one embodiment of the present application, a use of a core-shell structured polymer in any embodiment in a secondary battery is provided. Optionally, the secondary battery includes at least one of a lithium ion battery, a sodium ion battery, a magnesium ion battery, and a potassium ion battery.
[0147] In some embodiments, the core-shell structured polymer is used as a binder in a secondary battery.
[0148] In some embodiments, the core-shell structured polymer is used as a binder for a water-based primer layer in a secondary battery.
[0149] [Water-based primer]
[0150] In one embodiment of the present application, a water-based primer slurry is provided, comprising a binder, a conductive agent, and an aqueous medium, wherein the binder comprises the core-shell structure polymer described in any embodiment.
[0151] As used herein, the term "binder" refers to a chemical compound, polymer, or mixture that forms a colloidal solution or colloidal dispersion in a dispersion medium.
[0152] In some embodiments, the dispersion medium of the binder is an aqueous medium, such as deionized water, that is, the binder is dissolved in the aqueous medium.
[0153] Compared with non-core-shell structure polymers, core-shell structure polymers have improved stability and dispersibility, improved the filterability of water-based primer slurry, improved the dispersibility of water-based primer slurry, and reduced the diaphragm resistance of the electrode.
[0154] In some embodiments, the core-shell structure polymer is added to the aqueous base coating slurry in the form of an emulsion containing the core-shell structure polymer.
[0155] The core-shell structure polymer prepared by the preparation method in any of the above embodiments exists in the form of an emulsion and can be directly added to the primer slurry for use, thereby reducing production costs and improving production efficiency.
[0156] In some embodiments, the conductive agent may include at least one of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers.
[0157] In some embodiments, the aqueous medium is deionized water.
[0158] In some embodiments, the mass ratio of the conductive agent to the binder is 0.8:1 to 1:1.
[0159] By controlling the mass ratio of the conductive agent to the binder within an appropriate range, the bonding strength of the slurry electrode and the diaphragm resistance can be taken into account, and the bonding performance and dynamic performance of the electrode can be comprehensively improved.
[0160] In some embodiments, when the solid content of the aqueous primer slurry is 10% to 20%, the viscosity of the aqueous primer slurry is 300 mPa·s to 900 mPa·s.
[0161] In some embodiments, the solid content of the aqueous base coating slurry may be any one of 10%, 15%, 18%, and 20%.
[0162] In some embodiments, the viscosity of the aqueous primer slurry can be selected from any one of 350mPa·s to 900mPa·s, 350mPa·s to 800mPa·s, 380mPa·s to 800mPa·s, 400mPa·s to 800mPa·s, 350mPa·s to 700mPa·s, and 400mPa·s to 700mPa·s.
[0163] Controlling the solid content of the water-based primer slurry within an appropriate range ensures good adhesion to the electrode, while also ensuring the slurry has an appropriate viscosity, taking into account subsequent coating processing and coating drying, and comprehensively improving the processing performance and performance of the slurry.
[0164] The viscosity of the aqueous primer slurry with a solid content of 10% to 20% is 300mPa·s to 900mPa·s, which means that the aqueous primer slurry prepared with the core-shell structure binder does not need to add additional dispersants or thickeners to improve processing performance, which helps to improve production efficiency and optimize the production process.
[0165] [Water-based base coat]
[0166] In one embodiment of the present application, a method for preparing a water-based primer is provided, comprising the following steps:
[0167] Using a gravure coater, coating the primer slurry described in the fourth aspect on the surface of the current collector;
[0168] After drying, a water-based primer layer is obtained, and the thickness of the water-based primer layer is 1 μm to 3 μm.
[0169] The preparation method of the water-based primer layer disclosed in the present application can improve the bonding force of the electrode sheet and reduce the membrane resistance of the electrode sheet.
[0170] In one embodiment of the present application, a secondary battery is provided, comprising a positive electrode sheet, a separator, a negative electrode sheet and an electrolyte, wherein the positive electrode sheet and / or the negative electrode sheet comprise the aqueous primer layer described in any embodiment. In some embodiments, the secondary battery comprises at least one of a lithium ion battery, a sodium ion battery, a magnesium ion battery, and a potassium ion battery. During the charge and discharge process of the battery, active ions are embedded and extracted back and forth between the positive electrode sheet and the negative electrode sheet. The electrolyte plays the role of conducting ions between the positive electrode sheet and the negative electrode sheet. The separator is arranged between the positive electrode sheet and the negative electrode sheet, mainly to prevent the positive and negative electrodes from short-circuiting, while allowing ions to pass through.
[0171] [Positive electrode]
[0172] The positive electrode sheet includes a positive electrode current collector, a positive electrode film layer and a water-based primer layer arranged on at least one surface of the positive electrode current collector.
[0173] As an example, the positive electrode current collector has two surfaces facing each other in its thickness direction, and the positive electrode film layer and the aqueous primer layer are disposed on either or both of the two facing surfaces of the positive electrode current collector.
[0174] In some embodiments, the positive electrode current collector may be a metal foil or a composite current collector. For example, aluminum foil may be used as the metal foil. The composite current collector may include a polymer material base and a metal layer formed on at least one surface of the polymer material base. The composite current collector may be formed by forming a metal material (aluminum, aluminum alloy, nickel, nickel alloy, titanium, titanium alloy, silver and silver alloy, etc.) on a polymer material substrate (such as a substrate of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), polyethylene (PE), etc.).
[0175] In some embodiments, the positive electrode active material may adopt the positive electrode active material for batteries that is well known in the art. As an example, the positive electrode active material may include at least one of the following materials: lithium-containing phosphates with an olivine structure, lithium transition metal oxides, and their respective modified compounds. However, the present application is not limited to these materials, and other traditional materials that can be used as positive electrode active materials for batteries may also be used. These positive electrode active materials may be used alone or in combination of two or more. Examples of lithium transition metal oxides may include, but are not limited to, lithium cobalt oxide (such as LiCoO2), lithium nickel oxide (such as LiNiO2), lithium manganese oxide (such as LiMnO2, LiMn2O4), lithium nickel cobalt oxide, lithium manganese cobalt oxide, lithium nickel manganese oxide, lithium nickel cobalt manganese oxide (such as LiNi 1 / 3 Co 1 / 3 Mn 1 / 3 O2 (also referred to as NCM 333 ), LiNi 0.5 Co 0.2 Mn 0.3 O2 (also referred to as NCM 523 ), LiNi 0.5 Co 0.25 Mn 0.25 O2 (also referred to as NCM 211 ), LiNi 0.6 Co 0.2 Mn 0.2 O2 (also referred to as NCM 622 ), LiNi 0.8 Co 0.1 Mn 0.1 O2 (also referred to as NCM 811 ), lithium nickel cobalt aluminum oxide (such as LiNi 0.85 Co 0.15 Al 0.05 O2) and its modified compounds. Examples of olivine-structured lithium-containing phosphates may include, but are not limited to, at least one of lithium iron phosphate (such as LiFePO4 (also referred to as LFP)), a composite material of lithium iron phosphate and carbon, lithium manganese phosphate (such as LiMnPO4), a composite material of lithium manganese phosphate and carbon, lithium iron manganese phosphate, and a composite material of lithium iron manganese phosphate and carbon.
[0176] In some embodiments, the positive electrode film layer may further optionally include a binder. As an example, the binder may include at least one of polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), a vinylidene fluoride-tetrafluoroethylene-propylene terpolymer, a vinylidene fluoride-hexafluoropropylene-tetrafluoroethylene terpolymer, a tetrafluoroethylene-hexafluoropropylene copolymer, and a fluorine-containing acrylate resin.
[0177] In some embodiments, the positive electrode film layer may further include a conductive agent. For example, the conductive agent may include at least one of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers.
[0178] In some embodiments, the positive electrode plate can be prepared by the following method: the components for preparing the water-based primer layer in any embodiment, such as the emulsion of the core-shell structure polymer and the conductive agent, are dispersed in a solvent (such as deionized water) to form a water-based primer slurry, and then the water-based primer slurry is coated on the aluminum foil current collector using a gravure coater, and dried to form a water-based primer layer, i.e., a water-based primer current collector; the components for preparing the positive electrode film layer, such as the positive electrode active material, the conductive agent, the binder and any other components are dispersed in a solvent (such as N-methylpyrrolidone) to form a positive electrode slurry; the positive electrode slurry is coated on the water-based primer current collector, and after drying, cold pressing and other processes, the positive electrode plate can be obtained.
[0179] [Negative electrode]
[0180] The negative electrode plate includes a negative electrode current collector and a negative electrode film layer arranged on at least one surface of the negative electrode current collector.
[0181] As an example, the negative electrode current collector has two surfaces opposite to each other in its thickness direction, and the negative electrode film layer is disposed on either or both of the two opposite surfaces of the negative electrode current collector.
[0182] In some embodiments, the negative electrode current collector may be a metal foil or a composite current collector. For example, copper foil may be used as the metal foil. The composite current collector may include a polymer base layer and a metal layer formed on at least one surface of the polymer base material. The composite current collector may be formed by forming a metal material (copper, copper alloy, nickel, nickel alloy, titanium, titanium alloy, silver, and silver alloy, etc.) on a polymer base material (such as a base material of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), polyethylene (PE), etc.).
[0183] In some embodiments, the negative electrode active material may be a negative electrode active material for a battery that is well known in the art. As an example, the negative electrode active material may include at least one of the following materials: artificial graphite, natural graphite, soft carbon, hard carbon, silicon-based materials, tin-based materials, lithium titanate, etc. The silicon-based material may be selected from at least one of elemental silicon, silicon oxides, silicon-carbon composites, silicon-nitrogen composites, and silicon alloys. The tin-based material may be selected from at least one of elemental tin, tin oxides, and tin alloys. However, the present application is not limited to these materials, and other traditional materials that can be used as negative electrode active materials for batteries may also be used. These negative electrode active materials may be used alone or in combination of two or more.
[0184] In some embodiments, the negative electrode film layer may further include a binder. The binder may be selected from at least one of styrene-butadiene rubber (SBR), polyacrylic acid (PAA), sodium polyacrylate (PAAS), polyacrylamide (PAM), polyvinyl alcohol (PVA), sodium alginate (SA), polymethacrylic acid (PMAA), and carboxymethyl chitosan (CMCS).
[0185] In some embodiments, the negative electrode film layer may further include a conductive agent, which may be selected from at least one of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers.
[0186] In some embodiments, the negative electrode film layer may optionally include other additives, such as a thickener (eg, sodium carboxymethyl cellulose (CMC-Na)).
[0187] In some embodiments, the negative electrode sheet can be prepared by the following method: the components for preparing the negative electrode sheet, such as the negative electrode active material, the conductive agent, the binder and any other components, are dispersed in a solvent (such as deionized water) to form a negative electrode slurry; the negative electrode slurry is coated on the negative electrode current collector, and after drying, cold pressing and other processes, the negative electrode sheet can be obtained.
[0188] [Electrolytes]
[0189] The electrolyte conducts ions between the positive and negative electrodes. This application does not specify the type of electrolyte, and the electrolyte can be selected based on the needs. For example, the electrolyte can be liquid, gel, or solid.
[0190] In some embodiments, the electrolyte is an electrolyte solution comprising an electrolyte salt and a solvent.
[0191] In some embodiments, the electrolyte salt may be selected from at least one of lithium hexafluorophosphate, lithium tetrafluoroborate, lithium perchlorate, lithium hexafluoroarsenate, lithium bis(fluorosulfonyl)imide, lithium bis(trifluoromethanesulfonyl)imide, lithium trifluoromethanesulfonate, lithium difluorophosphate, lithium difluorooxalatoborate, lithium dioxalatoborate, lithium difluorodioxalatophosphate, and lithium tetrafluorooxalatophosphate.
[0192] In some embodiments, the solvent can be selected from at least one of ethylene carbonate, propylene carbonate, ethyl methyl carbonate, diethyl carbonate, dimethyl carbonate, dipropyl carbonate, methylpropyl carbonate, ethylpropyl carbonate, butylene carbonate, fluoroethylene carbonate, methyl formate, methyl acetate, ethyl acetate, propyl acetate, methyl propionate, ethyl propionate, propyl propionate, methyl butyrate, ethyl butyrate, 1,4-butyrolactone, cyclopentane, dimethyl sulfone, methyl ethyl sulfone and diethyl sulfone.
[0193] In some embodiments, the electrolyte may further include additives. For example, the additives may include negative electrode film-forming additives, positive electrode film-forming additives, and additives that can improve certain battery properties, such as additives that improve battery overcharge performance, and additives that improve battery high or low temperature performance.
[0194] [Isolation film]
[0195] In some embodiments, the secondary battery further includes a separator. The present application has no particular limitation on the type of separator, and any known porous separator with good chemical and mechanical stability can be selected.
[0196] In some embodiments, the material of the separator can be selected from at least one of glass fiber, non-woven fabric, polyethylene, polypropylene, and polyvinylidene fluoride. The separator can be a single-layer film or a multi-layer composite film, without particular limitation. When the separator is a multi-layer composite film, the materials of each layer can be the same or different, without particular limitation.
[0197] In some embodiments, the positive electrode sheet, the negative electrode sheet, and the separator can be formed into an electrode assembly through a winding process or a lamination process.
[0198] In some embodiments, the secondary battery may include an outer packaging that can be used to encapsulate the electrode assembly and the electrolyte.
[0199] In some embodiments, the outer packaging of the secondary battery can be a hard shell, such as a hard plastic shell, an aluminum shell, or a steel shell. Alternatively, the outer packaging of the secondary battery can be a soft shell, such as a pouch-type soft shell. The soft shell can be made of plastic, such as polypropylene, polybutylene terephthalate, and polybutylene succinate.
[0200] The present application has no particular limitation on the shape of the secondary battery, which may be cylindrical, square, or any other shape. For example, FIG2 shows a secondary battery 5 having a square structure as an example.
[0201] In some embodiments, referring to Figure 3, the outer packaging may include a shell 51 and a cover plate 53. The shell 51 may include a bottom plate and a side plate connected to the bottom plate, and the bottom plate and the side plate enclose a receiving cavity. The shell 51 has an opening connected to the receiving cavity, and the cover plate 53 can be covered on the opening to close the receiving cavity. The positive electrode sheet, the negative electrode sheet and the isolation membrane can be formed into an electrode assembly 52 through a winding process or a lamination process. The electrode assembly 52 is encapsulated in the receiving cavity. The electrolyte is infiltrated in the electrode assembly 52. The number of electrode assemblies 52 contained in the secondary battery 5 can be one or more, and those skilled in the art can select according to specific actual needs.
[0202] In some embodiments, secondary batteries can be assembled into a battery module. The number of secondary batteries contained in the battery module can be one or more. The specific number can be selected by those skilled in the art according to the application and capacity of the battery module.
[0203] Figure 4 shows an example battery module 4. Referring to Figure 4 , within the battery module 4, multiple secondary batteries 5 may be arranged sequentially along the length of the battery module 4. Of course, any other arrangement is also possible. Furthermore, the multiple secondary batteries 5 may be secured together using fasteners.
[0204] Optionally, the battery module 4 may further include a housing having a receiving space, and the plurality of secondary batteries 5 are received in the receiving space.
[0205] In some embodiments, the battery modules described above may also be assembled into a battery pack. The battery pack may contain one or more battery modules, and the specific number may be selected by those skilled in the art based on the application and capacity of the battery pack.
[0206] Figures 5 and 6 illustrate an example battery pack 1. Referring to Figures 5 and 6 , the battery pack 1 may include a battery box and multiple battery modules 4 disposed within the battery box. The battery box comprises an upper case 2 and a lower case 3. The upper case 2 can be positioned over the lower case 3 to form an enclosed space for accommodating the battery modules 4. The multiple battery modules 4 can be arranged in any manner within the battery box.
[0207] In addition, the present application also provides an electric device, which includes at least one of the secondary battery, battery module, or battery pack provided in the present application. The secondary battery, battery module, or battery pack can be used as a power source for the electric device, and can also be used as an energy storage unit for the electric device. The electric device may include mobile devices (such as mobile phones, laptops, etc.), electric vehicles (such as pure electric vehicles, hybrid electric vehicles, plug-in hybrid electric vehicles, electric bicycles, electric scooters, electric golf carts, electric trucks, etc.), electric trains, ships and satellites, energy storage systems, etc., but is not limited thereto.
[0208] As the electrical device, a secondary battery, a battery module or a battery pack can be selected according to its usage requirements.
[0209] Figure 7 shows an example of an electric device. This device is a pure electric vehicle, a hybrid electric vehicle, or a plug-in hybrid electric vehicle. To meet the high power and high energy density requirements of the secondary battery, a battery pack or battery module can be used.
[0210] Another example device may be a mobile phone, a tablet computer, a notebook computer, etc. Such a device is generally required to be lightweight and thin, and may use a secondary battery as a power source.
[0211] Example
[0212] Below, the embodiment of the present application is described. The embodiment described below is exemplary and is only used to explain the present application, and is not to be construed as limiting the present application. Where specific techniques or conditions are not specified in the embodiments, the techniques or conditions described in the literature in this area or the product specifications are used. Reagents or instruments used that do not specify the manufacturer are conventional products that can be obtained commercially.
[0213] 1. Preparation method
[0214] Example 1
[0215] 1) Preparation of core-shell polymers
[0216] First stage polymerization: 21 kg of deionized water, 21 g of sodium perfluorooctanoate, and 71.4 g of 5% potassium persulfate solution, where the conductivity of the deionized water is less than or equal to 2 μs / cm, are added sequentially into the reactor, and the reactor is closed;
[0217] The reactor was vacuumed and filled with nitrogen, and the operation was repeated until the oxygen concentration in the reactor was less than 100 ppm;
[0218] Add vinylidene fluoride monomer into the reactor until the pressure inside the reactor reaches 7.0 MPa; raise the temperature inside the reactor to 80°C to start the reaction, and continuously add vinylidene fluoride monomer during the reaction to maintain the reaction pressure inside the reactor constant;
[0219] Second stage polymerization: Add the remaining 9 kg of deionized water (the conductivity of the deionized water is less than or equal to 2 μs / cm), 60 g of polyoxyethylene-4-phenol ether ammonium sulfate, 1.5 kg of styrene monomer, and 1.5 kg of acrylic acid monomer into a stirring tank and stir uniformly to obtain a premixed solution;
[0220] When the total amount of vinylidene fluoride monomer added was 2.4 kg, the remaining 30.6 g of 5% concentration potassium persulfate solution and 48.0 g of 5% concentration ammonium persulfate were added, the reaction pressure was adjusted to 5.5 MPa, the temperature was raised to 90 ° C, and the premixed solution was slowly added to the reactor. The entire addition time of the premixed solution was 1.5 hours. At the same time, the remaining 0.6 kg of vinylidene fluoride monomer was gradually introduced;
[0221] The reaction was stopped when the pressure in the autoclave dropped to 0.2 MPa;
[0222] The mixture was cooled to room temperature and the material was filtered to obtain an emulsion of a core-shell structured vinylidene fluoride-acrylic acid-styrene copolymer with a Dv50 particle size of 400 nm.
[0223] 2) Preparation of water-based primer slurry
[0224] The solid content of the core-shell structured vinylidene fluoride-acrylic acid-styrene copolymer emulsion was adjusted to 25%;
[0225] Weigh 2.25 kg of conductive carbon black powder and 9 kg of core-shell structure vinylidene fluoride-acrylic acid-styrene copolymer emulsion and add them into the stirring tank in sequence;
[0226] Set the stirring speed to 300 rpm and the stirring time to 10 minutes;
[0227] Set the stirring speed to 2000 rpm and the stirring time to 120 minutes;
[0228] Weigh 25.5 kg of deionized water and add it to the stirring tank. Set the stirring speed to 2000 rpm and the stirring time to 120 minutes.
[0229] The slurry was filtered through a 300-mesh filter to obtain a water-based primer slurry.
[0230] 3) Preparation of water-based base coating
[0231] The water-based primer slurry was coated on the surface of the aluminum foil current collector substrate using a gravure coater and dried to obtain a water-based primer coating with a thickness of 2 μm, thereby obtaining a water-based primer current collector.
[0232] 4) Preparation of electrode
[0233] The components used to make the positive electrode film layer, lithium nickel cobalt manganese (NCM) material, conductive agent carbon black, polyvinylidene fluoride binder, and N-methylpyrrolidone (NMP) are stirred and mixed evenly in a weight ratio of 96.9:2.1:1:21 to obtain a positive electrode slurry with a solid content of 73%; the positive electrode slurry is then evenly coated on the water-based primer current collector, and then dried, cold pressed, and cut to obtain the positive electrode sheet.
[0234] 5) Preparation of negative electrode sheet
[0235] The active material artificial graphite, the conductive agent carbon black, the binder styrene-butadiene rubber (SBR), and the thickener sodium carboxymethyl cellulose (CMC) are dissolved in the solvent deionized water in a weight ratio of 96.2:0.8:0.8:1.2, and mixed evenly to prepare a negative electrode slurry; the negative electrode slurry is evenly coated on the negative electrode current collector copper foil once or multiple times, and the negative electrode sheet is obtained after drying, cold pressing, and slitting.
[0236] 6) Isolation film
[0237] Polypropylene film is used as the isolation film.
[0238] 7) Preparation of electrolyte
[0239] In an argon atmosphere glove box (H2O<0.1ppm, O2<0.1ppm), the organic solvent ethylene carbonate (EC) / ethyl methyl carbonate (EMC) was mixed uniformly in a volume ratio of 3 / 7, 12.5% LiPF6 lithium salt was added and dissolved in the organic solvent, and stirred uniformly to obtain the electrolyte of Example 1.
[0240] 8) Preparation of batteries
[0241] The positive electrode sheet, separator, and negative electrode sheet are stacked in order, with the separator positioned between the positive and negative electrode sheets to provide isolation. The cells are then wound to obtain a bare cell. The tabs are welded to the bare cell and placed in an aluminum shell. The cells are then baked at 80°C to remove moisture. The electrolyte is then injected and sealed to obtain an uncharged battery. The uncharged battery then undergoes a series of steps, including resting, hot and cold pressing, formation, shaping, and capacity testing, to obtain the lithium-ion battery product of Example 1.
[0242] Example 2 to Example 9
[0243] The preparation method is basically the same as that of Example 1, except that the mass content of the core and shell parts and the ratio of each monomer in the synthesis of the core-shell structure polymer are adjusted. Specific parameters are shown in Tables 1 and 2.
[0244] Example 10 to Example 13
[0245] The preparation method is basically the same as that in Example 1, except that the initiator mass and reaction temperature in the synthesis of the core-shell structure polymer are adjusted so that the core-shell structure polymer has different weight average molecular weights. Specific parameters are shown in Tables 1 and 2.
[0246] Example 10
[0247] The preparation method is basically the same as that of Example 1, except that the 5% concentration of potassium persulfate solution in the first stage polymerization is adjusted to 85.32 g. For specific parameters, see Tables 1 and 2.
[0248] Example 11
[0249] The preparation method is basically the same as that of Example 1, except that the 5% concentration of potassium persulfate solution in the first stage polymerization is adjusted to 78.54 g. For specific parameters, see Tables 1 and 2.
[0250] Example 12
[0251] The preparation method is basically the same as that of Example 1, except that the 5% concentration of potassium persulfate solution in the first stage polymerization is adjusted to 64.26 g, and the reaction temperature in the first stage polymerization is adjusted to 75° C. For specific parameters, see Tables 1 and 2.
[0252] Example 13
[0253] The preparation method is basically the same as that of Example 1, except that the 5% concentration of potassium persulfate solution in the first stage polymerization is adjusted to 60 g, and the reaction temperature in the first stage polymerization is adjusted to 75° C. For specific parameters, see Tables 1 and 2.
[0254] Example 14 to Example 17
[0255] The preparation method is basically the same as that of Example 1, except that the mass ratio of the conductive agent to the binder in the aqueous primer slurry is adjusted. Specific parameters are shown in Tables 1 and 2.
[0256] Example 18 to Example 21
[0257] The preparation method is basically the same as that of Example 1, except that the solid content of the water-based primer slurry is adjusted. The specific parameters are shown in Tables 1 and 2.
[0258] Example 22 to Example 23
[0259] The preparation method is basically the same as that of Example 1, except that the thickness of the water-based primer layer is adjusted. Specific parameters are shown in Tables 1 and 2.
[0260] Example 24
[0261] The preparation method is basically the same as that of Example 1, except that the acrylic acid monomer is replaced by a methacrylic acid monomer. For specific parameters, see Tables 1 and 2.
[0262] Example 25
[0263] The method is basically the same as Example 1, except that the preparation method of the water-based primer layer is adjusted. The specific preparation method is as follows:
[0264] The aqueous primer slurry was coated on the surface of the aluminum foil current collector substrate using a doctor blade technique, and after drying, a 2 μm thick aqueous primer layer was formed to obtain an aqueous primer current collector. Specific parameters are shown in Tables 1 and 2.
[0265] Examples 26-27
[0266] Examples 26 to 27 are basically the same as Example 1, except that the thickness of the water-based primer layer is adjusted. For specific parameters, see Tables 1 and 2.
[0267] Comparative Example 1
[0268] The preparation method is basically the same as that of Example 1, except that the binder in the conductive paste is polyvinylidene fluoride with a weight average molecular weight of 400,000.
[0269] Comparative Example 2
[0270] The preparation method is basically the same as that of Example 1, except that the 1.5 kg of styrene monomer and 1.5 kg of acrylic acid monomer in the second stage polymerization are adjusted to 3 kg of styrene monomer.
[0271] Comparative Example 3
[0272] The preparation method is basically the same as that of Example 1, except that the 1.5 kg of styrene monomer and 1.5 kg of acrylic acid monomer in the second stage polymerization are adjusted to 3 kg of acrylic acid monomer.
[0273] Comparative Example 4
[0274] The preparation method is basically the same as that of Example 1, except that the 5-core-shell structure vinylidene fluoride-acrylic acid-styrene copolymer emulsion is used to replace the vinylidene fluoride-acrylic acid-styrene copolymer emulsion prepared by the traditional method. The synthesis method is:
[0275] 30 kg of deionized water (conductivity less than or equal to 2 μs / cm), 21 g of sodium perfluorooctanoate, and 150 g of 5% potassium persulfate solution were added to the reactor in sequence, and the reactor was closed.
[0276] The reactor was vacuumed and filled with nitrogen, and the operation was repeated until the oxygen concentration in the reactor was less than 100 ppm;
[0277] Add vinylidene fluoride monomer, 1.5 kg of styrene monomer, and 1.5 kg of acrylic acid monomer into the reactor until the pressure in the reactor reaches 7.5 MPa;
[0278] The temperature in the kettle was raised to 85°C to start the reaction. During the reaction, vinylidene fluoride monomer was continuously introduced to maintain the reaction pressure in the kettle constant. The total mass of the introduced vinylidene fluoride monomer was 3 kg.
[0279] When the reaction is completed, the pressure in the autoclave will reach 0.2 MPa, and the unreacted vinylidene fluoride monomer is recovered; the mixture is cooled to room temperature, and the material is filtered to obtain an emulsion, namely, a vinylidene fluoride-acrylic acid-styrene copolymer emulsion.
[0280] 2. Test Method
[0281] 1. Weight average molecular weight of core-shell polymer
[0282] The core-shell polymer emulsion was vacuum dried at 120° C. for 180 minutes to obtain a core-shell polymer powder;
[0283] A Waters 2695 Isocratic HPLC gel chromatography instrument (differential refractive index detector 2141) was used. A 3.0% polystyrene solution sample was used as a reference, and a matching chromatographic column was selected (oil-based: Styragel HT5DMF7.8×300mm+Styragel HT4). A 3.0% core-shell polymer solution was prepared using purified N-methylpyrrolidone (NMP) solvent. The prepared solution was allowed to stand for one day before use. During the test, tetrahydrofuran was first drawn into a syringe and rinsed several times. Then 5 ml of the experimental solution was drawn, the air in the syringe was expelled, and the needle tip was wiped dry. Finally, the sample solution was slowly injected into the injection port. After the reading stabilized, the data was acquired and the weight-average molecular weight was read.
[0284] 2. Dv50 particle size test of core-shell polymers
[0285] Refer to the particle size distribution laser diffraction method in GB / T 19077-2016. Weigh 0.1g–0.13g of the core-shell polymer emulsion into a 50ml beaker. Then, weigh 5g of deionized water and add it to the beaker containing the core-shell polymer emulsion. Place a stirring bar approximately 2.5mm in length, and seal with plastic wrap. Ultrasonicate the sample for 5 minutes, then transfer it to a magnetic stirrer and stir at 500 rpm for at least 20 minutes. Two samples from each batch are tested. Determination is performed using a laser particle size analyzer, such as the Mastersizer 2000E from Malvern Instruments Ltd., UK.
[0286] 3. Viscosity test of water-based primer slurry
[0287] Use a rotary viscometer to measure the viscosity of water-based primer slurry. Select a suitable rotor, secure the viscometer rotor, and place the water-based primer slurry under the viscometer rotor, so that the slurry just covers the rotor scale line. Instrument model: Shanghai Fangrui NDJ-5S, rotor #62, speed of 30 rpm, measurable slurry viscosity range of 0-1000 mPa·s; rotor #63, speed of 30 rpm, measurable slurry viscosity range of 0-2000 mPa·s. Test temperature: 25°C, test time: 5 minutes, wait for the display to stabilize and read the data.
[0288] 4. Filtration performance test of water-based primer slurry
[0289] Take a 500ml beaker and place it at the lower end of a 200-mesh filter stand, take 500ml of water-based primer slurry, place it in the filter and filter, record the time when the slurry volume in the beaker reaches 300ml, this time is used to judge the filtration performance of the slurry. If the filtration time is less than 10s, it indicates that the filtration performance of the slurry is good, which is judged as "YES" and recorded as "Y"; if the slurry transition time is greater than 10s or cannot pass through the filter, it indicates that the filtration performance of the slurry is poor, which is judged as "NG" and recorded as "N".
[0290] 5. The difference in solid content of water-based primer after standing for 24 hours
[0291] Take a small piece of electrode and weigh it in the weight loss rate measuring instrument, record it as M0, and reset it to zero;
[0292] Take the upper layer of water-based primer slurry, apply a small amount on the electrode, and then put it into the weight loss rate meter to weigh it, which is recorded as M1;
[0293] Close the device and start drying;
[0294] After the end, record the weighing data, record it as M2, and calculate the solid content, the solid content is (M2-M0) / (M1-M0);
[0295] The solid content of the lower aqueous primer slurry was measured in the same manner, and the difference in solid content after the aqueous primer slurry was allowed to stand for 24 hours was calculated as the solid content of the lower aqueous primer slurry minus the solid content of the upper aqueous primer slurry.
[0296] 6. Adhesion of the electrode
[0297] With reference to GB-T2790-1995 national standard "Test method for 180° peel strength of adhesive", the adhesion test process of the embodiments and comparative examples of the present application is as follows: Use a blade to cut a sample with a width of 30mm and a length of 100-160mm, and stick a special double-sided tape on the steel plate. The tape is 20mm wide and 90-150mm long. Stick the positive electrode film layer of the electrode sample cut earlier on the double-sided tape, and then roll it three times in the same direction with a 2kg roller. Fix a paper tape with a width equal to the electrode and a length of 250mm on the electrode collector and fix it with wrinkle glue. Turn on the power of the Sansi tensile testing machine (sensitivity is 1N), the indicator light is on, adjust the limit block to the appropriate position, and fix the end of the steel plate without the electrode with the lower clamp. Fold the paper tape upwards, fix it with the upper clamp, and use the "up" and "down" buttons on the manual controller attached to the tensile testing machine to adjust the position of the upper clamp. The test is then performed and the value is read at a stretching speed of 50 mm / min. The force at which the electrode is under force equilibrium is divided by the width of the tape as the bonding force per unit length of the electrode, which represents the bonding strength between the material layer on the current collector and the current collector.
[0298] 7. Diaphragm resistance of the electrode
[0299] Cut the dried positive electrode sheet at the left, center, and right sides into small discs with a diameter of 10mm. Turn on the Yuanneng Technology electrode resistance meter, place it in the appropriate position on the "probe" of the electrode resistance meter, click the "Start" button, and wait for the reading to stabilize before reading. Test two positions on each small disc, and calculate the average of the six measurements to obtain the film resistance of the electrode sheet.
[0300] 8. Battery DC impedance
[0301] The battery DC impedance test procedure is as follows: At 25°C, the battery corresponding to Example 1 was charged at a constant current of 1 / 3*C to 4.3V, then charged at a constant voltage of 4.3V to a current of 0.05C. After 5 minutes, the voltage V1 was recorded. The battery was then discharged at 1 / 3C for 30 seconds, and the voltage V2 was recorded. The battery internal resistance (DCR) was calculated as 3*(V2-V1) / C.
[0302] 9. Thickness of water-based basecoat
[0303] Take a piece of aluminum foil and place it on a flat table. The aluminum foil should extend about 5 cm beyond the table. Press the aluminum foil on the table to prevent it from moving.
[0304] Open the micrometer and reset it to zero;
[0305] Select 5 points at different positions of the aluminum foil to measure the thickness of the aluminum foil in turn, and take the average value as L1;
[0306] Apply water-based primer slurry on one side of the aluminum foil using a gravure coater and dry it. Place the dried aluminum foil on a flat table with about 5 cm of aluminum foil extending beyond the table. Press the aluminum foil on the table to prevent it from moving.
[0307] Open the micrometer and reset it to zero;
[0308] Select 5 points at different positions of the aluminum foil to measure the thickness of the aluminum foil in turn, and take the average value as L2;
[0309] The thickness of the water-based base coating is (L2-L1).
[0310] 3. Analysis of test results of various embodiments and comparative examples
[0311] The aqueous primer slurry, aqueous primer coating and positive electrode sheet of each embodiment and comparative example were prepared according to the above method, and various parameters were measured. The results are shown in Tables 1 and 2 below.
[0312] Table 1 Preparation parameters and results of examples and comparative examples
[0313]
[0314]
[0315] Table 2 Preparation parameters and results of examples and comparative examples
[0316]
[0317]
[0318] According to the results in Table 1 and Table 2, the binders in the aqueous primer slurries in Examples 1 to 27 are all core-shell structure polymers, comprising a core portion and a shell portion that at least partially covers the core portion, the core portion comprising a structural unit derived from vinylidene fluoride, and the shell portion comprising a structural unit derived from vinylidene fluoride, a structural unit derived from acrylic acid or methacrylic acid, and a structural unit derived from styrene. Good results were achieved using the above-mentioned core-shell structure vinylidene fluoride-acrylic acid-styrene copolymer or core-shell structure vinylidene fluoride-methacrylic acid-styrene copolymer as a binder. Compared with the traditional polyvinylidene fluoride binder in Comparative Example 1, the core-shell structure vinylidene fluoride-acrylic acid-styrene copolymer or core-shell structure vinylidene fluoride-methacrylic acid-styrene copolymer binder provided in the present application can reduce the viscosity of the aqueous primer slurry, improve the filterability of the aqueous primer slurry, and improve the processing performance of the aqueous primer slurry.
[0319] From the vinylidene fluoride-styrene copolymer and the vinylidene fluoride-acrylic acid copolymer in Example 1, Comparative Examples 2 and 3, the core-shell structure vinylidene fluoride-acrylic acid-styrene copolymer disclosed in the present application can take into account the anti-settling property of the slurry and the adhesion of the electrode, and comprehensively improve the storage performance and usage performance of the water-based primer slurry.
[0320] From the comparison between Example 1 and Comparative Example 4, it can be seen that the core-shell structure polymer disclosed in the present application can reduce the viscosity of the slurry, improve the filterability of the slurry, improve the adhesion of the electrode and reduce the diaphragm resistance of the electrode, compared with the non-core-shell structure polymer prepared by the traditional preparation method, thereby comprehensively improving the processing performance and use performance of the water-based primer slurry.
[0321] From the comparison between Examples 1 to 3 and Examples 4 to 5, it can be seen that the mass content of the core portion is 40% to 50%. Based on the total mass of the core-shell structure polymer, the core-shell structure polymer can take into account the viscosity of the slurry and the adhesion of the electrode, and comprehensively improve the processing performance and usage performance of the water-based primer slurry.
[0322] From the comparison of Example 1, Examples 6 to 7 and Examples 8 to 9, it can be seen that the mass content of the structural unit derived from acrylic acid in the core-shell structure polymer is 10% to 40%. Based on the mass of the core-shell structure polymer, the core-shell structure polymer can take into account the viscosity of the water-based primer slurry and the adhesion of the electrode, and comprehensively improve the processing performance and use performance of the water-based primer slurry.
[0323] From the comparison of Example 1, Examples 4-5 and Examples 6-7, it can be seen that the mass content of the structural units derived from styrene in the core-shell structure polymer is 10% to 40%. Based on the mass of the core-shell structure polymer, the core-shell structure polymerization can take into account the adhesion force and membrane resistance of the electrode, and comprehensively improve the adhesion performance and dynamic performance of the electrode.
[0324] From the comparison between Examples 1, 11-12 and 10, 13, it can be seen that when the weight average molecular weight of the core-shell structure polymer is 300,000 to 500,000, the core-shell structure polymerization can take into account both the bonding force of the electrode and the membrane resistance, and comprehensively improve the bonding performance and dynamic performance of the electrode.
[0325] The aqueous base coating slurries in Examples 1 to 27 all include a core-shell structure polymer, a conductive agent and water, wherein the core-shell structure polymer is added to the aqueous coating slurry in the form of an emulsion.
[0326] From the comparison between Example 1, Examples 15-16 and Example 14, Example 17, it can be seen that the mass ratio of the conductive agent to the core-shell structure binder in the water-based primer slurry is 0.8:1 to 1:1, which can take into account the bonding force and membrane resistance of the slurry electrode, and comprehensively improve the bonding performance and dynamic performance of the electrode.
[0327] From the comparison between Examples 1, 19-20 and 18, 21, it can be seen that the solid content of the water-based primer slurry is 10% to 20%. The water-based primer slurry takes into account both the shipping viscosity and the adhesion of the electrode, and comprehensively improves the processing performance and use performance of the slurry.
[0328] It can be seen from Examples 1 to 17, Examples 19 to 20, and Examples 22 to 24 that when the solid content of the aqueous primer slurry is 10% to 20%, the viscosity of the aqueous primer slurry is 300 mPa.s to 900 mPa.s, which means that the aqueous coating slurry prepared by the core-shell structure binder does not need to add additional dispersants or thickeners to improve processing performance, which helps to improve production efficiency and optimize the production process.
[0329] The preparation methods of the water-based base coatings in Examples 1 to 24 all include the following steps:
[0330] Using a gravure coater, the prepared primer slurry is coated on the surface of the current collector;
[0331] After drying, a water-based primer layer is obtained, and the thickness of the water-based primer layer is 1 μm to 3 μm.
[0332] From the comparison between Example 1 and Example 25, it can be seen that the water-based primer layer prepared by the preparation method disclosed in this application can improve the adhesion of the electrode and reduce the membrane resistance of the electrode.
[0333] From the comparison between Example 1, Examples 22-23 and Examples 26-27, it can be seen that the coating thickness of the water-based primer is 1um-3um, which can reduce the diaphragm resistance of the electrode. At the same time, the electrode has good adhesion and improves the dynamic performance of the battery.
[0334] It should be noted that the present application is not limited to the above-mentioned embodiments. The above-mentioned embodiments are merely examples, and any embodiments having substantially the same structure and effect as the technical concept within the scope of the present application are all included in the technical scope of the present application. In addition, without departing from the scope of the present application, any other embodiments that can be conceived by those skilled in the art and that combine some of the constituent elements in the embodiments are also included in the scope of the present application.
Claims
1. A core-shell structure polymer, characterized in that The invention comprises a core portion and a shell portion at least partially covering the core portion, wherein the core portion comprises a structural unit derived from a monomer represented by formula I, and the shell portion comprises a structural unit derived from a monomer represented by formula I, a structural unit derived from a monomer represented by formula II, and a structural unit derived from a monomer represented by formula III. wherein R1, R2, and R3 are each independently selected from hydrogen, fluorine, chlorine, or a C 1-3 Alkyl, R4, R5, R6, R7, R8, R9 are each independently selected from hydrogen, substituted or unsubstituted C 1-5 Ar is an alkyl group, and Ar is a substituted or unsubstituted aromatic group.
2. The core-shell structure polymer according to claim 1, characterized in that R1 is fluorine, R2 and R3 are each independently selected from hydrogen, fluorine, chlorine or trifluoromethyl, and R4, R5, R6, R7, R8 and R9 are each independently selected from hydrogen or methyl.
3. The core-shell structure polymer according to claim 1 or 2, characterized in that The mass content of the core portion is 40% to 50% based on the mass of the core-shell structure polymer.
4. The core-shell structure polymer according to any one of claims 1 to 3, characterized in that The mass content of the structural unit derived from the monomer represented by formula II is 10% to 40%, based on the mass of the core-shell structure polymer.
5. The core-shell structure polymer according to any one of claims 1 to 4, characterized in that The mass content of the structural unit derived from the monomer represented by formula III is 10% to 40%, based on the mass of the core-shell structure polymer.
6. The core-shell structure polymer according to any one of claims 1 to 5, characterized in that The weight average molecular weight of the core-shell structure polymer is 300,000 to 500,000.
7. The core-shell structure polymer according to any one of claims 1 to 6, characterized in that The monomer represented by formula I is selected from one or more of vinylidene fluoride, tetrafluoroethylene, chlorotrifluoroethylene, and hexafluoropropylene.
8. The core-shell structure polymer according to any one of claims 1 to 7, characterized in that The monomer represented by formula II is selected from one or both of acrylic acid and methacrylic acid.
9. The core-shell structure polymer according to any one of claims 1 to 8, characterized in that The monomer represented by formula III is selected from one or two of styrene and 4-methylstyrene.
10. The core-shell structure polymer according to any one of claims 1 to 9, characterized in that The Dv50 particle size of the core-shell structure polymer is 100 nm to 10 μm.
11. A method for preparing a core-shell structure polymer, characterized in that: The preparation method The following steps are included: The core portion of the core-shell structure polymer is prepared by polymerizing the monomer represented by formula I under polymerizable conditions, and the shell portion of the core-shell structure polymer is prepared by polymerizing the monomer represented by formula I, the monomer represented by formula II, and the monomer represented by formula III, wherein the shell portion at least partially covers the core portion. wherein R1, R2, and R3 are each independently selected from hydrogen, fluorine, chlorine, C 1-3 One or more of the alkyl groups, R4, R5, R6, R7, R8, R9 are each independently selected from hydrogen, substituted or unsubstituted C 1-5 One or more of the alkyl groups, Ar is a substituted or unsubstituted aromatic group.
12. The method for preparing a core-shell structure polymer according to claim 11, characterized in that: R1 is fluorine, R2 and R3 are each independently selected from one or more of hydrogen, fluorine, chlorine, and trifluoromethyl, and R4, R5, R6, R7, R8, and R9 are each independently selected from one or two of hydrogen and methyl.
13. The method for preparing a core-shell structure polymer according to claim 11 or 12, characterized in that: The mass content of the core portion is 40% to 50% based on the mass of the core-shell structure polymer.
14. The method for preparing a core-shell structure polymer according to any one of claims 11 to 13, characterized in that: The mass content of the monomer represented by formula II is 10% to 40%, based on the total mass of the monomer represented by formula I, the monomer represented by formula II and the monomer represented by formula III.
15. The method for preparing a core-shell structure polymer according to any one of claims 11 to 14, characterized in that: The mass content of the monomer represented by formula III is 10% to 40%, based on the total mass of the monomer represented by formula I, the monomer represented by formula II and the monomer represented by formula III.
16. The method for preparing a core-shell structure polymer according to any one of claims 11 to 15, characterized in that: The preparation method includes a first stage polymerization and a second stage polymerization, First stage polymerization: providing an initiator, a first emulsifier, at least one monomer represented by formula I and an aqueous medium to carry out a first stage polymerization reaction to obtain a core portion, and continuously feeding the monomer represented by formula I during the first stage polymerization reaction; Second stage polymerization: After a period of reaction, an initiator, a second emulsifier, at least one monomer represented by formula II and a monomer represented by formula III, and an aqueous medium are added to the reaction vessel to carry out a second stage polymerization reaction to obtain a core-shell structure polymer, and the monomer represented by formula I is continuously input during the second stage polymerization reaction.
17. The method for preparing a core-shell structure polymer according to claim 16, wherein: The second stage of polymerization includes: After adding the initiator into the reaction container, a premixed solution comprising a second emulsifier, at least one monomer represented by formula II, a monomer represented by formula III and an aqueous medium is added.
18. The method for preparing a core-shell structure polymer according to claim 16 or 17, characterized in that: The mass of the monomer represented by formula I introduced in the first stage polymerization is 70% to 85% of the total mass of the monomer represented by formula I supplied in the polymerization reaction, and the mass of the monomer represented by formula I introduced in the second stage polymerization reaction is 15% to 30% of the total mass of the monomer represented by formula I supplied in the polymerization reaction.
19. The method for preparing a core-shell structure polymer according to any one of claims 16 to 18, characterized in that: The initiator provided in the first stage polymerization and the initiator provided in the second stage polymerization are both persulfates, the mass percentage of the initiator provided in the first stage polymerization is 0.05% to 0.075%, and the mass percentage of the initiator provided in the second stage polymerization is 0.05% to 0.075%, based on the total mass of the monomer represented by formula I, the monomer represented by formula II, and the monomer represented by formula III.
20. The method for preparing a core-shell structure polymer according to any one of claims 16 to 19, characterized in that: The mass percentage of the first emulsifier is 0.28% to 0.42%, based on the total mass of the monomer represented by formula I, the monomer represented by formula II, and the monomer represented by formula III.
21. The method for preparing a core-shell structure polymer according to any one of claims 16 to 20, characterized in that: The mass percentage of the second emulsifier is 0.8% to 1.2%, based on the total mass of the monomer represented by formula I, the monomer represented by formula II, and the monomer represented by formula III.
22. The method for preparing a core-shell structure polymer according to any one of claims 16 to 21, characterized in that: The mass percentage of the aqueous medium provided in the first stage polymerization is 200% to 500%, and the mass percentage of the aqueous medium provided in the second stage polymerization is 100% to 200%, based on the total mass of the monomer represented by formula I, the monomer represented by formula II and the monomer represented by formula III.
23. The method for preparing a core-shell structure polymer according to any one of claims 16 to 22, characterized in that: The reaction pressure of the first stage polymerization is 5.5 MPa to 7.5 MPa, and the reaction temperature is 75° C. to 85° C.
24. The preparation method according to any one of claims 16 to 23, characterized in that The reaction pressure of the second polymerization is 4.5 MPa to 6.5 MPa, and the reaction temperature is 86° C. to 95° C.
25. The method for preparing a core-shell structure polymer according to any one of claims 16 to 24, characterized in that: The initiator can be selected from one or both of potassium persulfate and ammonium persulfate.
26. The method for preparing a core-shell structure polymer according to any one of claims 16 to 25, characterized in that: The first emulsifier is an alkali metal perfluorooctanoate.
27. The method for preparing a core-shell structure polymer according to any one of claims 16 to 26, characterized in that: The second emulsifier is one or both of polyoxyethylene-4-phenol ether ammonium sulfate and nonylphenol polyoxyethylene ether ammonium sulfate.
28. A polymer emulsion, characterized in that The polymer emulsion comprises the core-shell structure polymer according to any one of claims 1 to 10.
29. Use of the core-shell structure polymer according to any one of claims 1 to 10 in a secondary battery.
30. A water-based primer slurry comprising a binder, a conductive agent and an aqueous medium, characterized in that: The binder comprises the core-shell structure polymer according to any one of claims 1 to 10.
31. The aqueous base coating slurry according to claim 30, characterized in that The core-shell structure polymer is added to the aqueous base coating slurry in the form of an emulsion containing the core-shell structure polymer.
32. The aqueous primer slurry according to claim 30 or 31, characterized in that: The mass ratio of the conductive agent to the binder is 0.8:1 to 1:
1.
33. The aqueous base coating slurry according to any one of claims 30 to 32, characterized in that When the solid content of the aqueous primer slurry is 10% to 20%, the viscosity of the aqueous primer slurry is 300 mPa·s to 900 mPa·s.
34. A method for preparing a water-based primer, characterized in that: The following steps are involved: Using a gravure coater, coating the aqueous primer slurry according to any one of claims 30 to 33 on the surface of the current collector; After drying, a water-based primer layer is obtained, and the thickness of the water-based primer layer is 1 μm to 3 μm.
35. A secondary battery, characterized in that: It comprises a positive electrode sheet, a separator, a negative electrode sheet and an electrolyte, and the positive electrode sheet and / or the negative electrode sheet comprises a water-based primer layer prepared by the preparation method according to claim 34.
36. The secondary battery according to claim 35, characterized in that The secondary battery includes at least one of a lithium ion battery, a sodium ion battery, a magnesium ion battery, and a potassium ion battery.
37. A battery module, characterized in that: Includes the secondary battery according to claim 35 or 36.
38. A battery pack, characterized in that: The battery module comprises at least one selected from the secondary battery according to claim 35 or 36 and the battery module according to claim 34.
39. An electrical device, characterized in that: The battery comprises at least one selected from the group consisting of the secondary battery according to claim 35 or 36, the battery module according to claim 37, and the battery pack according to claim 38.