Additive for carbon dioxide reduction catalyst, catalyst layer, cathode, ion exchange membrane-electrode assembly, and solid electrolyte electrolysis device

By using an aryl carbon carrier and inorganic particles or metal coordination compound additives in the catalyst layer, the problem of insufficient hydrophobicity of the catalyst layer is solved, and high electrolysis efficiency and conductivity of the carbon dioxide electrolytic reduction reaction are achieved.

CN118786249APending Publication Date: 2024-10-15IDEMITSU KOSAN CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380023492.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-02-28
Filing Date
2023-02-22
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

In the carbon dioxide reduction reaction, the insufficient hydrophobicity of the catalyst layer causes the electrolyte to leak through the ion exchange membrane, resulting in a decrease in the function of the catalyst layer, an increase in resistance, and a decrease in electrolysis efficiency.

Method used

Carbon carriers with aromatic groups are used as additives, combined with inorganic particles or metal coordination compounds, to improve the hydrophobicity and conductivity of the catalyst layer through chemical modification to ensure the efficiency of the catalyst layer in electrolysis reactions.

Benefits of technology

It effectively suppresses the functional decline of the catalyst layer, improves the electrolysis efficiency of the carbon dioxide electrolysis reduction reaction, maintains the conductivity and hydrophobicity of the catalyst layer, prevents electrolyte adhesion, and improves current density and selectivity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118786249A_ABST
    Figure CN118786249A_ABST
Patent Text Reader

Abstract

Provided are: a catalyst layer capable of suppressing a decrease in function; an additive for a carbon dioxide reduction catalyst, which has excellent conductivity of an electrode catalyst layer and excellent electrolytic efficiency of a carbon dioxide electrolytic reduction reaction; an electrode; an ion exchange membrane-electrode assembly; the additive for a carbon dioxide reduction catalyst is provided with a carrier containing carbon and having an aryl group on the surface.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The technology of the present invention relates to an additive for a carbon dioxide reduction catalyst, a catalyst layer, a cathode, an ion exchange membrane-electrode assembly, and a solid electrolyte type electrolysis device. Background Art

[0002] Carbon dioxide is emitted when energy is extracted from fossil fuels. It can be said that the increase in the concentration of carbon dioxide in the atmosphere is one of the causes of global warming. Since carbon dioxide is an extremely stable substance, there is currently almost no way to use it. However, there is also a demand for the times that global warming is becoming more and more serious, and a new technology for converting carbon dioxide into other substances and recycling it again is required. For example, people are developing a carbon dioxide reduction device that can directly reduce gaseous carbon dioxide.

[0003] For example, Patent Document 1 discloses that in order to obtain a catalyst layer for a carbon dioxide reduction electrode that exhibits a high partial current density by controlling wettability and can withstand long-term operation, the catalyst layer contains a metal catalyst supported on a carbon material, an ion conductive substance, and a hydrophilic polymer, and the BET specific surface area (A) obtained by adsorbing nitrogen is 2.4 Å. N2 ) and the BET specific surface area (A H20 ) ratio (A H2O / A N2 ) is less than 0.08.

[0004] Patent document 2 discloses that in a reduction reaction of a carbon compound, in order to make it possible to suppress the production ratio of hydrogen based on side reactions and to increase the production ratio of reduction products based on the reduction reaction of the carbon compound, an electrode body modified with a hydrophobic polymer is included in an electrode for reduction reaction used in the reduction reaction of the carbon compound.

[0005] Patent Document 3 discloses a method of solving the technical problem by grafting a hydrophobic and / or hydrophilic molecule onto carbon.

[0006] Furthermore, Non-Patent Document 1 discloses a method of controlling the wettability of an electrode and preventing a decrease in function by adding polytetrafluoroethylene (PTFE) fine particles to a catalyst layer for a carbon dioxide reduction electrode.

[0007] Prior art literature

[0008] Patent Literature

[0009] Patent Document 1: Japanese Patent Application Publication No. 2021-147677

[0010] Patent Document 2: Japanese Patent Application Publication No. 2021-21095

[0011] Patent Document 3: Japanese Patent Application Publication No. 2021-2528

[0012] Non-patent literature

[0013] Non-patent literature 1: Z. Xing, L Hu, D. S. Ripatti, X. Hu, X. Feng, Nature Communications, 2021, 12, 136. Summary of the invention

[0014] Problem that the invention aims to solve

[0015] In an electrolysis device having a catalyst layer that performs a carbon dioxide reduction reaction and an ion exchange membrane, if the electrolyte permeates the ion exchange membrane and seeps into the catalyst layer, the function of the catalyst layer is degraded.

[0016] In Patent Documents 1, 2 and Non-Patent Document 1, although attempts are made to hydrophobize the catalyst layer by adding a hydrophobic polymer to the catalyst layer, the hydrophobic polymer is insulating and increases the resistance of the catalyst layer. In addition, in Patent Document 3, although a hydrophobic compound is loaded on the gas diffusion layer or the intermediate layer between the gas diffusion layer and the catalyst layer to improve the hydrophobicity, the hydrophobicity of the catalyst layer itself has not yet been improved, and the effect of hydrophobization is limited.

[0017] The present invention is made in view of the above situation. The purpose of the technical subject of the present invention is to provide a catalyst layer that can suppress the decline of function, as well as an additive for a carbon dioxide reduction catalyst, an electrode, an ion exchange membrane-electrode assembly and a solid electrolyte electrolysis device that have excellent conductivity and electrolysis efficiency of the carbon dioxide electrolysis reduction reaction of the electrode catalyst layer.

[0018] Solutions for solving problems

[0019] <1> An additive for a carbon dioxide reduction catalyst comprises a carrier containing carbon and having an aromatic group on the surface.

[0020] <2> An additive for a carbon dioxide reduction catalyst having a carrier containing carbon, wherein the ratio of the amount of water vapor adsorbed at 25° C. and a water vapor pressure of 2.2 kPa to the amount of water vapor adsorbed at the same temperature and a water vapor pressure of 3.1 kPa is less than 0.5.

[0021] <3> according to <1> In the additive for the carbon dioxide reduction catalyst, the aromatic group comprises one or more selected from a phenyl group and a condensed ring group having 2 to 6 benzene rings.

[0022] <4> according to <3> In the additive for the carbon dioxide reduction catalyst, the condensed ring group having 2 to 6 benzene rings comprises at least one selected from the group consisting of naphthyl, anthracenyl, phenanthryl and pyrene.

[0023] <5> according to <1> , <3> and <4> The additive for a carbon dioxide reduction catalyst as described above is characterized in that the aryl group has one or more substituents selected from the group consisting of an alkyl group, a fluoroalkyl group, a phenyl group, a fluorophenyl group and a fluorine atom.

[0024] <6> according to <1> and <3> to <5> The additive for a carbon dioxide reduction catalyst according to any one of the preceding claims, wherein the aryl group is any one or more of the groups shown in (1) to (8);

[0025] [Chemical formula 1]

[0026]

[0027] In (1) to (8), * represents a bonding portion with the surface of the support.

[0028] <7> A catalyst layer comprising: an additive having a carrier, the carrier comprising carbon and having an aromatic group on the surface, and

[0029] A catalyst comprising a carrier, wherein the carrier comprises carbon and carries inorganic fine particles or a metal coordination compound.

[0030] <8> A catalyst layer comprising:

[0031] An additive having a carrier containing carbon, wherein the ratio of the amount of water vapor adsorbed at 25°C and a water vapor pressure of 2.2 kPa to the amount of water vapor adsorbed at the same temperature and a water vapor pressure of 3.1 kPa is less than 0.5, and

[0032] A catalyst comprising a carrier, wherein the carrier comprises carbon and carries inorganic fine particles or a metal coordination compound.

[0033] <9> according to <7> or <8> The catalyst layer, wherein the inorganic particles are particles selected from gold, silver, copper, nickel, iron, cobalt, zinc, chromium, palladium, tin, manganese, aluminum, indium, bismuth, molybdenum and carbon nitride; the metal coordination compound is a metal coordination compound obtained by coordination of a ligand with a metal selected from copper, nickel, iron, cobalt, zinc, manganese, molybdenum and aluminum or an ion of the metal.

[0034] <10> according to <7> In the catalyst layer, the aromatic group comprises at least one selected from a phenyl group and a condensed ring group having 2 to 6 benzene rings.

[0035] <11> The catalyst layer according to <10>, wherein the condensed ring group having 2 to 6 benzene rings includes one or more selected from the group consisting of naphthyl, anthracenyl, phenanthrenyl and pyrenyl.

[0036] <12> according to <7> The catalyst layer, wherein the aryl group has one or more substituents selected from the group consisting of an alkyl group, a fluoroalkyl group, a phenyl group, a fluorophenyl group and a fluorine atom.

[0037] <13> according to <7> The catalyst layer, wherein the aromatic group is any one or more of the groups shown in (1) to (8),

[0038] [Chemical formula 2]

[0039]

[0040] In (1) to (7), * represents a bonding portion with the surface of the support.

[0041] <14> A cathode having: <9> The catalyst layer and the gas diffusion layer.

[0042] <15> An ion exchange membrane-electrode assembly having: <14> The cathode, solid electrolyte, and anode.

[0043] <16> The ion exchange membrane-electrode assembly according to <15>, wherein the solid electrolyte is an anion exchange membrane.

[0044] <17> A solid electrolyte electrolysis device comprising: the cathode according to <14>, an anode forming a pair of electrodes with the cathode,

[0045] a solid electrolyte interposed between the cathode and the anode in a contacting state, and

[0046] A voltage applying unit applies a voltage between the cathode and the anode.

[0047] <18> according to <17> The solid electrolyte electrolysis device, wherein the solid electrolyte is an anion exchange membrane.

[0048] Effects of the Invention

[0049] According to the technology of the present invention, a catalyst layer capable of suppressing functional degradation, an additive for a carbon dioxide reduction catalyst, a cathode, an ion exchange membrane-electrode assembly and a solid electrolyte electrolysis device having excellent conductivity of an electrode catalyst layer and electrolysis efficiency of a carbon dioxide electrolytic reduction reaction can be provided.

[0050] Brief description of the attached figure

[0051] Figure 1This is a schematic diagram of an ion exchange membrane-electrode assembly that can be preferably used in this embodiment.

[0052] Figure 2 It is a schematic diagram of a solid electrolyte electrolysis device preferably used in this embodiment.

[0053] Figure 3 It is a graph showing the relative water vapor adsorption amount of Examples and Comparative Examples. DETAILED DESCRIPTION

[0054] The upper limit and lower limit of the numerical range described in this specification can be arbitrarily combined. For example, when the numerical range is described as "A to B" and "C to D", the numerical range of "A to D" and "C to B" is also included in the technical scope of the present invention.

[0055] In addition, unless otherwise specified, the numerical range of "lower limit value to upper limit value" described in this specification means more than the lower limit value and less than the upper limit value.

[0056] <Additives for CO2 reduction catalysts>

[0057] The additive for a carbon dioxide reduction catalyst according to the first embodiment includes a carrier containing carbon and having an aromatic group on the surface.

[0058] The carbon dioxide reduction catalyst additive according to the second embodiment has a carrier containing carbon, and the ratio of the water vapor adsorption amount at 25° C. and water vapor pressure 2.2 kPa to the water vapor adsorption amount at the same temperature and water vapor pressure 3.1 kPa is less than 0.5.

[0059] The carbon dioxide reduction catalyst additive according to the first embodiment and the carbon dioxide reduction catalyst additive according to the second embodiment of the present technology may be collectively referred to as “the carbon dioxide reduction catalyst additive according to the present embodiment”.

[0060] In general, a carbon dioxide reduction electrolysis device includes a cathode having a gas diffusion layer and a catalyst layer that performs a carbon dioxide reduction reaction, an ion exchange membrane, an anode, and an electrolytic solution (electrolyte) supplied to the anode.

[0061] The ion exchange membrane has the property of allowing electrolyte to pass through in addition to ions. It is often found that the electrolyte supplied to the anode passes through the ion exchange membrane in a small amount, causing excess water inside the catalyst layer; the electrolyte dissolved in the electrolyte precipitates in the form of salt near the cathode, blocking the flow path of carbon dioxide, etc. These phenomena bring about adverse effects such as hindering the supply of carbon dioxide to the catalyst layer, causing a decrease in electrolysis performance such as current density and selectivity. In particular, the higher the reaction temperature, the more significant this effect occurs.

[0062] As a method for controlling the amount of water in the catalyst layer, there is a method for controlling the hydrophobicity of the catalyst layer. In the aforementioned Patent Document 1, the hydrophobicity is controlled by adding the amount of polyvinyl alcohol, polyvinyl pyrrolidone, etc., in Patent Document 2, the hydrophobicity is controlled by adding polystyrene, and in Non-Patent Document 1, the hydrophobicity is controlled by adding PTFE.

[0063] However, these hydrophobic polymers are insulators, and the addition of the hydrophobic polymer increases the resistance of the catalyst layer, causes heat generation, and reduces the electrolysis efficiency.

[0064] In Patent Document 3, hydrophobicity is improved by supporting a hydrophobic compound on the gas diffusion layer or the intermediate layer between the gas diffusion layer and the catalyst layer without using a hydrophobic polymer. However, the hydrophobicity of the catalyst layer has not been improved, so the effect of hydrophobization is limited.

[0065] In contrast, by using the carbon dioxide reduction catalyst additive according to the present embodiment as a constituent component of the catalyst layer of an electrode having a catalyst layer, not only the surface of the catalyst layer but also the entire catalyst layer can be made hydrophobic without impairing the conductivity of the catalyst layer. The reason for this is presumably as follows.

[0066] In the first embodiment of the present invention, the additive for the carbon dioxide reduction catalyst includes a carrier containing carbon with excellent electrical conductivity, and an aromatic group is provided on the surface of the carrier, so that the additive can bring hydrophobicity to the catalyst layer. Since the aromatic group is fixed to the surface of the carrier by chemical bonds, the catalyst layer can be reliably hydrophobized, and at the same time, it can be hydrophobized not only on the surface of the catalyst layer, but also throughout the interior of the catalyst layer.

[0067] The carbon dioxide reduction catalyst additive according to the second embodiment has a carrier containing carbon with excellent conductivity, and the ratio of the specific water vapor adsorption amount is less than 0.5, and the additive has conductivity and excellent hydrophobicity. Therefore, by adding the additive to the catalyst layer, the conductivity of the catalyst layer can be hydrophobicized not only on the surface of the catalyst layer but also throughout the interior of the catalyst layer without damaging the conductivity of the catalyst layer.

[0068] As a result, even if the electrolyte permeates the ion exchange membrane, the electrolyte can be prevented from adhering to the catalyst layer containing the additive for the carbon dioxide reduction catalyst according to the present embodiment, and it is difficult to hinder the supply of carbon dioxide to the catalyst layer. Accordingly, the electrolysis performance such as current density and selectivity will not be impaired, so the electrolysis efficiency of the carbon dioxide electrolytic reduction reaction is excellent.

[0069] Hereinafter, regarding the additive for a carbon dioxide reduction catalyst according to the present embodiment, a first embodiment and a second embodiment will be described in order.

[0070] [Additive for Carbon Dioxide Reduction Catalyst According to First Embodiment]

[0071] The additive for a carbon dioxide reduction catalyst according to the first embodiment has a carrier containing carbon and having an aromatic group on the surface.

[0072] As described above, the additive has conductivity and hydrophobicity by having an aromatic group on the surface of the support composed of carbon, and by incorporating the additive into the catalyst layer, conductivity and hydrophobicity can be imparted to the entire catalyst layer.

[0073] (Aryl)

[0074] Examples of the aryl group include a phenyl group and a group obtained by removing one hydrogen atom from a condensed ring containing two or more benzene rings (condensed ring group).

[0075] Among them, from the viewpoint of suppressing the steric hindrance of the aromatic groups on the surface of the carrier and ensuring the conductivity of the additive, the aromatic group preferably includes one or more selected from a phenyl group and a condensed ring group having 2 to 6 benzene rings. By making the number of benzene rings possessed by the aromatic group 6 or less, it is difficult to hinder the charge transfer between the carriers, and the conductivity is excellent.

[0076] Examples of the fused ring group having 2 to 6 benzene rings include naphthalene, anthracene, phenanthrene, pyrene, triphenylene, A group formed by removing one hydrogen atom from a fused ring such as perylene, pentacene, and pentaphene.

[0077] Among the above, the fused ring group having 2 to 6 benzene rings preferably includes a group formed by removing one hydrogen atom from one or more fused rings selected from naphthalene, anthracene, phenanthrene and pyrene. In other words, the fused ring group having 2 to 6 benzene rings preferably includes one or more selected from naphthyl, anthracenyl, phenanthryl and pyrenyl.

[0078] The fused ring group having 2 to 6 benzene rings is more preferably a pyrenyl group as a substituent.

[0079] The aryl group bonded to the surface of the carrier according to the present embodiment may be unsubstituted, or may further have one or two or more substituents.

[0080] Examples of the substituent include an alkyl group, an alkenyl group, a fluorinated alkyl group, an aryl group, a fluorinated aryl group, and a fluorine atom. The substituent may further have a substituent.

[0081] The alkyl group may be a group having 1 to 30 carbon atoms, and may be linear, branched, or cyclic. Specifically, for example, methyl, benzyl (phenylmethyl), trityl (triphenylmethyl), ethyl, n-propyl, isopropyl, n-butyl, tert-butyl, n-hexyl, cyclohexyl, n-octyl, n-dodecyl, etc. may be mentioned. The alkyl group may further have a substituent.

[0082] The upper limit of 30 for the number of carbon atoms in the alkyl group includes the number of carbon atoms of the substituent that may be further present. The same applies to the alkenyl group, the fluorinated alkyl group, the aryl group, and the fluorinated aryl group.

[0083] The alkyl group preferably has 1 to 25 carbon atoms, and more preferably has 2 to 20 carbon atoms.

[0084] When the alkyl group is linear, the number of carbon atoms is preferably 10 to 14. When the alkyl group is branched, the number of carbon atoms is preferably 1 to 3 and the group further preferably has 1 to 5 unsubstituted phenyl groups.

[0085] Examples of the alkenyl group include alkenyl groups having 2 to 30 carbon atoms, and may be linear, branched, or cyclic. Specific examples thereof include vinyl groups.

[0086] The alkenyl group preferably has 2 to 25 carbon atoms, and more preferably has 2 to 20 carbon atoms.

[0087] Fluorinated alkyl groups include fluoroalkyl groups having 1 to 30 carbon atoms, which may be linear, branched, or cyclic. Specifically, groups in which one or more hydrogen atoms in the aforementioned alkyl groups are replaced by fluorine atoms may be mentioned, such as fluoromethyl and fluoroethyl.

[0088] The fluoroalkyl group preferably has 1 to 25 carbon atoms, and more preferably has 2 to 20 carbon atoms.

[0089] When the fluoroalkyl group is linear, it preferably has 1 to 4 carbon atoms.

[0090] The aryl group as a substituent may be the same as the aryl group bonded to the surface of the support according to the present embodiment, but the number of carbon atoms is preferably 6 to 12. Specific examples thereof include phenyl and naphthyl.

[0091] Examples of the fluorinated aryl group include groups in which one or more hydrogen atoms in an aryl group as a substituent are substituted with fluorine atoms, and examples thereof include a fluorinated phenyl group having 1 to 4 fluorine atoms and a fluorinated naphthyl group having 1 to 7 fluorine atoms.

[0092] Among the above, when the aryl group bonded to the surface of the carrier according to the present embodiment has a substitution value, the substituent preferably includes one or more selected from the group consisting of an alkyl group, a fluoroalkyl group, a phenyl group, a fluorophenyl group and a fluorine atom.

[0093] Furthermore, the number of the substituents may be 1 to 2 or more, or may be 2 or more to 2 or more.

[0094] For example, when the aromatic group bonded to the surface of the carrier involved in this embodiment is a phenyl group, the phenyl group can be a structure having two fluoromethyl groups, or a structure in which four of the five hydrogen atoms of the phenyl group are substituted with fluorine atoms and the remaining one hydrogen atom is substituted with a fluorophenyl group.

[0095] Furthermore, the aromatic group bonded to the surface of the carrier involved in the present embodiment is preferably a phenyl group having a substituent, and a condensed ring group having 2 to 6 unsubstituted benzene rings, and is further preferably a phenyl group having a substituent selected from a triphenylmethyl group, a straight-chain unsubstituted alkyl group having 10 to 14 carbon atoms, and a straight-chain fluoroalkyl group having 1 to 4 carbon atoms, and a condensed ring group having 4 to 5 unsubstituted benzene rings, and is further preferably a phenyl group having a substituent selected from a straight-chain unsubstituted alkyl group having 11 to 13 carbon atoms and a straight-chain fluoroalkyl group having 2 to 3 carbon atoms, and a condensed ring group having 4 unsubstituted benzene rings.

[0096] More specifically, the aryl group bonded to the surface of the carrier involved in the present embodiment is preferably any one or more of the groups represented by the following (1) to (8). In (1) to (8), * represents the bonding portion to the surface of the carrier involved in the present embodiment. The aryl group is more preferably any one or more of the groups represented by the following (1) to (3) and (5), and is further preferably any one or more of the groups represented by the following (2), (3) and (5).

[0097] [Chemical formula 3]

[0098]

[0099] The carrier according to the present embodiment may have one type of aryl group or two or more types of aryl groups.

[0100] The carrier according to the present embodiment may have one aryl group or may have two or more aryl groups. The presence of the aryl group in the carrier can be confirmed and quantified by infrared spectroscopy.

[0101] (Method of introducing aromatic groups onto the surface of a carrier)

[0102] The method for introducing an aromatic group into the surface of the carrier according to the present embodiment (the method for chemical modification) is not particularly limited.

[0103] For example, carbon black is used as the carrier according to the present embodiment, and an aromatic compound having one primary amino group is used as a precursor. A chemical bond can be formed by causing a nucleophilic reaction of the aromatic ring on the surface of the carbon black through a diazotization reaction.

[0104] Examples of the aromatic compound include benzene and condensed ring compounds containing two or more benzene rings. The condensed ring compound containing two or more benzene rings is preferably a condensed ring compound having 2 to 6 benzene rings.

[0105] Specific examples thereof include aniline, aminonaphthalene, aminoanthracene, aminophenanthrene, and aminopyrene.

[0106] The aromatic compound having one primary amino group may further have a substituent other than the primary amino group. As the substituent, there may be mentioned: an alkyl group, an alkenyl group, a fluoroalkyl group, an aryl group, a fluoroaryl group, a fluorine atom, etc., and the substituent may further have a substituent. The details of the substituent that the aromatic compound having one primary amino group may have are the same as the substituent that the aryl group bonded to the surface of the carrier possessed by the additive for the carbon dioxide reduction catalyst involved in the first embodiment may have, and the preferred mode is also the same.

[0107] More specifically, the aromatic compound having one primary amino group is preferably any one or more of the compounds represented by the following (11) to (18).

[0108] [Chemical formula 4]

[0109]

[0110] (Carrier)

[0111] The support according to this embodiment contains carbon.

[0112] Since carbon generally has electrical conductivity, the support according to the present embodiment is a conductive support.

[0113] Carbon is not limited as long as it can be used as a conductive material for the gas diffusion layer in the electrode of the device for reducing carbon dioxide, and examples thereof include carbon black (furnace black, acetylene black, Ketjen black, medium particle thermal cracking carbon black, etc.), activated carbon, graphite, carbon nanotubes, carbon nanofibers, carbon nanohorns, graphene nanoplatelets, nanoporous carbon, etc., among which carbon black is preferred. Furthermore, as a structure, a porous structure is preferred. As carbon with a porous structure, porous carbon materials represented by graphene can be cited.

[0114] The shape, size, grade, etc. of carbon black are not limited, but the DBP oil absorption (dibutyl phthalate oil absorption) is preferably 50 to 500 ml / 100 g, more preferably 100 to 300 ml / 100 g, and further preferably 100 to 200 ml / 100 g. In addition, the primary particle size is preferably 5 to 200 nm, more preferably 10 to 100 nm, and further preferably 10 to 50 nm.

[0115] The DBP oil absorption of carbon black is determined in accordance with JIS K 6217-4:2001 (method for determining oil absorption), and the primary particle size is determined, for example, by laser diffraction particle size distribution measurement.

[0116] Carbon black may be a commercially available product, and examples thereof include Vulcan (registered trademark) XC-72 (manufactured by Cabot Corporation), Denka BLACK HS-100 (manufactured by Denka Corporation), Ketjen black EC-600JD (manufactured by Lion Specialty Chemicals Co., Ltd.), and Conductex-7055 Ultra (manufactured by Birla Carbon Co., Ltd.).

[0117] The additive for a carbon dioxide reduction catalyst according to the first embodiment preferably includes a carrier containing carbon and having an aromatic group on the surface.

[0118] [Additive for Carbon Dioxide Reduction Catalyst According to Second Embodiment]

[0119] The carbon dioxide reduction catalyst additive according to the second embodiment has a carrier containing carbon, and the ratio of the water vapor adsorption amount at 25° C. and water vapor pressure 2.2 kPa to the water vapor adsorption amount at the same temperature and water vapor pressure 3.1 kPa is less than 0.5.

[0120] In other words, the water vapor adsorption at 25°C and water vapor pressure of 2.2 kPa (unit: cm 3 (STP) / g) is set as a, and the water vapor adsorption amount (unit: cm 3 When (STP) / g) is set to b, a / b is less than 0.5.

[0121] The water vapor adsorption amount a at 25°C and a water vapor pressure of 2.2 kPa is strongly affected by the number of monolayer adsorbed molecules corresponding to the interaction force between the outermost surface of the additive and the adsorbed water molecules, and therefore represents the water adsorption capacity of the additive. The water vapor adsorption amount b at 25°C and a water vapor pressure of 3.1 kPa is strongly affected by the number of adsorbed molecules corresponding to the adsorption capacity of the additive, and thus corresponds to the surface area per unit mass of the additive, so the ratio of the water vapor adsorption amount a to the water vapor adsorption amount b (a / b) represents the surface hydrophilicity of the additive.

[0122] a / b<0.5 means that the additive for the carbon dioxide reduction catalyst exhibits high hydrophobicity and high electrical conductivity. The smaller a / b is, the more preferable it is, and it may be 0, but is usually greater than 0.01.

[0123] a / b is preferably 0.5 or less, more preferably 0.4 or less, further preferably 0.35 or less, further preferably 0.3 or less, further preferably 0.2 or less, further preferably 0.15 or less.

[0124] There is no particular limitation on the method for making the ratio (a / b) of the water vapor adsorption amount a of the additive for the carbon dioxide reduction catalyst at 25°C and a water vapor pressure of 2.2 kPa to the water vapor adsorption amount b at the same temperature and a water vapor pressure of 3.1 kPa less than 0.5. For example, a / b<0.5 can be achieved by chemically modifying the surface of a carrier containing carbon with an aromatic group.

[0125] As described above, the carbon dioxide reduction catalyst additive according to the first embodiment preferably has a ratio of the amount of water vapor adsorbed at 25°C and a water vapor pressure of 2.2 kPa to the amount of water vapor adsorbed at the same temperature and a water vapor pressure of 3.1 kPa of less than 0.5.

[0126] In addition, in the additive for a carbon dioxide reduction catalyst according to the second embodiment, it is preferred that the carrier composed of carbon has an aromatic group on the surface of the carrier.

[0127] In addition, the carbon dioxide reduction catalyst additive in the technology of the present invention is preferably covered with an ionomer described below. By covering the carbon dioxide reduction catalyst additive with an ionomer, the hydrophobic effect can be more effectively exerted on the catalyst also present in the ionomer, and the electrolysis efficiency can be improved.

[0128] <Catalyst layer>

[0129] The catalyst layer according to the first embodiment includes: an additive having a carrier containing carbon and having an aromatic group on the surface; and a catalyst including the carrier containing carbon and supporting inorganic fine particles or a metal complex.

[0130] The catalyst layer involved in the second embodiment includes: an additive, which has a carrier containing carbon, and the ratio of the water vapor adsorption at 25°C and a water vapor pressure of 2.2 kPa to the water vapor adsorption at the same temperature and a water vapor pressure of 3.1 kPa is less than 0.5; and a catalyst, which includes a carrier containing carbon and carrying inorganic particles or a metal coordination compound.

[0131] The catalyst layer according to the first embodiment and the catalyst layer according to the second embodiment may be simply referred to as “catalyst layer according to the present embodiment”.

[0132] In addition, the "additive having a carrier containing carbon and having an aromatic group on the surface" contained in the catalyst layer according to the first embodiment is sometimes referred to as the additive according to the first embodiment. The "additive having a ratio of a water vapor adsorption amount at 25°C and a water vapor pressure of 2.2 kPa to a water vapor adsorption amount at the same temperature and a water vapor pressure of 3.1 kPa of less than 0.5" contained in the catalyst layer according to the second embodiment is sometimes referred to as the additive according to the second embodiment.

[0133] Furthermore, the additive according to the first embodiment and the additive according to the second embodiment may be collectively referred to simply as “the additive according to the present embodiment”.

[0134] In the catalyst layer involved in the present embodiment, the type of catalyst contained in the catalyst layer is not particularly limited. The catalyst layer involved in the present embodiment is suitable for use as a catalyst layer containing a carbon dioxide reduction catalyst, but can also be suitable for various catalyst layers that want to avoid disadvantages caused by water immersion, water vapor contact, salt precipitation, etc. of the catalyst layer.

[0135] (additive)

[0136] The additive according to the first embodiment is the same as the additive for the carbon dioxide reduction catalyst according to the first embodiment, and the preferred aspects are also the same.

[0137] An additive having a carrier containing carbon and having an aromatic group on the surface can suppress the decline in the function of the catalyst contained in the catalyst layer because it can make the catalyst layer hydrophobic not only on the surface but also throughout the entire catalyst layer from the inside of the catalyst layer without damaging the conductivity of the catalyst layer containing the additive.

[0138] In the additive involved in the second embodiment, the "ratio of the water vapor adsorption amount at 25°C and a water vapor pressure of 2.2 kPa to the water vapor adsorption amount at the same temperature and a water vapor pressure of 3.1 kPa" is the same as the "ratio (a / b) of the water vapor adsorption amount a at 25°C and a water vapor pressure of 2.2 kPa to the water vapor adsorption amount b at the same temperature and a water vapor pressure of 3.1 kPa" in the additive for the carbon dioxide reduction catalyst involved in the second embodiment.

[0139] The additive according to the second embodiment also exhibits higher hydrophobicity and higher conductivity as a / b is smaller. A smaller a / b is more preferable and may be 0, but is usually greater than 0.01.

[0140] a / b is preferably 0.5 or less, more preferably 0.4 or less, further preferably 0.35 or less, further preferably 0.3 or less, further preferably 0.2 or less, further preferably 0.15 or less.

[0141] By making the catalyst layer contain the additive involved in the second embodiment, the catalyst layer can be hydrophobized not only on the surface but also throughout the entire catalyst layer from the inside of the catalyst layer without damaging the conductivity of the catalyst layer, thereby suppressing the decline in the function of the catalyst contained in the catalyst layer.

[0142] The additives involved in the first embodiment and the additives involved in the second embodiment can make the catalyst layer containing these additives hydrophobic not only on the surface but also throughout the entire range from the inside, and can maintain conductivity. Therefore, they can be used as additives for various catalyst layers that want to avoid disadvantages caused by water immersion, water vapor contact, salt precipitation, etc. of the catalyst layer.

[0143] (catalyst)

[0144] The catalyst layer according to the present embodiment includes a catalyst including a carrier containing carbon and supporting inorganic fine particles or a metal complex.

[0145] In the catalyst of the technology of the present invention, the component that exhibits catalytic action is inorganic particles or metal coordination compounds supported on a carrier, but in the technology of the present invention, the inorganic particles and metal coordination compounds are called "catalyst sources", and the carrier supporting the catalyst source is called "catalyst".

[0146] [Carrier]

[0147] The carrier used may be the carrier according to the present embodiment contained in the additive for a carbon dioxide reduction catalyst according to the first present embodiment, and preferably contains carbon black.

[0148] Preferred embodiments of carbon black are the same as those described in the description of the additive for a carbon dioxide reduction catalyst according to the first embodiment.

[0149] [Inorganic microparticles, metal coordination compounds]

[0150] The carrier according to the present embodiment supports inorganic fine particles or a metal complex as a catalyst source.

[0151] Inorganic particles and metal complexes are not particularly limited as long as they are components that exhibit catalytic activity. It should be noted that in the technology of the present invention, inorganic particles refer to metals and inorganic compounds having an average particle size of 1 to 100 nm as measured by photographic observation using a scanning electron microscope or the like.

[0152] For example, when the catalyst source is used in a catalyst layer for a fuel cell, platinum, gold, nickel, ruthenium, rhodium, etc. can be used as inorganic particles, and nickel complexes, cobalt complexes, iron complexes, manganese complexes, zinc complexes, etc. can be used as metal complexes.

[0153] In addition, for example, when the catalyst source is used for a catalyst layer for a secondary battery electrode, platinum, gold, nickel, iridium, metal oxides, etc. can be used as inorganic particles. In addition, nickel complexes, cobalt complexes, iron complexes, manganese complexes, zinc complexes, etc. can be used as metal complexes.

[0154] When the catalyst layer is used as a catalyst layer for reducing carbon dioxide, it is preferred that the inorganic fine particles and the metal complex use a catalyst source having a function of generating at least carbon monoxide by a reduction reaction.

[0155] Specifically, the inorganic fine particles for reducing carbon dioxide are preferably selected from the group consisting of gold, silver, copper, nickel, iron, cobalt, zinc, chromium, palladium, tin, manganese, aluminum, indium, bismuth, molybdenum, and carbon nitride. The inorganic fine particles may be used alone or in combination of two or more.

[0156] Among the above, from the viewpoint of the reaction efficiency of the carbon dioxide reduction reaction, the material of the inorganic fine particles is preferably silver, gold, zinc, tin, copper and bismuth, more preferably silver, gold, copper and tin, and even more preferably silver, gold and copper.

[0157] Consider from the viewpoint of the reaction speed of carbon dioxide reduction reaction, the average particle diameter of the inorganic particles as the carbon dioxide reduction catalyst source is preferably below 65nm, preferably below 60nm, preferably below 50nm, preferably below 40nm, preferably below 30nm. In addition, the lower limit of average particle diameter is unrestricted, and is preferably above 1nm, more preferably above 5nm, from the aspect of manufacturing ease.

[0158] The average particle size can be measured by, for example, photographic observation using a scanning electron microscope or the like.

[0159] The metal complex used as a catalyst source for reducing carbon dioxide is a metal complex in which a ligand is coordinated to a metal or an ion of the metal. The metal ion is preferably selected from copper, nickel, iron, cobalt, zinc, manganese, molybdenum and aluminum.

[0160] Among the above, from the viewpoint of the reaction efficiency of the carbon dioxide reduction reaction, the metal is preferably nickel, cobalt, iron, copper, zinc and manganese, more preferably nickel, cobalt, iron and copper, and further preferably nickel, cobalt and iron. The metal coordination compound may contain only one metal or ions of the metal, or may contain two or more metals or ions of the metal.

[0161] The type of ligand is not particularly limited, and examples thereof include phthalocyanine coordination compounds, porphyrin coordination compounds, pyridine coordination compounds, metal-supported covalently bonded triazine structures, metal-organic structures, etc. Among them, phthalocyanine coordination compounds, porphyrin coordination compounds, pyridine coordination compounds, and metal-supported covalently bonded triazine structures are preferred, phthalocyanine coordination compounds, porphyrin coordination compounds, and metal-supported covalently bonded triazine structures are more preferred, and porphyrin coordination compounds and metal-supported covalently bonded triazine structures are further preferred. The metal coordination compound may contain only one ligand, or may contain two or more ligands.

[0162] As described above, the carbon dioxide reduction catalyst layer according to the present embodiment is preferably a catalyst layer comprising:

[0163] The additive according to the present embodiment (the additive for the carbon dioxide reduction catalyst according to the present embodiment); and

[0164] A catalyst comprising a carrier comprising carbon and carrying inorganic fine particles or a metal coordination compound,

[0165] The inorganic particles are particles selected from gold, silver, copper, nickel, iron, cobalt, zinc, chromium, palladium, tin, manganese, aluminum, indium, bismuth, molybdenum and carbon nitride; the aforementioned metal coordination compound is a metal coordination compound coordinated with a metal selected from copper, nickel, iron, cobalt, zinc, manganese, molybdenum and aluminum or an ion of the metal.

[0166] The inorganic fine particles and the metal complex are supported on the carrier according to the present embodiment by a known method such as vapor deposition, precipitation, adsorption, deposition, bonding, welding, physical mixing, and spraying.

[0167] In addition, the catalyst in the technology of the present invention is preferably covered with an ionomer described below. By covering the catalyst with an ionomer, an ion conduction path between the covered catalyst and the solid electrolyte described below is easily formed, and the ions generated by the reaction are easily moved, which can improve the electrolysis efficiency.

[0168] [Ionomer]

[0169] The catalyst layer may further contain an ionomer.

[0170] The ionomer functions as a binder resin in the catalyst layer. It is a matrix resin (continuous phase) that can disperse and immobilize the additives and catalysts involved in the present embodiment, and also has the function of transferring ions generated by electrolysis and improving the CO2 electrolysis efficiency. In addition, from the viewpoint of improving conductivity, the ionomer is preferably a polymer electrolyte. The polymer electrolyte is more preferably an ion exchange resin. The ion exchange resin can be a cation exchange resin or an anion exchange resin, but is preferably an anion exchange resin.

[0171] In particular, when an anion exchange resin is used, the anion exchange resin itself has a carbon dioxide adsorption capacity, and the ease of ion transfer of the ion exchange resin and the electrolysis efficiency of carbon dioxide can be greatly improved.

[0172] Examples of the cation exchange resin include fluorine resins having a sulfone group and styrene-divinylbenzene copolymers having a sulfone group. Commercially available products may also be used, such as Nafion (manufactured by Chemours), Aquivion (manufactured by Solvay Specialty Polymers), DIAION (manufactured by Mitsubishi Chemical Corporation), and Fumasep (manufactured by FUMATECH).

[0173] Examples of the anion exchange resin include resins having one or more ion exchange groups selected from quaternary ammonium groups, primary amino groups, secondary amino groups, and tertiary amino groups. Commercially available products may also be used, such as Sustainion (manufactured by Dioxide Materials), Fumasep (manufactured by FUMATECH), PENTION (manufactured by Xergy), DURION (manufactured by Xergy), NEOSEPTA (manufactured by ASTOM), and TOYOPEARL (manufactured by Tosoh Corporation).

[0174] From the viewpoint of improving conductivity, the basic site density of the anion exchange resin in a dry state is preferably 2.0 to 5.0 mmol / cm 3 , more preferably 2.5 mmol / cm 3 Above and less than 4.5mmol / cm 3 , more preferably 2.9 mmol / cm 3 Above and less than 4.5mmol / cm 3 .

[0175] The base site density of anion exchange resin can be determined by 1 It can be obtained by integrating the signal during H NMR measurement.

[0176] In addition, for an anion exchange resin, a dry state means a state in which the content of free water in the anion exchange resin is 0.01 g or less per 1 g of the resin. For example, the anion exchange resin can be brought into a dry state by heating in a vacuum.

[0177] When the cathode according to the present embodiment is used in an ion exchange membrane-electrode assembly and a solid electrolyte electrolyzer described later, the ionomer is preferably made of the same resin as that of the solid electrolyte (ion exchange membrane) from the viewpoint of improving conductivity.

[0178] From the viewpoint of improving the hydrophobicity of the catalyst layer and suppressing the decrease in catalyst function, the content of the additive according to the present embodiment in the catalyst layer is preferably 1 to 90 mass %, more preferably 5 to 70 mass %, and even more preferably 10 to 50 mass %.

[0179] From the viewpoint of further improving the production efficiency of synthesis gas containing CO, the content of the catalyst according to the present embodiment in the catalyst layer is preferably 5 to 90 mass %, more preferably 10 to 80 mass %, and even more preferably 15 to 60 mass %.

[0180] <Cathode>

[0181] The cathode (cathode) according to the present embodiment includes the above-mentioned carbon dioxide reduction catalyst layer according to the present embodiment and a gas diffusion layer.

[0182] By providing the cathode according to the present embodiment with a catalyst layer containing the additive according to the present embodiment, it is possible to stably produce synthesis gas containing CO without hindering the carbon dioxide reduction reaction in the catalyst layer. Therefore, the electrolysis efficiency of the carbon dioxide electrolytic reduction reaction is excellent.

[0183] [Gas diffusion layer]

[0184] The gas diffusion layer is made of, for example, carbon paper, nonwoven fabric, or a metal mesh, and examples thereof include graphite carbon, glassy carbon, titanium, and SUS steel.

[0185] <Ion exchange membrane-electrode assembly>

[0186] The ion exchange membrane-electrode assembly according to the present embodiment includes the cathode according to the present embodiment described above, a solid electrolyte, and an anode.

[0187] The ion exchange membrane-electrode assembly according to the present embodiment includes a cathode having a catalyst layer containing the additive according to the present embodiment, and therefore can stably produce synthesis gas containing CO without hindering the carbon dioxide reduction reaction in the catalyst layer. Therefore, the electrolysis efficiency of the carbon dioxide electrolytic reduction reaction is excellent.

[0188] Figure 1 This is a schematic diagram of an ion exchange membrane-electrode assembly that can be preferably used in this embodiment. Figure 1, an ion exchange membrane-electrode assembly 50 is shown, which has: a gas diffusion layer 10, a catalyst layer 20, a solid electrolyte 30, and an anode 40. The catalyst layer 20 includes: an ionomer 22, a plurality of catalysts 24 according to the present embodiment, and a plurality of additives according to the present embodiment (additives for carbon dioxide reduction catalysts according to the present embodiment) 26. The combination of the gas diffusion layer 10 and the catalyst layer 20 constitutes a cathode according to the present embodiment.

[0189] like Figure 1 As shown, carbon dioxide (CO 2 ) is supplied to the catalyst layer 20 through the gas diffusion layer 10 , and carbon monoxide (CO) is generated through a reduction reaction.

[0190] the following, Figure 1 The description is given with symbols omitted.

[0191] [Solid Electrolyte]

[0192] The ion exchange membrane-electrode assembly according to the present embodiment includes a solid electrolyte.

[0193] The solid electrolyte may be a polymer membrane. The polymer may be various ionomers, which may be a cation exchange resin or an anion exchange resin, but is preferably an anion exchange resin. That is, the solid electrolyte is preferably an anion exchange membrane. In addition, it is more preferred to use the same anion exchange resin as the ionomer used in the above-mentioned catalyst layer.

[0194] As the solid electrolyte, a commercially available product as a cation exchange membrane or an anion exchange membrane may be used.

[0195] When an anion exchange membrane is used as the solid electrolyte, the base site density is preferably 0.5 to 5.0 mmol / cm 3 , more preferably 2.5 mmol / cm 3 Above and less than 4.5mmol / cm 3 , more preferably 2.9 mmol / cm 3 Above and less than 4.5mmol / cm 3 .

[0196] As the cation exchange membrane, for example, the following can be used: a strongly acidic cation exchange membrane formed by introducing a sulfone group into a fluororesin matrix, Nafion 117, Nafion 115, Nafion 212, Nafion 350 (manufactured by Chemrous), a strongly acidic cation exchange membrane formed by introducing a sulfone group into a styrene-divinylbenzene copolymer matrix, Neosepta CSE (manufactured by ASTOM), etc.

[0197] Examples of the anion exchange membrane include an anion exchange membrane having one or more ion exchange groups selected from quaternary ammonium groups, primary amino groups, secondary amino groups, and tertiary amino groups. Specifically, examples include Neosepta (registered trademark) ASE, AHA, ACS, AFX (manufactured by ASTOM Co., Ltd.); SELEMION (registered trademark) AMVN, DSVN, AAV, ASVN, AHO (manufactured by Asahi Glass Co., Ltd.), etc.

[0198] Regarding the reduction reaction of carbon dioxide, the reduction reaction at the cathode involved in this embodiment varies depending on the type of solid electrolyte. When a cation exchange membrane is used as the solid electrolyte, the reduction reaction of the following reaction formulas (1) and (2) is generated, and when an anion exchange membrane is used as the solid electrolyte, the reduction reaction of the following reaction formulas (3) and (4) is generated.

[0199] CO2+2H - +2e - →CO+H2O (1)

[0200] 2H + +2e - →H2 (2)

[0201] H2O+CO2+2e - →CO+2OH - (3)

[0202] 2H2O+2e - →H2+2OH - (4)

[0203] [anode]

[0204] The oxidation reaction at the anode varies depending on the type of solid electrolyte. When a cation exchange membrane is used as the solid electrolyte, an oxidation reaction of the following reaction formula (5) occurs, and when an anion exchange membrane is used as the solid electrolyte, an oxidation reaction of the following reaction formula (6) occurs.

[0205] 2H2O→O2+4H + +4e - (5)

[0206] 4OH - →O2+2H2O+4e - (6)

[0207] The anode is a gas diffusion electrode comprising a gas diffusion layer.

[0208] The gas diffusion layer includes, for example, a metal mesh. Examples of the electrode material of the anode include Ir, IrO2, Ru, RuO2, Co, CoOx, Cu, CuOx, Fe, FeOx, FeOOH, FeMn, Ni, NiOx, NiOOH, NiCo, NiCe, NiC, NiFe, NiCeCoCe, NiLa, NiMoFe, NiSn, NiZn, SUS, Au, and Pt.

[0209] <Solid electrolyte electrolysis device>

[0210] The solid electrolyte electrolysis device according to the present embodiment comprises: the cathode according to the present embodiment described above, an anode forming a pair of electrodes with the cathode, a solid electrolyte interposed in contact with the cathode and the anode, and a voltage applying unit for applying a voltage between the cathode and the anode.

[0211] The solid electrolyte electrolysis device according to the present embodiment includes a cathode having a catalyst layer containing the additive according to the present embodiment, and therefore can stably produce synthesis gas containing CO without hindering the carbon dioxide reduction reaction in the catalyst layer. Therefore, the electrolysis efficiency of the carbon dioxide electrolytic reduction reaction is excellent.

[0212] Figure 2 It is a schematic diagram of a solid electrolyte electrolysis device preferably used in this embodiment.

[0213] Figure 2 A solid electrolyte electrolysis device 800 is shown, which comprises: a cathode 200 constituting the electrode involved in this embodiment, an anode 400 constituting a pair of electrodes with the cathode 200, a solid electrolyte 300 interposed between the cathode 200 and the anode 400 in a contact state, and a voltage application unit 700 for applying a voltage between the cathode 200 and the anode 400.

[0214] Figure 2 The solid electrolyte electrolysis device 800 shown further includes a cathode current collecting plate 100 , an anode current collecting plate 500 , and an electrolyte 600 .

[0215] The electrode according to the present embodiment described above can be used as the cathode 200. Figure 1 The solid electrolyte 300 is the same as the solid electrolyte 30 in the embodiment of the present invention, and the solid electrolyte 300 is preferably an anion exchange membrane. Figure 1 The anode 40 in is the same.

[0216] The details of the cathode 200, the solid electrolyte 300 and the anode 400 are as described above.

[0217] Hereinafter, each element other than the cathode 200 , the solid electrolyte 300 , and the anode 400 will be described with reference numerals omitted.

[0218] [Cathode collector plate]

[0219] As the cathode collector plate, for example, metal materials such as copper (Cu), nickel (Ni), stainless steel (SUS), nickel-plated steel, and brass can be listed, among which copper is preferred from the viewpoint of ease of processing and cost. When the material is a metal material, the shape of the cathode collector plate can be, for example, metal foil, metal plate, metal film, porous metal, perforated metal, foamed metal, etc.

[0220] A gas supply hole for supplying a raw gas containing carbon dioxide to the cathode and a gas recovery hole for recovering a generated gas containing carbon monoxide may also be provided on the cathode collector plate. By having the gas supply hole and the gas recovery hole, the raw gas can be uniformly and efficiently fed to the cathode, and the generated gas (including the unreacted raw gas) can be discharged. The gas supply hole and the gas recovery hole can each independently be provided with only one or with two or more. In addition, the shape, position, size, etc. of the gas supply hole and the gas recovery hole are not limited and can be appropriately set. Moreover, in the case where the cathode collector plate is air permeable, the gas supply hole and the gas recovery hole are not necessarily required.

[0221] It should be noted that, when the cathode has a function of transferring electrons, a cathode current collecting plate is not necessarily required.

[0222] [Anode collector plate]

[0223] Anode collector plate (anode collector plate) preferably has conductivity in order to receive electrons from anode, and possesses rigidity to support anode. From this viewpoint, anode collector plate can be suitably made of metal materials such as titanium (Ti), copper (Cu), nickel (Ni), stainless steel (SUS), nickel-plated steel, brass, etc.

[0224] The anode collector plate may also be provided with a gas flow path for feeding a raw material gas (H2O, etc.) to the anode. By providing the anode collector plate with a gas flow path, the raw material gas can be fed to the anode uniformly and efficiently. It should be noted that the number, shape, position, size, etc. of the gas flow path are not limited and can be set appropriately.

[0225] [Voltage application unit]

[0226] The voltage applying unit has the function of applying voltage between the cathode and the anode by applying voltage to the cathode collector plate and the anode collector plate. Here, since the two collector plates are conductors, electrons are supplied to the cathode on the one hand and electrons are received from the anode on the other hand. In addition, for the voltage applying unit, in order to apply a suitable voltage, a control unit not shown in the figure may also be electrically connected.

[0227] [Electrolyte]

[0228] The electrolyte solution is preferably an aqueous solution having a pH of 5 or more.

[0229] For example, there can be mentioned a carbonate aqueous solution, a bicarbonate aqueous solution (for example, a KHCO 3 aqueous solution), a sulfate aqueous solution, a borate aqueous solution, sodium hydroxide, a potassium hydroxide aqueous solution, a sodium chloride aqueous solution, and the like.

[0230] (Reaction gas supply unit)

[0231] In the solid electrolyte electrolysis device involved in the present embodiment, a reaction gas supply unit (not shown) may also be provided outside the solid electrolyte electrolysis device. That is, as long as CO2 as a reaction gas is supplied to the catalyst layer provided by the cathode, the reaction gas may be supplied from the reaction gas supply unit to the gas supply hole via a pipe (not shown) or the like, or the reaction gas may be sprayed onto the surface of the cathode collector plate opposite to the surface in contact with the cathode. In addition, from an environmental perspective, it is appropriate to use factory exhaust gas discharged from a factory as the reaction gas.

[0232] [CO generation method]

[0233] Next, a CO generation method using the solid electrolyte electrolysis device according to the present embodiment will be described.

[0234] First, a reaction gas supply unit (not shown) supplies CO 2 , which is a raw material, in a gas phase to the solid electrolyte electrolysis device. At this time, CO 2 is supplied to the cathode through a gas supply hole provided in the cathode current collector plate, for example.

[0235] Next, the CO2 supplied to the cathode comes into contact with the catalyst layer of the cathode, and when a cation exchange membrane is used as a solid electrolyte, the reduction reactions of the aforementioned reaction equations (1) and (2) are generated, and when an anion exchange membrane is used as a solid electrolyte, the reduction reactions of the aforementioned reaction equations (3) and (4) are generated, thereby generating a synthetic gas containing at least CO and H2.

[0236] Next, the generated synthesis gas containing CO and H 2 is sent to a gas recovery device (not shown) through a gas recovery hole provided in the cathode current collector plate, for example, and is recovered as various predetermined gases.

[0237] Example

[0238] Next, the technology of the present invention will be specifically described using examples, but the technology of the present invention is not limited to these examples at all.

[0239] <Additive Manufacturing>

[0240] [Example 1]

[0241] After irradiating an ethanol dispersion containing 0.5 g of carbon black with an average particle size of 30 nm with ultrasonic waves for 10 minutes, the dispersion is allowed to stand in a vacuum chamber with a reduced pressure environment of 10 kPa (absolute pressure) for 10 minutes. Next, 8.3 mL of a 0.5 mol / L sodium nitrite aqueous solution is added to the dispersion. After adding 4 mmol of 4-tritylaniline [the compound represented by formula (11)] to the dispersion, 2 mL of hydrochloric acid is added and stirred at 15°C for more than 5 hours. After adding sodium hydroxide solution to the dispersion to neutralize it, the obtained slurry is washed with distilled water, the solids are recovered by a centrifuge, and the solids are vacuum dried at 60°C overnight to prepare the additive of Example 1.

[0242] In addition, the average particle diameter of carbon black is calculated|required by laser diffraction type particle size distribution measurement.

[0243] [Examples 2 to 8]

[0244] In the production of the additive of Example 1, the additives of Examples 2 to 8 were produced in the same manner except that the basic organic compounds shown in Tables 1 and 2 were used instead of 4-tritylaniline.

[0245] It should be noted that the basic organic compounds used in the production of the additives of Examples 2 to 8 are compounds represented by the above-mentioned formulae (12) to (18).

[0246] [Comparative Example 1]

[0247] In Comparative Example 1, carbon black having an average particle size of 30 nm was used as an additive.

[0248] [Comparative Example 2]

[0249] In Comparative Example 2, polytetrafluoroethylene (PTFE, manufactured by Nanoshel, trade name “Polytetrafluoroethylene Nanopowder”) having an aerodynamic particle size of 30 to 50 nm was used as an additive.

[0250] [Comparative Examples 3 and 4]

[0251] In Comparative Examples 3 and 4, no additive was used.

[0252] <Production of Catalyst>

[0253] [Examples 1 to 7 and Comparative Examples 1 to 3]

[0254] The same catalyst was used in Examples 1 to 7 and Comparative Examples 1 to 3. The catalyst was produced as follows.

[0255] In a beaker, 0.1 g of a carbon black carrier (the carrier involved in the present embodiment) is mixed in 100 mL of ethanol, and the obtained ethanol dispersion is irradiated with ultrasound for 10 minutes. Thereafter, the dispersion is allowed to stand in a vacuum chamber in a reduced pressure environment of 10 kPa (absolute pressure) for 10 minutes. Thereafter, silver nitrate is reduced by mixing 11.7 mL of a 0.1 mol / L AgNO3 solution with 1 mL of a 2.3 mol / L sodium phosphinate solution and stirring at 15 ° C for 16 hours. After the reaction is completed, the obtained slurry is washed with distilled water, the solids are recovered by a centrifuge, and the solids are vacuum dried at 60 ° C for one night to obtain catalyst powders of Examples 1 to 7 and Comparative Examples 1 to 3. The catalyst obtained is a carbon black loaded with Ag particles as a catalyst source, and the mass of the loaded Ag particles is 40 parts by mass relative to 100 parts by mass of carbon black not loaded with Ag particles.

[0256] [Example 8 and Comparative Example 4]

[0257] The same catalyst was used in Example 8 and Comparative Example 4. The preparation was carried out as follows.

[0258] In a beaker, 0.4 g of a carbon black carrier (carrier involved in the present embodiment), 1.1 mmol of pentaethylenehexamine and 0.7 mmol of nickel chloride (II) hexahydrate were mixed in 15 mL of ethanol, and ultrasonic waves were irradiated to the obtained ethanol dispersion for 10 minutes. Thereafter, the ethanol was evaporated by heating and drying the ethanol dispersion, and the obtained mixture was heated at 900 ° C in an inert gas using an electric furnace for more than 30 seconds and calcined. Thereafter, the product was washed with an aqueous sulfuric acid solution, the solid was recovered by a suction filter, and the solid was vacuum dried at 60 ° C for one night to obtain a catalyst powder loaded with a Ni coordination compound. The catalyst powder was used as the catalyst powder of Example 8 and Comparative Example 4.

[0259] The obtained catalyst had a supported Ni mass of 1 part by mass based on 100 parts by mass of carbon black on which no Ni complex was supported.

[0260] <Solid electrolyte electrolysis device>

[0261] [Example 1]

[0262] 43 mg of the obtained catalyst powder was dispersed in ethanol, and 12 mg of anion exchange resin as an ionomer to which 5 mg of the additive of Example 1 was added was mixed in the dispersion. 1 The HNMR measurement showed that the base site density was 2.8 mmol / cm 3 The anion exchange resin is a fluorine-based resin having an aromatic ring in the main chain as a base material and a quaternary ammonium group (quaternary alkylamine group) bonded to the main chain as a side chain.

[0263] After mixing, the dispersion was irradiated with ultrasound for 10 minutes and allowed to stand in a vacuum chamber at a reduced pressure of 10 kPa (absolute pressure) for 10 minutes. The dispersion was coated on carbon paper using a spray coater to form a cathode. The cathode had a coating film of the dispersion as a catalyst layer and carbon paper as a gas diffusion layer.

[0264] The anion exchange membrane with a thickness of about 30 μm (base site density 2.8 mmol / cm 3 ), a carbon anode loaded with iridium oxide (manufactured by Dioxide Materials) is laminated to the above cathode to form an ion exchange membrane-electrode assembly.

[0265] The anode is connected to an electrolyte tank (0.5 mol / L KHCO3 aqueous solution).

[0266] [Examples 2 to 7 and Comparative Examples 1 to 2]

[0267] In the manufacture of the solid electrolyte electrolysis device of Example 1, except that the additive of Example 1 was changed to any additive of Examples 2 to 7 and Comparative Examples 1 to 2, the solid electrolyte electrolysis devices of Examples 2 to 7 and Comparative Examples 1 to 2 were manufactured in the same manner.

[0268] [Example 8]

[0269] In the manufacture of the solid electrolyte electrolysis device of Example 1, the solid electrolyte electrolysis device of Example 8 was manufactured in the same manner except that the additive was changed from the additive of Example 1 to the additive of Example 8, and the ionomer was changed from the ionomer of Example 1 to Nafion (manufactured by Chemours).

[0270] [Comparative Example 3]

[0271] A solid electrolyte electrolysis device of Comparative Example 3 was manufactured in the same manner as in the manufacture of the solid electrolyte electrolysis device of Example 1, except that no additive was added.

[0272] [Comparative Example 4]

[0273] The solid electrolyte electrolysis device of Comparative Example 4 was manufactured in the same manner as that of Example 8, except that no additive was added.

[0274] <Evaluation of Solid Electrolyte Electrolyzer>

[0275] [Examples 1 to 7 and Comparative Examples 1 to 3]

[0276] Using each solid electrolyte electrolysis device of Examples 1 to 7 and Comparative Examples 1 to 3, pure CO2 was supplied to the cathode, and the solid electrolyte electrolysis device was heated to 50°C, and the applied potential of the cathode was set to -2.6 V relative to the anode, or -1 A / cm 2 The CO generation current density [mA / cm 2 ] and CO selectivity [%]. When a constant current is applied, the voltage [V] is measured instead of the current.

[0277] Table 1 shows the results.

[0278] [Table 1]

[0279]

[0280] <Evaluation of Solid Electrolyte Electrolyzer>

[0281] [Example 8 and Comparative Example 4]

[0282] Using each solid electrolyte electrolysis device of Example 8 and Comparative Example 4, pure CO2 was supplied to the cathode. At room temperature, the potential applied to the cathode was set to -1.8 V relative to the silver / silver chloride reference electrode, and CO2 was electrolyzed. The CO generation current density [mA / cm 2 ] for measurement.

[0283] Table 2 shows the results.

[0284] [Table 2]

[0285] Table 2

[0286]

[0287] As shown in Tables 1 and 2, when using additives obtained by chemically modifying the surface of the support with various aromatic amine compounds as raw materials (Examples 1 to 7), when applying -1A / cm 2At such a high current, a low required voltage and a high CO selectivity were shown. In addition, in Example 8, a high current density was shown.

[0288] On the other hand, in Comparative Example 1 using an additive that does not chemically modify the support surface with an aromatic group, Comparative Example 2 using an insulating hydrophobic polymer as an additive, and Comparative Example 3 using no additive, the required voltage becomes high and the CO selectivity decreases. In Comparative Example 4 using no additive, a low current density is shown.

[0289] <Water vapor adsorption amount of additives>

[0290] For the additives of Examples 1 to 4, 6, 7 and Comparative Example 1, the water vapor adsorption amount (a) at 25°C and a water vapor pressure of 2.2 kPa and the water vapor adsorption amount (b) at 25°C and a water vapor pressure of 3.1 kPa were measured using BELSORP-max (manufactured by Bel Co., Ltd., Japan), and the ratio (a / b) between the two is shown in Table 3. In the measurement, 0.2 to 0.3 g of the additive sample was heated at 120°C under vacuum for more than 5 hours to remove the adsorbed gas on the surface in advance, and then water vapor was introduced at 25°C to determine the adsorption amount at each water vapor pressure.

[0291] In addition, a graph in which the relative water vapor adsorption amount is plotted against the relative pressure is shown in FIG. Figure 3 Here, in Figure 3 In the formula, the relative pressure on the vertical axis means the value obtained by dividing each water vapor pressure by the saturated water vapor pressure (3.1 kPa) at 25°C. In addition, the relative water vapor adsorption on the horizontal axis means the value (a / b) obtained by dividing the water vapor adsorption at each relative pressure (a) by the water vapor adsorption at the saturated water vapor pressure at 25°C (b). When expressed by a formula, it is as shown below.

[0292] Relative pressure = (water vapor pressure at each measurement point) / (saturated water vapor pressure [= 3.1 kPa])

[0293] Relative water vapor adsorption = (water vapor adsorption at each measurement point) / (water vapor adsorption at saturated water vapor pressure)

[0294] exist Figure 3 In the graph, when the relative pressure on the horizontal axis is 0.7, it means that the relative pressure = 2.2 / 3.1, and the corresponding relative water vapor adsorption amount on the vertical axis is the ratio (a / b).

[0295] The "ratio (a / b)" shown in Table 3 is the relative water vapor adsorption amount when the relative pressure on the horizontal axis is 0.7.

[0296] It should be explained that Figure 3The details of each curve in are as follows.

[0297] -▲-(Ex.1): Example 1 (4-tritylaniline)

[0298] -■-Ex.2): Example 2 (1-aminopyrene)

[0299] -△-(Ex.3): Example 3 (3,5-bis(trifluoromethyl)aniline)

[0300] -□-(Ex.4): Example 4 (4-aminononafluorobiphenyl)

[0301] -×-(Ex.6): Example 6 (2-aminoanthracene)

[0302] -O- (Ex.7): Example 7 (4-ethylaniline)

[0303] -·-(Co-Ex.1): Comparative Example 1 (unmodified carbon black)

[0304] [Table 3]

[0305] Table 3

[0306] Ratio (a / b) Example 1 0.16 Example 2 0.10 Example 3 0.35 Example 4 0.16 Example 6 0.19 Example 7 0.46 Comparative Example 1 0.52

[0307] From Table 3 and Figure 3 It is found that the ratio (a / b) of the water vapor adsorption amount (a) at 25°C and a water vapor pressure of 2.2 kPa to the water vapor adsorption amount (b) at 25°C and a water vapor pressure of 3.1 kPa is less than 0.5. This means that the additive of the example exhibits high hydrophobicity and high conductivity.

[0308] As described above, it is estimated that by using the conductive additive according to the present embodiment, the hydrophobic effect can be exhibited without hindering high conductivity.

[0309] Industrial Applicability

[0310] According to this embodiment, for a solid electrolyte electrolysis device, for example, CO2 gas discharged from a factory is used as a raw material, and a voltage application unit is used with renewable energy such as a solar cell, so that a synthesis gas containing at least CO and H2 at a desired generation ratio can be generated. The synthesis gas thus generated can be used to generate fuel substrates, chemical raw materials, etc. through methods such as FT synthesis (Fischer-Tropsch synthesis) and methanation.

[0311] Explanation of symbols

[0312] 10: Gas Diffusion Layer

[0313] 20: Catalyst layer

[0314] 22: Ionomer

[0315] 24: Catalyst

[0316] 26: Additives (Additives for carbon dioxide reduction catalysts)

[0317] 30: Solid electrolyte (ion exchange membrane)

[0318] 40: anode

[0319] 50: Ion exchange membrane-electrode junction

[0320] 100: Cathode collector plate

[0321] 200: cathode

[0322] 300: Solid electrolyte (ion exchange membrane)

[0323] 400: anode

[0324] 500: Anode collector plate

[0325] 600: Electrolyte

[0326] 700: Voltage applying unit

[0327] 800: Solid electrolyte electrolysis device

Claims

1. An additive for a carbon dioxide reduction catalyst, comprising a carrier comprising carbon and having an aromatic group on the surface.

2. An additive for a carbon dioxide reduction catalyst, comprising a carrier containing carbon, wherein the ratio of the amount of water vapor adsorbed at 25° C. and a water vapor pressure of 2.2 kPa to the amount of water vapor adsorbed at the same temperature and a water vapor pressure of 3.1 kPa is less than 0.

5. 3 . The additive for a carbon dioxide reduction catalyst according to claim 1 , wherein the aryl group comprises one or more selected from a phenyl group and a condensed ring group having 2 to 6 benzene rings. 4 . The additive for a carbon dioxide reduction catalyst according to claim 3 , wherein the condensed ring group having 2 to 6 benzene rings comprises one or more selected from the group consisting of a naphthyl group, an anthracenyl group, a phenanthrenyl group and a pyrenyl group. 5 . The additive for a carbon dioxide reduction catalyst according to claim 1 , wherein the aryl group has one or more substituents selected from the group consisting of an alkyl group, a fluoroalkyl group, a phenyl group, a fluorophenyl group and a fluorine atom.

6. The additive for a carbon dioxide reduction catalyst according to any one of claims 1 and 3 to 5, wherein the aryl group is any one or more of the groups shown in (1) to (8); [Chemical formula 1] In (1) to (8), * represents a bonding portion with the surface of the support.

7. A catalyst layer comprising: An additive having a carrier comprising carbon and having an aromatic group on the surface, and A catalyst comprising a carrier, wherein the carrier comprises carbon and carries inorganic fine particles or a metal coordination compound.

8. A catalyst layer comprising: An additive having a carrier containing carbon, wherein the ratio of the amount of water vapor adsorbed at 25°C and a water vapor pressure of 2.2 kPa to the amount of water vapor adsorbed at the same temperature and a water vapor pressure of 3.1 kPa is less than 0.5, and A catalyst comprising a carrier, wherein the carrier comprises carbon and carries inorganic fine particles or a metal coordination compound.

9. The catalyst layer according to claim 7 or 8, wherein the inorganic particles are particles selected from gold, silver, copper, nickel, iron, cobalt, zinc, chromium, palladium, tin, manganese, aluminum, indium, bismuth, molybdenum and carbon nitride; and the metal coordination compound is a metal coordination compound obtained by coordination of a ligand with a metal selected from copper, nickel, iron, cobalt, zinc, manganese, molybdenum and aluminum or an ion of the metal. 10 . The catalyst layer according to claim 7 , wherein the aryl group comprises one or more selected from the group consisting of a phenyl group and a condensed ring group having 2 to 6 benzene rings. 11 . The catalyst layer according to claim 10 , wherein the condensed ring group having 2 to 6 benzene rings comprises one or more selected from the group consisting of naphthyl, anthracenyl, phenanthrenyl and pyrenyl. 12 . The catalyst layer according to claim 7 , wherein the aryl group has one or more substituents selected from the group consisting of an alkyl group, a fluoroalkyl group, a phenyl group, a fluorophenyl group, and a fluorine atom.

13. The catalyst layer according to claim 7, wherein the aryl group is any one or more of the groups shown in (1) to (8), [Chemical formula 2] In (1) to (8), * represents a bonding portion with the surface.

14. A cathode comprising: the catalyst layer according to claim 9, and a gas diffusion layer.

15. An ion exchange membrane-electrode assembly comprising: the cathode according to claim 14, a solid electrolyte, and an anode. 16 . The ion exchange membrane-electrode assembly according to claim 15 , wherein the solid electrolyte is an anion exchange membrane.

17. A solid electrolyte electrolysis device comprising: The cathode according to claim 14, an anode forming a pair of electrodes with the cathode, a solid electrolyte interposed between the cathode and the anode in a contacting state, and A voltage applying unit applies a voltage between the cathode and the anode.

18. The solid electrolyte type electrolysis device according to claim 17, wherein the solid electrolyte is an anion exchange membrane.