Rhenium-tungsten alloy wire, method for producing same, and medical needle

By controlling the atomic concentration ratio of tungsten to rhenium and the content of rhenium in the rhenium-tungsten alloy wire, combined with the doping of potassium, the problem of discoloration of the rhenium-tungsten alloy wire is solved, improving stability and yield, and is suitable for probes and medical needles and other applications.

CN118786256APending Publication Date: 2024-10-15SPECIAL CERAMIC MATERIALS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380024253.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-30
Filing Date
2023-03-30
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

Rhenium-tungsten alloy wire is prone to discoloration during storage, resulting in changes in resistance, reduced friction and increased risk of falling off, affecting yield.

Method used

By maintaining the atomic concentration ratio W/Re of tungsten (W) and rhenium (Re) above 2.5 on the surface of the rhenium-tungsten alloy wire, the formation of rhenium oxide is suppressed, and techniques such as XPS analysis and electrolytic polishing are used to ensure surface uniformity and control Rhenium content is between 2-30% by weight, combined with potassium doping to improve high temperature tensile strength and processability.

Benefits of technology

It effectively suppresses the discoloration of rhenium-tungsten alloy wire, improves long-term storage stability and yield, and ensures the mechanical properties and wear resistance of probes, medical needles and other products.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118786256A_ABST
    Figure CN118786256A_ABST
Patent Text Reader

Abstract

The rhenium-tungsten alloy wire according to an embodiment is a wire comprising a tungsten alloy containing rhenium, and the ratio (W / Re) of the atomic concentration (atomic%) of tungsten (W) to the atomic concentration (atomic%) of rhenium (Re) as determined by XPS analysis in an arbitrary measurement region having a diameter of 50 [mu] m in the wire surface is 2.5 or more. A medical needle according to an embodiment uses a rhenium tungsten alloy wire according to an embodiment.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The embodiments described below relate to a rhenium-tungsten alloy wire, a method for producing the same, and a medical needle. Background Art

[0002] Tungsten alloy (ReW) wire containing a specified amount of rhenium (Re) has improved resistance characteristics and wear resistance compared to ordinary tungsten (W) wire. In addition, the tensile strength in a wide range of temperatures and the ductility after recrystallization are also improved. Therefore, it has been used in semiconductor inspection probes, electron tube heaters, filament materials for earthquake-resistant bulbs, thermocouples, fluorescent display tube filaments, medical needles, etc.

[0003] After the surface mixture layer produced in the manufacturing process is removed by electrolytic polishing, the ReW wire is a white silver color with a metallic luster. As the storage period is extended, the surface changes to, for example, blue, yellow, or magenta. If discoloration occurs, the resistance of the probe may change. For filaments used in display tubes, the uniformity of the coating (electrodeposition surface treatment) of the oxide used to release hot electrons disappears. For medical needles, quality degradation and impurities such as changes in the friction of the discolored part and the risk of the discolored part falling off become problems.

[0004] Therefore, the discolored part cannot be used and needs additional treatment such as re-electrolysis. Furthermore, the additional treatment changes the size of the wire, and the resistance and strength change, so it becomes unusable and the yield rate decreases. Therefore, after the electrolysis process, for example, the wire is fully dried, and the wound wire reel is sealed and packaged under reduced pressure and stored in a manner isolated from the external environment. However, there are differences in the occurrence of discoloration in ReW wires stored in the same manner.

[0005] Prior art literature

[0006] Patent Literature

[0007] Patent Document 1: Japanese Patent Application Laid-Open No. 4-308003

[0008] Patent Document 2: Japanese Patent Application Publication No. 2021-95585

[0009] Non-patent literature

[0010] Non-patent literature 1: Saburo Nagakura and five others, "Iwanami Physical and Chemical Dictionary 5th Edition", Iwanami Shoten, February 1998, p. 541 Summary of the invention

[0011] Problems to be solved by the invention

[0012] An object of the present invention is to provide a ReW wire that can be easily stored for a long period of time by suppressing discoloration.

[0013] Means for solving problems

[0014] In order to solve the above-mentioned problems, the rhenium tungsten alloy wire involved in the embodiment is a wire composed of a tungsten alloy containing rhenium, and in any measurement area with a unit area of ​​50 μm in diameter on the surface of the wire, the ratio W / Re of the atomic concentration (atomic %) of tungsten (W) to the atomic concentration (atomic %) of rhenium (Re) based on XPS analysis is greater than 2.5. BRIEF DESCRIPTION OF THE DRAWINGS

[0015] Figure 1 The figure is an example of the analysis results of the sample with discoloration and the sample without discoloration by X-ray photoelectron spectroscopy (XPS).

[0016] Figure 2 is a graph showing the color change of the ReW line and its reflection spectrum.

[0017] Figure 3 This is the state diagram of the Re-W binary system.

[0018] Figure 4a These are the results of EDS (energy dispersive X-ray spectrometry) analysis of the sample cross section before the surface mixture layer is removed.

[0019] Figure 4b The results of EDS analysis of a cross section of the sample before the surface mixture layer was removed.

[0020] Figure 4c The results of EDS analysis of a cross section of the sample before the surface mixture layer was removed.

[0021] Figure 5a is the potential-pH diagram of tungsten (W).

[0022] Figure 5b This is the potential-pH diagram of rhenium (Re).

[0023] Figure 6 It is an illustration of particle size distribution. DETAILED DESCRIPTION

[0024] Hereinafter, the rhenium tungsten alloy wire of the embodiment will be described with reference to the drawings. Hereinafter, the rhenium tungsten alloy wire may also be referred to as ReW wire. It should be noted that the drawings are schematic, and for example, the ratio of the dimensions of each part is not limited to the drawings.

[0025] The rhenium tungsten alloy wire involved in the embodiment is a wire composed of a tungsten alloy containing rhenium, and in an arbitrary measurement area with a unit area of ​​50 μm in diameter on the surface of the wire, the ratio W / Re of the atomic concentration (atomic %) of tungsten (W) to the atomic concentration (atomic %) of rhenium (Re) based on XPS analysis is greater than 2.5.

[0026] Among rhenium oxides, Re2O5, also known as rhenium pentoxide, is a blue compound. ReO3, also known as rhenium trioxide, is a red cubic crystal with a metallic luster. Re2O7, also known as rhenium heptoxide, is a yellow orthorhombic crystal (Non-Patent Document 1). Thus, rhenium oxides have colors, and the colors change depending on the type of oxide. As a result of repeated and in-depth studies, the following understanding was obtained: the color change of the ReW line is caused by rhenium oxide.

[0027] exist Figure 1 An example of the results of analyzing a sample (A) with discoloration and a sample (B) without discoloration by X-ray photoelectron spectroscopy (XPS) in a 26 wt% Re-W line of φ0.152 mm after electrolytic polishing to give it a metallic luster and storing it for a certain period of time is shown in the figure. The device used was Quantera SXM manufactured by PHI, the X-ray source was single crystal spectroscopic A1Kα rays, the X-ray output power was 12.5 W, and the analysis range was φ50 μm.

[0028] More W-Metal and tungsten oxide were detected in B (sample without discoloration) than in A (sample with discoloration), and more rhenium oxide was detected in A than in B. The results of the ratio W / Re of the atomic concentration of tungsten (W) and the atomic concentration of rhenium (Re) based on XPS semi-quantitative analysis of the same part are shown in Table 1. In the discolored sample, the presence ratio of rhenium is large, so rhenium oxide is easily generated. Table 1a shows the composition of the measurement range of the discolored sample (A) and the non-discolored sample (B). It can be seen from Table 1a that the surface of the ReW line is composed of C, N, O, W and Re. Therefore, it can be said that the surface of the ReW line can contain C, N, O, W and Re. The content of C, N, and O in the non-discolored sample (B) is roughly equal to the content of C, N, and O in the discolored sample (A). In addition, the W content in the sample (B) without discoloration is larger than that in the sample (A) with discoloration, and the Re content in the sample (B) without discoloration is smaller than that in the sample (A) with discoloration.

[0029] [Table 1]

[0030]

[0031] [Table 1a]

[0032] Composition (atomic %) C N O W Re total W / Re Sample A with color change 50.0 2.9 35.8 5.2 6.1 100.0 0.9 No discoloration sample B 47.0 4.1 35.7 10.7 2.5 100.0 4.3

[0033] exist Figure 2 The color change of the ReW line and its reflection spectrum are shown in FIG. The color change shows the color of the rhenium oxide mentioned above (blue, purple (red and blue), and yellow). As for the reflection spectrum of each color change part, a spectroscopic system is assembled in a microscope, and a microscopic spectroscopic system (DF-1037 manufactured by Techno Synthetic) capable of spectroscopic measurement of micro points is used to measure under the conditions of a measurement point of about φ10μm, an exposure time of 10ms, and an accumulation number of 200 times.

[0034] For the visible light wavelength of 400nm to 700nm, if it is white silver (metallic color) without discoloration, the difference between the maximum and minimum values ​​of the reflectance is less than 5%. On the other hand, the reflectance of the discolored part changes, and changes to a spectrum with a peak that differs from the minimum value by more than 5% in the wavelength portion corresponding to each color. Therefore, the discolored part is judged based on whether the difference between the maximum and minimum values ​​of the reflectance in the wavelength of 400nm to 700nm of the visual or reflection spectrum exceeds 5%. Figure 2 The difference between the maximum value and the minimum value of the reflectance of the reflection spectrum for judging the color change portion is noted in the figure.

[0035] The main reason for the increase in the abundance ratio of rhenium (Re) on the surface is the deviation in the material of the element wire. Figure 3 The binary phase diagram of Re-W is shown in . For example, as a method for producing Re-W, a powder metallurgy method of mixing tungsten (W) powder and rhenium (Re) powder, molding them, and sintering them is generally adopted.

[0036] The sintering of Re-W progresses through solid phase diffusion, so depending on the particle size distribution of each powder, the mixing state of the powder, or the molding and sintering conditions, it is impossible to diffuse and homogenize (solid solution) rhenium in the tungsten matrix. As a result, a phase region (segregation phase of σ phase) with a locally high composition ratio of rhenium is generated. By its presence on the surface, the existence ratio of rhenium on the surface becomes larger.

[0037] In addition, since the surface removal treatment of the ReW wire after the wire drawing process, such as electrolytic polishing, is insufficient, a layer with unstable composition remains on the surface of the ReW wire, and the presence ratio of rhenium may increase. Figure 4a , Figure 4b and Figure 4c 2 shows the results of EDS (energy dispersive X-ray spectrometry) analysis of the sample cross section before the surface mixture layer is removed. Figure 4a This is an image showing a secondary electron image of a sample cross section based on EDS. Figure 4a The arrow in the figure indicates the surface mixture layer. Figure 4a As shown, the thickness of the surface mixture layer is not uniform and fluctuates. Figure 4bFigure 2 is an image showing the W element mapping based on EDS of the sample cross section. Figure 4b As shown, there is a portion with low tungsten concentration in the surface mixture layer ( Figure 4b In addition, Figure 4c Figure 2 is an image showing the Re element mapping based on EDS of the sample cross section. Figure 4c As shown, there is a portion with a high rhenium concentration in the surface mixture layer ( Figure 4c The above analysis results show that there is a portion with a high rhenium concentration in the surface mixture layer. In addition, the thickness of the surface mixture layer varies depending on the location. When the surface removal amount is insufficient, the surface mixture layer partially remains, and therefore, the presence ratio of rhenium may become larger.

[0038] In addition, when electrolytic polishing is used for surface treatment, depending on the conditions of electrolysis, tungsten may be preferentially dissolved, and the presence ratio of rhenium may increase. Figure 5a and Figure 5b The potential-pH diagram of tungsten (W) and rhenium (Re) is shown in FIG. Figure 5a is the potential-pH diagram of tungsten (W). Figure 5b is the potential-pH diagram of rhenium (Re). Figure 5a and Figure 5b In the figure, the horizontal axis represents pH and the vertical axis represents potential (V). Since tungsten is easily dissolved, tungsten is easily dissolved preferentially when the electrolysis rate is slow or the electrolysis potential is low. Therefore, the existence ratio of rhenium on the surface may become larger.

[0039] For the ReW line of the embodiment, surface polishing is performed, and semi-quantitative analysis is performed by XPS analysis. For example, chemical polishing such as electrolytic polishing can be performed. For XPS analysis, for example, QuanteraSXM manufactured by PHI is used, the X-ray source is single crystal spectroscopic A1Kα ray, the X-ray output power is 12.5W, and the analysis range is set to φ50μm.

[0040] In the ReW wire of the embodiment, in any measurement area, the ratio W / Re of the atomic concentration (atomic %) of tungsten (W) to the atomic concentration (atomic %) of rhenium (Re) based on XPS analysis is 2.5 or more. By setting the ratio W / Re of the atomic concentration of tungsten to rhenium in the surface to 2.5 or more, the formation of rhenium oxide can be suppressed. Furthermore, when the ReW wire of the embodiment is used as a raw material to manufacture a probe or a medical needle, discoloration is suppressed and it can be manufactured with a high yield. The value of the ratio W / Re can be adjusted by, for example, using at least one of the particle size of the raw material tungsten powder, the particle size of the raw material rhenium powder, the sintering temperature during manufacturing, and the polishing speed of electrolytic polishing, or a combination of multiple ones.

[0041] The content of rhenium contained in the ReW wire of the embodiment is, for example, 2% by weight or more and less than 30% by weight. In addition, the content of rhenium contained in the ReW wire of the embodiment is, for example, preferably 10% by weight or more and 28% by weight or less. The content of rhenium is a value analyzed by inductively coupled plasma-optical emission spectrometry (ICP-OES). Rhenium improves the elongation of tungsten at high temperatures and improves processability. In addition, strength is improved by solid solution strengthening.

[0042] When the rhenium content is less than 2% by weight, the effect is not sufficient. For example, when using a ReW wire with a rhenium content of less than 2% by weight as a raw material for a probe, the deformation of the completed probe increases with the frequency of use, resulting in poor contact and reduced semiconductor inspection accuracy. If the rhenium content becomes more than 30% by weight, it exceeds the solid solubility limit with tungsten, so it is impossible to diffuse and homogenize (solid dissolve) rhenium in the tungsten matrix. As a result, it is possible to produce a phase region with a locally high rhenium composition ratio (segregation phase of the σ phase), partially reducing W / Re. When such a part appears on the surface, it is easy to discolor.

[0043] When ReW wire having a rhenium content of 2 wt% or more and less than 30 wt% is used as a raw material to manufacture a probe or a medical needle, discoloration can be suppressed, and high yield can be achieved. In addition, the mechanical properties (strength, wear resistance) of the manufactured probe or medical needle can be ensured. The rhenium content is preferably 10 wt% or more and 28 wt% or less, for example.

[0044] The ReW wire of the embodiment may contain potassium (K) of more than 30 wtppm and less than 90 wtppm as a doping material. The potassium content is a value analyzed by inductively coupled plasma optical emission spectrometry (ICP-OES). By containing potassium, the tensile strength and creep strength at high temperatures are improved by utilizing the doping effect. When the potassium content is less than 30 wtppm, the doping effect becomes insufficient. If the potassium content exceeds 90 wtppm, the processability is reduced, and the yield may be greatly reduced. By containing potassium of more than 30 wtppm and less than 90 wtppm as a dopant, for example, it is possible to produce thin wires for thermocouples and electron tube heaters using the ReW wire of the embodiment as a raw material with a high yield while ensuring high temperature characteristics (preventing wire breakage and deformation during high temperature use).

[0045] The ReW wire of the embodiment has a diameter of, for example, 0.1 mm or more and 1.00 mm or less.

[0046] The ReW wire of this embodiment suppresses surface discoloration, greatly contributing to long-term storage and improved yield. In addition, the ReW wire of the embodiment can be applied to medical needles. In addition, it can also be applied to ReW wire applications for thermocouples and probes.

[0047] Next, a method for producing the ReW wire according to the embodiment will be described. The production method is not particularly limited, and examples thereof include the following methods.

[0048] The tungsten powder and the rhenium powder are mixed so that the rhenium content is 2% by weight or more and less than 30% by weight. There is no particular limitation on the mixing method, but a method of mixing the powders in a slurry state using water or an alcohol solution is particularly preferred in order to obtain a powder with good dispersibility. In addition, in order to ensure the homogeneity of the powder batch, it is more preferred to dry-mix the same powder batch after drying the slurry.

[0049] The mixed rhenium powder preferably has an average particle size of less than 8 μm. The particle size distribution preferably has an SD value of less than 11 μm. Figure 6 An explanatory diagram of the particle size distribution is shown in . The horizontal axis is the particle size (μm), the left vertical axis is the frequency (%), and the right vertical axis is the cumulative (%). The SD value is the value obtained by SD = (d(84%) - d(16%)) / 2 when d(84%) is set as the cumulative particle size of 84% and d(16%) is set as the cumulative particle size of 16%, and becomes an indicator of the distribution width of the measured particle size. In addition, the particle size distribution is measured by the laser diffraction method. As for the amount of powder used in one measurement, it is set to be carried out with the amount recommended by the measuring device. Generally, 0.02g is recommended. In addition, the measurement sample is set to be fully stirred before measurement and then measured.

[0050] The tungsten powder is pure tungsten powder except for inevitable impurities or doped tungsten powder containing potassium (K) in an amount that takes into account the yield of the wire. The tungsten powder preferably has an average particle size of less than 16 μm and a particle size distribution SD value of less than 13 μm.

[0051] When the average particle size of the rhenium powder is 8 μm or more, when the SD value of the rhenium powder is 11 μm or more, when the average particle size of the tungsten powder is 16 μm or more, or when the SD value of the tungsten powder is 13 μm or more, the diffusion distance of the rhenium atoms or tungsten atoms used to diffuse and homogenize (solid solution) rhenium in the tungsten matrix is ​​increased, and the σ phase is easily generated.

[0052] The ratio of the average particle size of the rhenium powder to the average particle size of the tungsten powder (Re average particle size / W average particle size) is preferably 0.4 or more and 2.0 or less. When the ratio of the average particle size of the rhenium powder to the average particle size of the tungsten powder is less than 0.4 or exceeds 2.0, the diffusion distance of the rhenium atoms to the center of the tungsten particles or the diffusion distance of the tungsten atoms to the center of the rhenium particles becomes longer, and there is a possibility that the σ phase is easily generated.

[0053] Next, the mixed powder is placed in a specified mold for compression molding. The compression pressure at this time is preferably 150 MPa or more. For the molded body, in order to facilitate handling, a pre-sintering treatment can be performed in a hydrogen furnace at 1200-1400°C. The obtained molded body is sintered in a hydrogen atmosphere, or in an inert gas atmosphere such as argon, or in a vacuum. The sintering temperature is preferably above 2500°C. When the sintering temperature is less than 2500°C, the diffusion of rhenium atoms and tungsten atoms is not fully carried out during sintering. The upper limit of the sintering temperature is 3400°C (the melting point of tungsten is below 3422°C).

[0054] The relative density of the sintered body (relative density (%) relative to the true density = [sintered body density / true density] × 100%) is preferably 90% or more. In addition, in one sintered body, for example, the ratio of the density of the lowest part such as the lower end during the current sintering to the average density of the entire sintered body is preferably 0.98 or more. By making the relative density of the sintered body 90% or more and making the ratio of the density of the lowest part relative to the average density of the entire sintered body 0.98 or more, the fluctuation of the rhenium content can be suppressed.

[0055] The sintered body obtained in the main sintering step is subjected to a first swaging process. The first swaging process is preferably performed at a heating temperature of 1300 to 1600° C. The reduction rate of the cross-sectional area (reduction rate) by the first heating treatment (first heating) is preferably 5 to 15%.

[0056] Rolling may be performed instead of the first rotary forging process. The rolling process is preferably performed at a heating temperature of 1200 to 1600°C. The surface reduction rate in the first heating is preferably 40 to 75%. As a rolling mill, a double-roll rolling mill, a four-roll rolling mill, a die roll rolling mill, etc. can be used. The manufacturing efficiency can be greatly improved by rolling. The first rotary forging (SW) process can be combined with the rolling process.

[0057] The sintered body (ReW rod) that has been subjected to the first rotary swaging, rolling, or a combination of the first rotary swaging and rolling is subjected to the second rotary swaging (SW) process. The second rotary swaging process is preferably performed at a heating temperature of 1200 to 1500° C. The area reduction rate in the first heating (first heating) is preferably about 5 to 20%.

[0058] The ReW rod that has completed the second rotary forging step is then subjected to a recrystallization treatment, which can be performed, for example, using a high-frequency heating device in a hydrogen atmosphere, an inert gas atmosphere such as argon, or a vacuum, at a treatment temperature in the range of 1800 to 2600°C.

[0059] The third rotary forging process is performed on the ReW rod that has completed the recrystallization treatment. The third rotary forging process is preferably performed at a heating temperature of 1200 to 1500°C. The surface reduction rate in the first heating is preferably about 10 to 30%. The third rotary forging process is performed until the ReW rod has a diameter that can be processed by wire drawing (preferably a diameter of 2 to 4 mm).

[0060] For the ReW rod material that has completed the third rotary forging process, a lubricant is applied to the surface and dried to smoothly perform the wire drawing (DW: drawing) process. For the wire drawing process, the lubricant is applied, the lubricant is dried, the process of heating to a processable temperature, and the process of drawing using a drawing die is repeated. For the lubricant, a carbon (C)-based lubricant with excellent heat resistance is preferably used.

[0061] The processing temperature is set according to the wire diameter of the wire drawing process. The processing temperature is preferably below 1100°C, for example. The surface reduction rate of each die is preferably 10 to 35%. In the middle of the wire drawing process, an annealing process and a surface grinding process (such as an electrolytic process) can be added under known conditions as needed.

[0062] The ReW wire that has completed the wire drawing process is ground. For example, the grinding process includes electrochemical grinding (electrolytic grinding) in a sodium hydroxide aqueous solution with a concentration of 3 to 15% by weight. The surface reduction rate in the grinding process is preferably 10 to 25%. In the case of less than 10%, it may not be possible to remove the mixture of the unevenness on the material surface generated in the rotary forging process and the wire drawing process and the unevenness attached to the material surface. In the case of insufficient surface removal, the mixture layer remains locally, so the presence ratio of rhenium may increase. If it exceeds 25%, the material yield deteriorates.

[0063] In the case of electrolytic polishing, the polishing speed is preferably 0.5 to 3.0 μm / sec. If it is slower than 0.5 μm / sec, tungsten on the surface may be preferentially dissolved, and the presence ratio of rhenium on the surface may increase. If it exceeds 3.0 μm / sec, the amount of electrolysis per unit time may increase, resulting in rapid electrolysis, and the correction of the cross-sectional shape of the ReW line may become insufficient.

[0064] For the ReW wire that has completed the grinding process, for example, a drying process can be performed. The drying process is performed, for example, using a vacuum dryer with the temperature inside the box set to a range of 50 to 80°C. The drying time is, for example, more than 1 hour. Then, a prescribed delivery inspection is performed. When storing the ReW wire after vacuum drying, for example, by placing it in a moisture-proof storage box with a relative humidity of less than 5%, it is possible to prevent the adsorption of moisture. For example, except for the case of performing characteristic and quantity inspections, the ReW wire is placed in the moisture-proof storage box and stored.

[0065] The ReW wire is wound on a reel for delivery, for example, while undergoing a delivery inspection. For the ReW wire that has completed the delivery inspection, for example, the outermost surface of the reel for delivery is covered with a protective paper and fixed with a rubber band, etc. Then, for example, it is stored in an aluminum bag, degassed, and sealed.

[0066] By using an appropriate amount of the ReW wire obtained in the above-mentioned steps and carrying out necessary steps under known conditions, a probe or medical needle having a predetermined wire diameter and necessary properties (strength, hardness, etc.) can be obtained.

[0067] (Example 1)

[0068] A doped tungsten powder having an average particle size of 13 μm and an SD value of 12 μm and a rhenium powder having an average particle size of 6 μm and an SD value of 7 μm, containing potassium (K) in an amount of 50 to 80 wt ppm in the final wire, was mixed in a slurry state using an alcohol solution so that the rhenium content was 10 wt %. The obtained slurry was dried to obtain a raw material powder.

[0069] The mixed powder of the raw materials is pressed into a molded body. The molded body is subjected to a pre-sintering treatment at 1300°C in a hydrogen furnace. The molded body is sintered at 3000°C in a hydrogen atmosphere to obtain a sintered body. The sintered body is subjected to a first rotary forging process by heating to a temperature of 1400°C and a reduction rate of 14% in the cross-sectional area processed by a single heat treatment. The sintered body subjected to the first rotary forging process is subjected to a second rotary forging process by heating to a temperature of 1300°C and a reduction rate of 15% in the cross-sectional area processed by a single heat treatment.

[0070] The ReW rod that had completed the second rotary forging process was subjected to recrystallization treatment in a hydrogen atmosphere at a treatment temperature of 2400° C. After the recrystallization treatment, the third rotary forging process was performed at a heating temperature of 1300° C. and a cross-sectional area reduction rate of 13% by the first heating treatment process, thereby obtaining a rod having a diameter of 2.5 mm.

[0071] A lubricant is applied to the surface of the rod material subjected to the third rotary forging process and dried. The obtained rod material is subjected to wire drawing. The wire drawing process is performed at 1000°C so that the reduction rate of the cross-sectional area in the first drawing process becomes 10% to 35%. During the wire drawing process, an annealing process is performed at 1300°C.

[0072] The ReW wire that had been drawn was electropolished in an aqueous sodium hydroxide solution with a concentration of 8 wt%. The electropolishing process was performed with a cross-sectional area reduction rate of 15 to 20% and a polishing rate of 2.2 μm / sec. The diameter of the obtained ReW wire was 0.8 mm.

[0073] For the electrolytically polished ReW, a vacuum dryer with an internal temperature of 70°C was used for a 2-hour drying process. The obtained ReW wire was wound on a 100m / reel shipping reel, the outermost surface was covered with protective paper, and fixed with a rubber band. The shipping reel on which the ReW wire was wound was placed in an aluminum bag together with a desiccant containing silica gel, and the aluminum bag was degassed and sealed.

[0074] Three rolls were made for the same roll, and the three roll samples were placed on a 1m high platform in a room with a humidity of less than 60% and a room temperature of less than 30°C and stored side by side for 8 months. Figure 2 The presence or absence of color change was confirmed by the difference between the maximum value and the minimum value of the reflectance in the wavelength range of 400 nm to 700 nm in the reflectance spectrum described above.

[0075] (Example 2)

[0076] The ReW wire was manufactured in the same manner as in Example 1 except that the raw material tungsten powder was not doped with potassium, the ratio of rhenium was 26% by weight, and the wire diameter of the final ReW wire was 0.15 mm, and was wound on a 500 m / reel shipping reel, and stored in an aluminum bag together with a desiccant using the same packaging method as in Example 1. As in Example 1, three reels were manufactured for the same reel, and the reels were stored for 8 months using the same method as in Example 1. After 8 months, the presence or absence of discoloration was confirmed.

[0077] (Comparative Example 1)

[0078] Using the same raw material powder as in Example 1, the same steps as in Example 1 are carried out until the wire drawing process to manufacture ReW wire. For the obtained ReW wire, an electrolytic grinding process is carried out at a grinding speed of 0.4 μm / second to obtain a ReW wire with a wire diameter of 0.8 mm. The obtained ReW wire is wound on a shipping reel of 100 m / reel, the outermost surface is covered with protective paper, and fixed with a rubber band. The shipping reel wound with the ReW wire is placed in an aluminum bag together with a desiccant containing silica gel, and the aluminum bag is degassed and sealed. For the same reel, 3 reels are made and stored for 8 months using the same method as in Example 1. After 8 months, the presence or absence of discoloration is confirmed.

[0079] (Comparative Example 2)

[0080] The same raw material powder as in Example 2 was used, and the same steps as in Example 2 were performed until the wire drawing process to manufacture a ReW wire. The obtained ReW wire was subjected to an electrolytic grinding process at a grinding speed of 0.4 μm / second to obtain a ReW wire with a wire diameter of 0.15 mm. The obtained ReW wire was wound on a 500 m / reel shipping reel and packaged in the same manner as in Comparative Example 1. Three reels were made for the same reel and stored for 8 months in the same manner as in Example 1. After 8 months, the presence or absence of discoloration was confirmed.

[0081] Table 2 shows the measurement results of rhenium content, potassium content and W / Re. The analysis of rhenium content and potassium content was carried out by inductively coupled plasma optical emission spectrometry (ICP-OES). In addition, the lower detection limit of potassium is 5 wtppm, and the case where there is no addition and the analysis value is less than 5 wtppm is recorded as "-". W / Re is obtained by XPS analysis. For XPS analysis, Quantera SXM manufactured by PHI was used, the X-ray source was single crystal spectrometry A1Kα ray, the X-ray output power was 12.5W, and the analysis range was φ50μm.

[0082] [Table 2]

[0083]

[0084] As can be seen from Table 2, the ReW wire according to the embodiment can suppress discoloration even during long-term storage, and can significantly improve the yield rate in medical needle processing. In the ReW wires of Comparative Examples 1 and 2, the electrolytic polishing speed is slow, so the presence ratio of rhenium on the surface becomes large, and the W / Re ratio is less than 2.5.

[0085] Several embodiments of the present invention are illustrated above, but these embodiments are presented as examples and are not intended to limit the scope of the invention. These new embodiments can be implemented in various other forms, and various omissions, substitutions, changes, etc. can be made without departing from the scope of the main purpose of the invention. The modified examples of these embodiments are included in the scope and main purpose of the invention, and are also included in the invention recorded in the patent claims and the scope equivalent thereto. In addition, the above-mentioned embodiments can be implemented in combination with each other.

[0086] The invention according to the embodiment will be described below.

[0087] <1> Rhenium tungsten alloy wire is a wire composed of a tungsten alloy containing rhenium, wherein in an arbitrary measurement area with a unit area of ​​50 μm in diameter on the surface of the wire, the ratio W / Re of the atomic concentration (atomic %) of tungsten (W) to the atomic concentration (atomic %) of rhenium (Re) based on XPS analysis is 2.5 or more.

[0088] <2> The rhenium tungsten alloy wire according to <1>, wherein a content of the rhenium is 2% by weight or more and less than 30% by weight.

[0089] <3> The rhenium tungsten alloy wire according to <1>, wherein a content of the rhenium is 10 wt % or more and 28 wt % or less.

[0090] <4> The rhenium tungsten alloy wire according to any one of <1> to <3>, wherein a potassium (K) content is 30 wtppm or more and 90 wtppm or less.

[0091] <5> The rhenium tungsten alloy wire according to any one of <1> to <4>, wherein the diameter is 0.1 mm or more and 1.00 mm or less.

[0092] <6> The rhenium tungsten alloy wire according to any one of <1> to <5>, which is used as a wire material for a medical needle.

[0093] <7> The method for producing a rhenium-tungsten alloy wire according to any one of <1> to <6>.

[0094] <8> A medical needle using the rhenium tungsten alloy wire according to any one of <1> to <6>.

[0095] Description of Reference Numerals

[0096] A…Sample with color change

[0097] B…Sample without discoloration

Claims

1. Rhenium tungsten alloy wire is a wire composed of a tungsten alloy containing rhenium, wherein in any measurement area with a unit area of ​​50 μm in diameter on the surface of the wire, the ratio W / Re of the atomic concentration (atomic %) of tungsten (W) to the atomic concentration (atomic %) of rhenium (Re) based on XPS analysis is 2.5 or more.

2. The rhenium-tungsten alloy wire according to claim 1, wherein: The rhenium content is 2% by weight or more and less than 30% by weight.

3. The rhenium-tungsten alloy wire according to claim 1, wherein: The rhenium content is 10 wt % or more and 28 wt % or less.

4. The rhenium-tungsten alloy wire according to claim 1, wherein: The potassium (K) content is 30 wt ppm or more and 90 wt ppm or less. The rhenium-tungsten alloy wire according to claim 1 , having a diameter of 0.1 mm or more and 1.00 mm or less. The rhenium tungsten alloy wire according to any one of claims 1 to 5, which is used as a wire material for a medical needle. 7 . The method for producing the rhenium-tungsten alloy wire according to claim 1 . 8 . A medical needle using the rhenium tungsten alloy wire according to claim 1 .