Magnesium alloy insert, preparation method thereof and electronic equipment

By preparing aluminum coating on the surface of magnesium alloy inserts and die-casting to form magnesium alloy inserts, the problem of poor performance after magnesium alloys are embedded in high-strength materials is solved, the interface bonding force between magnesium alloy and insert materials is improved, and the overall The mechanical properties and surface treatment capabilities meet the requirements for lightweight, high strength and high stiffness of magnesium alloy inserts.

CN118788951APending Publication Date: 2024-10-18GOERTEK INC
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410831154.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-25
Publication Date
2024-10-18

AI Technical Summary

Technical Problem

After magnesium alloys are embedded in high-strength materials, their performance is poor, especially in application scenarios that meet high strength, high stiffness and high-gloss surface treatment. Excessive interface stress leads to interface cracks and galvanic corrosion problems.

Method used

An aluminum coating is prepared on the surface of the insert to be processed, and the aluminum powder particles are sprayed to form a dense aluminum coating through plasma cold spraying technology, and the preliminary processing insert is die-cast into the magnesium alloy matrix to embed the aluminum coating into the magnesium alloy matrix to form Magnesium alloy inserts improve the interface bonding force between magnesium alloy and insert materials to avoid interface cracks and galvanic corrosion.

Benefits of technology

It improves the performance of magnesium alloy and high-strength material inserts, enhances the overall mechanical properties and surface treatment capabilities, solves component failure and galvanic corrosion problems caused by excessive interface stress, and achieves lightweight magnesium alloy inserts , high strength and high stiffness requirements.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118788951A_ABST
    Figure CN118788951A_ABST
Patent Text Reader

Abstract

The invention discloses a magnesium alloy insert, a preparation method of the magnesium alloy insert and electronic equipment, and belongs to the technical field of material machining forming. The method comprises the steps that an aluminum coating is prepared on a preset surface area of a to-be-machined insert, a primarily-machined insert is obtained, and the to-be-machined insert is made of stainless steel and titanium alloy; and the primarily-machined insert is die-cast into the magnesium alloy base body, the aluminum coating is embedded into the magnesium alloy base body, and the magnesium alloy insert is obtained. The technical effect that the using performance of the magnesium alloy embedded with the high-strength material is improved is achieved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of material processing and forming, and in particular to a magnesium alloy insert and a preparation method thereof, and an electronic device. Background Art

[0002] In recent years, the rapid development of consumer electronic product technology has put forward higher and higher requirements on the structural materials and component performance of electronic devices. In order to adapt to the trend of electronic devices being thin and small, the shell materials of electronic devices need to have a series of characteristics, such as low density, high strength and stiffness, excellent impact resistance and vibration reduction performance, strong electromagnetic shielding ability, good heat dissipation performance, easy forming and processing, beautiful surface, durability, low cost, easy recycling and environmental protection. Traditional plastics and aluminum materials are gradually unable to meet these requirements. However, magnesium and its alloys, as ideal materials for manufacturing electronic device shells, have shown broad application prospects. Magnesium and its alloy materials have many advantages, including low density, light weight, high strength and stiffness, excellent impact resistance and vibration reduction performance, and good electromagnetic shielding ability and heat dissipation performance. However, it is undeniable that magnesium alloy materials also face some disadvantages in use. For example, for some mechanical structural parts such as brackets, thin-walled support parts and other product parts, it is difficult for magnesium alloys to have advantages in application scenarios where the design requirements meet high strength, high stiffness and high-gloss surface treatment.

[0003] In order to meet the requirements of lightweight and high strength / rigidity performance of structural parts, high-strength materials are added to magnesium alloys. Although magnesium alloys embedded with high-strength materials can improve their strength, they still have poor performance. Summary of the invention

[0004] The main purpose of the present application is to provide a magnesium alloy insert and a preparation method thereof, and an electronic device, aiming to solve the technical problem of poor performance after high-strength materials are embedded in magnesium alloys.

[0005] To achieve the above object, the present application provides a method for preparing a magnesium alloy insert, the method comprising:

[0006] Prepare an aluminum coating on a preset surface area of ​​an insert to be processed to obtain a pre-processed insert, wherein the material of the insert to be processed includes stainless steel and titanium alloy;

[0007] The pre-machined insert is die-casted into a magnesium alloy substrate, and the aluminum coating is embedded in the magnesium alloy substrate to obtain a magnesium alloy insert.

[0008] In one embodiment, the step of preparing an aluminum coating on a predetermined surface area of ​​the insert to be processed comprises:

[0009] Placing the insert to be processed in the spraying direction of the plasma cold spraying equipment;

[0010] Aluminum powder particles are sprayed onto the preset surface area by spraying carrier gas, so as to form an aluminum coating on the preset surface area.

[0011] In one embodiment, the aluminum powder particles are prepared by ion atomization method;

[0012] And / or, the diameter of the aluminum powder particles is 0.5 μm-20 μm;

[0013] And / or, the aluminum powder particles are dried at 80° C.-120° C. for 10 min-20 min before spraying.

[0014] In one embodiment, the spray carrier gas is high-pressure nitrogen;

[0015] and / or, the carrier gas temperature of the spray carrier gas is 120° C.-250° C.;

[0016] And / or, the carrier gas pressure of the spraying carrier gas is 0.8MPa-2.0MPa.

[0017] In one embodiment, the spraying distance of the spray carrier gas is 10 mm-30 mm;

[0018] The feeding rate of the aluminum powder particles is 0.6 g / s-2.0 g / s.

[0019] In one embodiment, the thickness of the aluminum coating is 10 μm-60 μm;

[0020] And / or, the aluminum coating is a fine-grained aluminum coating with a grain size of 0.1 μm-20 μm.

[0021] In one embodiment, before the step of preparing an aluminum coating on a predetermined surface area of ​​the insert to be processed to obtain a pre-processed insert, the step further includes:

[0022] Prepare materials to be processed;

[0023] The material to be processed is processed according to a preset shape to obtain the insert to be processed, and the processing includes at least one of CNC machine tool processing, forging, casting, rolling and extrusion.

[0024] In one embodiment, after the step of die-casting the pre-machined insert into a magnesium alloy substrate and embedding the aluminum coating into the magnesium alloy substrate to obtain a magnesium alloy insert, the step further includes:

[0025] performing sandblasting, passivation and spraying treatments on the magnesium alloy part of the magnesium alloy insert;

[0026] The magnesium alloy portion is masked, and the insert portion of the magnesium alloy insert is polished.

[0027] In addition, to achieve the above-mentioned purpose, the present application also provides a magnesium alloy insert, which is prepared by the method for preparing the magnesium alloy insert as described above.

[0028] In addition, to achieve the above-mentioned purpose, the present application also provides an electronic device, which includes the magnesium alloy insert as described above.

[0029] The present application provides a magnesium alloy insert and a preparation method thereof, and an electronic device. An aluminum coating is prepared on a preset surface area of ​​the insert to be processed to obtain a preliminary processed insert, and the material of the insert to be processed includes stainless steel and titanium alloy; the preliminary processed insert is die-cast into a magnesium alloy matrix, and the aluminum coating is embedded in the magnesium alloy matrix to obtain a magnesium alloy insert. By preparing an aluminum coating on the surface of the insert to be processed, the aluminum coating can serve as a transition between the magnesium alloy and the insert material after the magnesium alloy insert is formed by die-casting. The physical and chemical properties of magnesium alloy and aluminum are similar. Compared with the direct die-casting method, the interface bonding force between the magnesium alloy matrix and the insert material is improved, and the problem of interface cracks caused by excessive interface stress leading to component failure can be avoided, thereby improving the performance of magnesium alloy and high-strength material inserts. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] In order to more clearly illustrate the embodiments of the present drawings or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present drawings. For ordinary technicians in this field, other drawings can be obtained based on the structures shown in these drawings without paying any creative work.

[0031] Figure 1 This is a schematic diagram of the structure of the stainless steel insert in Example 1 of the present application;

[0032] Figure 2 This is a schematic structural diagram of a magnesium alloy substrate in Example 1 of the present application;

[0033] Figure 3 This is a schematic diagram of the structure of the magnesium alloy insert in Example 1 of the present application.

[0034] Description of Figure Numbers:

[0035] 100, stainless steel insert; 200, magnesium alloy substrate; 300, magnesium alloy insert.

[0036] The realization of the purpose, functional features and advantages of this application will be further explained in conjunction with embodiments and with reference to the accompanying drawings. DETAILED DESCRIPTION

[0037] It should be understood that the specific embodiments described herein are only used to explain the present application and are not used to limit the present application.

[0038] Hereinafter, the magnesium alloy insert and its preparation method, and the implementation mode of the electronic device of the present application are specifically disclosed with appropriate reference to the drawings. However, there may be cases where unnecessary detailed descriptions are omitted. For example, there are cases where detailed descriptions of well-known matters and repeated descriptions of actually the same structure are omitted. This is to avoid the following description from becoming unnecessarily lengthy and to facilitate the understanding of those skilled in the art. In addition, the drawings and the following descriptions are provided for those skilled in the art to fully understand the present application, and are not intended to limit the subject matter described in the claims.

[0039] "Scope" disclosed in the present application is limited in the form of lower limit and upper limit, and a given range is limited by selecting a lower limit and an upper limit, and the selected lower limit and upper limit define the boundary of a special range. The scope limited in this way can be including end values ​​or not including end values, and can be arbitrarily combined, that is, any lower limit can be combined with any upper limit to form a scope. For example, if the scope of 60-120 and 80-110 is listed for a specific parameter, it is understood that the scope of 60-110 and 80-120 is also expected. In addition, if the minimum range values ​​1 and 2 are listed, and if the maximum range values ​​3, 4 and 5 are listed, the following scope can be all expected: 1-3, 1-4, 1-5, 2-3, 2-4 and 2-5. In the present application, unless otherwise specified, the numerical range "ab" represents the abbreviation of any real number combination between a and b, wherein a and b are real numbers. For example, the numerical range "0-5" means that all real numbers between "0-5" are listed in this document, and "0-5" is just an abbreviation of these numerical combinations. In addition, when a parameter is expressed as an integer ≥ 2, it is equivalent to disclosing that the parameter is, for example, an integer of 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc.

[0040] In order to make the above-mentioned purposes, features and advantages of the present application more obvious and understandable, the technical solution of the present application is further described below in conjunction with the accompanying drawings and embodiments. However, the present application is not limited to the listed embodiments, and should also include any other known changes within the scope of the rights claimed in the present application.

[0041] In recent years, the rapid development of consumer electronic product technology has put forward higher and higher requirements on the structural materials and component performance of electronic devices. In order to adapt to the trend of electronic devices being thinner and smaller, electronic device shells, such as notebooks, AR (Augmented Reality), VR (Virtual Reality), PAD (Portable Android Device), etc., these materials need to have a series of characteristics, such as low density, high strength and stiffness, excellent impact resistance and vibration reduction performance, strong electromagnetic shielding ability, good heat dissipation performance, easy forming and processing, beautiful surface, durability, low cost, easy recycling and environmental protection requirements. Traditional plastics and aluminum materials are gradually unable to meet these requirements. However, magnesium and its alloys, as ideal materials for manufacturing electronic device shells, have shown broad application prospects. Magnesium and its alloy materials have many advantages, including low density, light weight, high strength and stiffness, excellent impact resistance and vibration reduction performance, and good electromagnetic shielding ability and heat dissipation performance. However, it is undeniable that magnesium alloy materials also face some disadvantages in use. For example, for some mechanical structural parts such as brackets, thin-walled support parts and other product parts, it is difficult for magnesium alloys to have an advantage in application scenarios where the design requires high strength, high stiffness and high-gloss surface treatment.

[0042] In order to meet the requirements of lightweight and high strength / rigidity performance of structural parts, many design ideas have emerged in the industry, such as magnesium alloy composite materials; magnesium alloy insert die casting, which has been studied more deeply, is to add high-strength materials such as aluminum alloy, stainless steel, titanium alloy, etc. to magnesium alloy die casting to achieve high strength and high stiffness performance under the condition of reducing a certain density; magnesium alloy insert aluminum alloy technology is relatively easy to achieve because the properties and physical properties of the two materials are similar, but magnesium alloy insert stainless steel die casting and magnesium alloy insert titanium alloy die casting are difficult to achieve because the properties and physical properties of the two materials are quite different. Through investigation and understanding, although there are relevant technical reports on magnesium alloy die-casting directly embedded in stainless steel inserts in the industry, through actual verification and analysis, due to the large difference between the melting point, expansion coefficient, thermal conductivity and elastic modulus of magnesium alloy and stainless steel materials and the standard electrode difference, after the two metals are directly inserted into the die-casting, not only the interface stress of the two metals is too large, resulting in interface cracks and causing component failure, but also when there is a solute medium between the interface of magnesium alloy and stainless steel, galvanic corrosion will occur, affecting the stability and performance of magnesium alloy structural parts, so magnesium alloy direct die-casting insert stainless steel has no great practical production significance. The embodiment of the present application can use a transition cold sprayed aluminum coating that has good contact with magnesium alloy on the stainless steel surface to improve the performance of magnesium alloy insert stainless steel die-casting.

[0043] The present application embodiment provides a method for preparing a magnesium alloy insert. In this embodiment, the method for preparing the magnesium alloy insert comprises the following steps S10 to S20:

[0044] Step S10, preparing an aluminum coating on a preset surface area of ​​the insert to be processed to obtain a pre-processed insert, wherein the material of the insert to be processed includes stainless steel and titanium alloy;

[0045] The insert to be processed refers to the workpiece to be embedded in the matrix and not covered with aluminum coating. The surface of the insert to be processed is covered with aluminum coating to become the primary processing insert. The material of the insert to be processed can include stainless steel and titanium alloy. Both stainless steel and titanium alloy have higher strength than magnesium alloy. After the stainless steel insert or titanium alloy insert is embedded in the magnesium alloy, the overall density is improved, and the strength performance is significantly improved, so it can meet the requirements of low density and high strength.

[0046] The preset surface area refers to the area of ​​the insert to be processed that is preset to be prepared with the aluminum coating. The preset surface area can be the entire surface of the insert to be processed, or it can be determined according to the depth of the insert to be processed embedded in the magnesium alloy, and is set so that the height of the preset surface area is equal to the embedding depth, or the height of the preset surface area is greater than the embedding depth, so that the overlapped portion of the pre-processed insert and the magnesium alloy is transitioned by the aluminum coating, and the area of ​​the aluminum coating is greater than or equal to the overlapped area of ​​the pre-processed insert and the magnesium alloy substrate.

[0047] Methods for preparing aluminum coating on the surface of the insert to be processed include plasma cold spraying, electroplating, 3D printing or PVD (Physical Vapor Deposition). Through the above coating preparation methods, a dense aluminum coating with a certain thickness is formed on the surface of the insert to be processed.

[0048] As an example, before the step of preparing an aluminum coating on a preset surface area of ​​the insert to be processed to obtain a pre-processed insert, the method further includes:

[0049] Step A10, preparing materials to be processed;

[0050] The material to be processed refers to the raw material for preparing the insert to be processed. The types of raw materials are different when inserts to be processed are selected from different materials. The model and shape of the material to be processed can also be selected according to the strength and shape requirements of the magnesium alloy insert. The inserts to be processed made of stainless steel can include grades such as 304, 304L, 304N, 309, 309S, 310, 316, 316L, 321, 410, and 416. The inserts to be processed made of titanium alloy can include grades such as TA1, TA2, TA3, TA4, TA5, TC4, TC6, and TC11. The shape of the material to be processed can include plates, pipes, bars, or other shaped materials.

[0051] Step A20, processing the material to be processed according to a preset shape to obtain the insert to be processed, wherein the processing includes at least one of CNC machine tool processing, forging, casting, rolling and extrusion.

[0052] The preset shape refers to the shape designed for the insert to be processed according to actual needs. It is understandable that the insert to be processed can be the same as the primary processed insert in overall shape, that is, there is no need to perform a large amount of shaping after the primary processed insert is embedded in the magnesium alloy. The processing method of the material to be processed includes at least one of CNC machine tool processing, forging, casting, rolling and extrusion. According to the properties of the material to be processed, a suitable processing method is selected to obtain an insert to be processed with a suitable shape.

[0053] As an example, before the step of preparing the aluminum coating on the preset surface area of ​​the insert to be processed, the insert surface can also be pretreated. In the process of insert surface pretreatment, the insert surface is polished by mechanical polishing to a near mirror state, and after cleaning, the surface is treated with 205# zircon sand and is ready for use.

[0054] As an example, the steps of preparing an aluminum coating on a predetermined surface area of ​​an insert to be machined include:

[0055] Step B10, placing the insert to be processed in the spraying direction of the plasma cold spraying equipment;

[0056] This embodiment adopts a plasma cold spraying method to prepare an aluminum coating. Plasma cold spraying is a method of obtaining a functional coating by using the kinetic energy of high-speed gas to drive powder particles to achieve effective deposition. It can prepare a thick coating with high coating density, high bonding strength with the substrate, and relatively low temperature. Plasma cold spraying equipment is a device that performs plasma spraying to form a coating on the surface of a workpiece. The plasma cold spraying equipment includes a spray gun, and the coating material is sprayed out from the nozzle of the spray gun. After the coating material reaches the surface of the workpiece, it adheres to form a coating. The spraying direction refers to the direction in which the nozzle sprays the coating material, and the spraying direction is determined by the direction of the nozzle. In an operative method, the spraying direction is set to a direction parallel to the horizontal plane, the insert to be processed is placed in the spraying direction, and the plane where the surface of the insert to be processed is located is set perpendicular to the horizontal plane, so that the spraying is more uniform and an aluminum coating with a relatively uniform thickness is formed.

[0057] Step B20, spraying aluminum powder particles onto the preset surface area by spraying carrier gas to form an aluminum coating on the preset surface area.

[0058] The spray carrier gas refers to the gas sprayed from the spray gun. The spray carrier gas can carry the powdered coating material. It is understood that there is no reaction between the spray carrier gas and the coating material. The coating material of this embodiment is aluminum powder particles, and the spray carrier gas can be selected from high-pressure nitrogen or inert gas. The spray carrier gas impacts the aluminum powder particles to the preset surface area of ​​the pre-processed insert, and the aluminum powder particles undergo plastic deformation in the preset surface area, and the temperature is reduced and the aluminum coating is formed by cooling and deposition.

[0059] In one feasible method, aluminum powder particles are prepared by ion atomization method, which has the characteristics of high sphericity, high purity and uniform particle size distribution, which is conducive to the formation of a dense aluminum coating. High-purity aluminum powder particles with a mass content greater than or equal to 99% are selected, and the thin oxide film on the surface of the particles is more likely to form a strong bond, and the deposition efficiency is higher. The diameter of the aluminum powder particles can be 0.5μm-20μm, for example, 0.5μm, 1μm, 3μm, 5μm, 10μm, 13μm, 15μm, 18μm, 20μm. The larger the diameter of the aluminum powder particles, the greater the kinetic energy required for plastic deformation, which is not conducive to the formation of a smooth and dense coating. Aluminum powder particles with small diameters have higher deposition efficiency, but are not easy to obtain, and the preparation cost also increases significantly. The aluminum powder particles can also be dried at 80°C-120°C for 10min-20min before spraying. The drying temperature can be 80°C, 90°C, 100°C, 110°C, 120°C, and the drying time can be 10min, 12min, 15min, 18min, 20min.

[0060] In one practicable manner, the surface of the pre-machined insert is degreased before spraying, and the carrier gas temperature of the spray carrier gas is set to 120°C-250°C, for example, 120°C, 150°C, 180°C, 200°C, 220°C, 250°C. By setting the temperature of the spray carrier gas within a suitable range, the aluminum powder particles can be preheated, the resistance of the aluminum powder particles to plastic deformation can be reduced, and the deposition rate can be increased. The carrier gas pressure of the spray carrier gas can be 0.8MPa-2.0MPa, for example, 0.8MPa, 0.9MPa, 1.0MPa, 1.5MPa, 2.0MPa. The greater the carrier gas pressure, the greater the impact force of the spray carrier on the aluminum powder particles. The coating formed by too low a carrier pressure has poor density and weak interface bonding. The spraying distance of the spray carrier gas is 10mm-30mm. The spraying distance refers to the distance between the nozzle position and the preset surface area of ​​the pre-processed insert. The spraying distance can be set in combination with the temperature and pressure of the spray carrier gas, for example, 10mm, 15mm, 20mm, 25mm, 30mm. The powder feeding rate of aluminum powder particles is 0.6g / s-2.0g / s, for example, 0.6g / s, 0.8g / s, 1.0g / s, 1.2g / s, 1.5g / s, 1.8g / s, 2.0g / s. If the powder feeding rate is too low, the deposition rate of the aluminum coating is low. If the powder feeding rate is too high, some particles with a low degree of plastic deformation may exist, resulting in poor surface quality of the coating.

[0061] In an operative manner, the thickness of the aluminum coating is 10 μm-60 μm, for example, 10 μm, 20 μm, 25 μm, 30 μm, 35 μm, 40 μm, 45 μm, 50 μm, 60 μm. In the case where the thickness of the aluminum coating is too small, the aluminum coating has a small effect on improving the interface bonding. The prepared aluminum coating can be a fine-grained aluminum coating with a grain size of 0.1 μm-20 μm.

[0062] Step S20, die-casting the pre-machined insert into a magnesium alloy substrate, and embedding the aluminum coating into the magnesium alloy substrate to obtain a magnesium alloy insert.

[0063] Die casting belongs to the metal casting process, which uses the inner cavity of the mold to apply high pressure to the molten metal to form a casting. In this embodiment, a primary processing insert made of stainless steel or titanium alloy is embedded in a magnesium alloy matrix by die casting to obtain a magnesium alloy insert. During the die casting process, a part of the primary processing insert is embedded in the magnesium alloy matrix, and a part is exposed outside the magnesium alloy matrix. The part embedded in the magnesium alloy matrix is ​​transitioned by an aluminum coating. The magnesium alloy matrix is ​​used as a part to meet the lightweight requirements, and the insert made of stainless steel or titanium alloy can improve the overall strength. The aluminum coating forms a transition between the magnesium alloy matrix and the primary processing insert, achieving a firm bond at the joint. The selected grades of the magnesium alloy matrix may include AZ91D, AZ31B, AZ40, AZ41, etc.

[0064] As an example, after the step of die-casting the pre-processed insert into a magnesium alloy substrate and embedding the aluminum coating into the magnesium alloy substrate to obtain the magnesium alloy insert, the method may further include:

[0065] Step C10, performing sandblasting, passivation and spraying treatment on the magnesium alloy part of the magnesium alloy insert;

[0066] After the magnesium alloy insert is prepared, the original magnesium alloy matrix becomes the magnesium alloy part, and the original pre-processed insert becomes the insert part. Different parts of the magnesium alloy insert have different requirements in actual use and can be treated differently. For the magnesium alloy part, it can be cleaned and dried after die casting to clean the surface of the magnesium alloy insert, and then sandblasted, passivated and sprayed to prepare a coating on the surface of the magnesium alloy part to meet the requirements of appearance, wear resistance or corrosion resistance.

[0067] Step C20, masking the magnesium alloy portion, and polishing the insert portion of the magnesium alloy insert.

[0068] After the magnesium alloy part is processed, the insert part is processed. The magnesium alloy part can be shielded by a baffle, and metallographic high-gloss polishing can be performed to carry out surface decoration to achieve good appearance requirements and make up for the defects of poor surface treatment of the magnesium alloy.

[0069] In this embodiment, an aluminum coating is prepared on a preset surface area of ​​the insert to be processed to obtain a primary processed insert, and the material of the insert to be processed includes stainless steel and titanium alloy; the primary processed insert is die-cast into a magnesium alloy substrate, and the aluminum coating is embedded in the magnesium alloy substrate to obtain a magnesium alloy insert. By preparing an aluminum coating on the surface of the insert to be processed, the aluminum coating can serve as a transition between the magnesium alloy and the insert material after die-casting to form a magnesium alloy insert. The physical and chemical properties of magnesium alloy and aluminum are similar. Compared with the direct die-casting method, the interface bonding force between the magnesium alloy substrate and the insert material is improved, and the problem of interface cracks caused by excessive interface stress leading to component failure can be avoided, thereby improving the performance of magnesium alloy and high-strength material inserts.

[0070] The embodiment of the present application also provides a magnesium alloy insert, which is prepared by the method for preparing the magnesium alloy insert as described above. The magnesium alloy insert includes a magnesium alloy matrix and an insert, and the material of the insert includes stainless steel and titanium alloy. In an operative method, the magnesium alloy matrix is ​​a bracket body, which is composited with the insert to form a composite bracket structure that can achieve lightweight requirements and has high strength.

[0071] By coating a layer of fine-grained aluminum coating on the surface of the stainless steel insert for the magnesium alloy die-cast bracket, the magnesium alloy bracket and the high-strength material insert such as stainless steel can be die-casted into one piece, thereby improving the mechanical properties such as the overall strength of the material. The obtained magnesium alloy insert composite material structural parts have mechanical properties higher than those of pure magnesium alloy materials, as well as advantages such as high strength, high rigidity, high dimensional stability, and good lightweight, without undesirable problems such as cracking between dissimilar metals. At the same time, the exposed magnesium substrate surface of the non-magnesium alloy material insert can achieve better surface decoration treatment, such as anode, PVD, high gloss, etc., which solves the problem of poor surface treatment of magnesium alloy.

[0072] The embodiment of the present application also provides an electronic device, which includes the magnesium alloy insert as described above. The types of electronic devices include computer, communication and consumer electronic products, as well as emerging AR, VR, and PAD products. The beneficial effects of this embodiment refer to the preparation method of the magnesium alloy insert and the embodiment of the magnesium alloy insert, which will not be repeated here.

[0073] The following describes the implementation of the method for preparing the magnesium alloy insert of the present application in conjunction with specific examples.

[0074] Example 1

[0075] (1) Die casting insert processing, such as Figure 1 As shown, Figure 1 Schematic diagram of the structure of the stainless steel insert 100. The insert 100 is made of 316L stainless steel, a stamping or forging part, and has a thickness of 0.5 mm-2.5 mm.

[0076] (2) The surface pretreatment of 316L stainless steel 100 inserts is done by mechanical polishing. The surface is polished to a value close to the mirror state. After cleaning, the surface is treated with 205# zirconium sand.

[0077] (3) Spraying aluminum coating on the surface of insert 100. The surface of insert 100 made of 316L stainless steel is cold-sprayed with aluminum layer; the spraying material is high-purity aluminum (mass content ≥99%), and the diameter of aluminum powder particles is 0.5μm-20μm; the equipment is plasma cold spraying equipment; the equipment model is integrated cold spraying equipment JHL-CS600, the equipment power is 16KW, high-speed cold spraying technology is adopted, the spraying carrier gas is high-pressure nitrogen, the surface is degreased before spraying, the carrier gas temperature is 120℃-250℃, the carrier gas pressure is 0.8MPa-2.0MPa, the spraying distance is 20mm, and the powder feeding rate is 0.6g / s-2.0g / s; the spraying powder is prepared by ion atomization method and dried at 80℃-120℃ for 15min before use; the spraying thickness is 10μm-60μm; the grain size is 0.1μm-20μm.

[0078] (4) Using magnesium alloy as AZ91D material, Figure 2 is a schematic diagram of the structure of the magnesium alloy substrate 200, such as Figure 2 As shown, the magnesium alloy substrate 200 adopts a bracket structure, and the insert 100 after spraying the aluminum coating is placed in a magnesium alloy die-casting mold to die-cast a composite material structure. The die-casting process conditions are: pouring temperature of 700°C, mold temperature of 210°C, injection speed of 5m / s; Figure 3 is a schematic diagram of the structure of the magnesium alloy insert 300, such as Figure 3 As shown in the figure, after die casting, a part of the stainless steel is embedded in the magnesium alloy body, and a part is exposed outside. Hot chamber die casting is carried out according to the magnesium alloy die casting process conditions, and the workpiece is taken out after die casting and surface grinding is carried out.

[0079] (5) Post-processing of magnesium alloy die-cast composite materials: the magnesium alloy part can be processed by cleaning + drying + sandblasting + passivation + spraying + drying. After the treatment, the magnesium alloy part is masked and the stainless steel surface is metallographically high-gloss polished to achieve high-gloss surface treatment of magnesium alloy inserts.

[0080] The serial numbers of the above-mentioned embodiments of the present application are for description only and do not represent the advantages or disadvantages of the embodiments.

[0081] The above are only preferred embodiments of the present application, and are not intended to limit the patent scope of the present application. Any equivalent structure or equivalent process transformation made using the contents of the present application specification and drawings, or directly or indirectly applied in other related technical fields, are also included in the patent protection scope of the present application.

Claims

1. A method for preparing a magnesium alloy insert, characterized in that: The method includes: Prepare an aluminum coating on a preset surface area of ​​an insert to be processed to obtain a pre-processed insert, wherein the material of the insert to be processed includes stainless steel and titanium alloy; The pre-machined insert is die-casted into a magnesium alloy substrate, and the aluminum coating is embedded in the magnesium alloy substrate to obtain a magnesium alloy insert.

2. The method according to claim 1, characterized in that The step of preparing an aluminum coating on a predetermined surface area of ​​the insert to be processed comprises: Placing the insert to be processed in the spraying direction of the plasma cold spraying equipment; Aluminum powder particles are sprayed onto the preset surface area by spraying carrier gas, so as to form an aluminum coating on the preset surface area.

3. The method according to claim 2, characterized in that The aluminum powder particles are prepared by ion atomization method; And / or, the diameter of the aluminum powder particles is 0.5 μm-20 μm; And / or, the aluminum powder particles are dried at 80° C.-120° C. for 10 min-20 min before spraying.

4. The method according to claim 2, characterized in that The spraying carrier gas is high-pressure nitrogen; and / or, the carrier gas temperature of the spray carrier gas is 120° C.-250° C.; And / or, the carrier gas pressure of the spraying carrier gas is 0.8MPa-2.0MPa.

5. The method according to claim 2, characterized in that The spraying distance of the spray carrier gas is 10mm-30mm; The feeding rate of the aluminum powder particles is 0.6 g / s-2.0 g / s.

6. The method according to claim 1, characterized in that The thickness of the aluminum coating is 10 μm-60 μm; And / or, the aluminum coating is a fine-grained aluminum coating with a grain size of 0.1 μm-20 μm.

7. The method according to claim 1, characterized in that Before the step of preparing an aluminum coating on a preset surface area of ​​the insert to be processed to obtain a pre-processed insert, the step further includes: Prepare materials to be processed; The material to be processed is processed according to a preset shape to obtain the insert to be processed, and the processing includes at least one of CNC machine tool processing, forging, casting, rolling and extrusion.

8. The method according to any one of claims 1 to 7, characterized in that After the step of die-casting the pre-processed insert into the magnesium alloy matrix and embedding the aluminum coating into the magnesium alloy matrix to obtain the magnesium alloy insert, the method further includes: performing sandblasting, passivation and spraying treatments on the magnesium alloy part of the magnesium alloy insert; The magnesium alloy portion is masked, and the insert portion of the magnesium alloy insert is polished.

9. A magnesium alloy insert, characterized in that: The magnesium alloy insert is prepared by the method for preparing a magnesium alloy insert according to any one of claims 1 to 8.

10. An electronic device, characterized in that: The electronic device comprises the magnesium alloy insert as claimed in claim 9.