Quantum dot light conversion film, preparation method thereof and backlight module

By adjusting the thickness and material composition of the quantum dot film layer in the quantum dot light conversion film, combined with the melt co-extrusion process and packaging film layer design, the problem of large fluctuations in film thickness and color point during the production process of the quantum dot light conversion film is solved. problem, achieving ultra-thin, high-stability and high-brightness quantum dot light conversion films.

CN118789915AActive Publication Date: 2024-10-18FUDAN UNIV YIWU RES INST
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202410783072.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-18
Publication Date
2024-10-18
Estimated Expiration
2044-06-18

AI Technical Summary

Technical Problem

Existing quantum dot light conversion films have problems with large fluctuations in film thickness and color points during the production process, resulting in unstable product quality and making it difficult to achieve large-scale use of ultra-thin quantum dot light conversion films.

Method used

A quantum dot light conversion film structure is designed, including a base film, a first quantum dot film layer and a second quantum dot film layer. By adjusting the thickness and material composition of the quantum dot film layer, the color point fluctuation is reduced, and melting is adopted. The co-extrusion process prepares the ultra-thin film layer, which is combined with the encapsulation film layer to improve light extraction rate and brightness.

Benefits of technology

It achieves a reduction in the thickness and color point fluctuation of the quantum dot light conversion film, improves product batch stability and luminescence uniformity, reduces production difficulty and cost, and is suitable for ultra-thin quantum dot light conversion films for display devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118789915A_ABST
    Figure CN118789915A_ABST
Patent Text Reader

Abstract

The invention provides a quantum dot light conversion film, a preparation method of the quantum dot light conversion film and a backlight module comprising the quantum dot light conversion film. The quantum dot light conversion film comprises a base film, a first quantum dot film layer, a second quantum dot film layer and a packaging film layer which are sequentially arranged in a contact mode. The base film comprises a barrier film layer and a PET film layer, and the barrier property of the base film is that WVTR is less than or equal to 2g / m < 2 >. Day; the first quantum dot film layer comprises first quantum dots and first resin, the second quantum dot film layer comprises second quantum dots and polyethylene glycol terephthalate, the packaging film layer comprises second resin and inorganic oxide particles, and the first quantum dots and the second quantum dots are selected from one or two of red quantum dots and green quantum dots; the total mass fraction of the red quantum dots and the green quantum dots in the first quantum dot film layer is 0.01-1%. The structure of the double-quantum-dot film layer can reduce the quantum dot content of the first quantum dot film layer and reduce the color dot volatility of the first quantum dot film layer, and products with stable color dot batches can be produced more easily.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present disclosure relates to the field of quantum dot light conversion technology, and in particular, to a quantum dot light conversion film and a preparation method thereof, and a backlight module. Background Art

[0002] The typical quantum dot light conversion film is a sandwich structure, with upper and lower barrier films and a red and green quantum dot resin layer in the middle. Because of the protection of the barrier film, the quantum dots in the quantum dot layer are generally selected to have higher performance efficiency and narrower half-peak width (such as half-peak width <20nm), which can show better color gamut coverage, but the cost is high, which affects its large-scale use; at the same time, because the red and green quantum dot resin layer has a high quantum dot content, it is difficult to control the relevant color point (color coordinates). Considering the thickness fluctuation of the coating equipment, if the red and green quantum dot resin layer is too thin, the color point deviation caused by the equipment coating thickness fluctuation deviation (such as ±3μm) will cause the display device to have a color point deviation, causing quality problems. Therefore, the general resin layer thickness is about 100μm. If the thickness continues to be reduced, it will easily cause color point deviation, that is, the color points of the quantum dot light conversion films of the same batch or different batches are different, which will lead to product quality problems. Therefore, it is difficult to achieve ultra-thin quantum dot light conversion films. Summary of the invention

[0003] The purpose of the present disclosure is to provide a quantum dot light conversion film and a preparation method thereof, and a backlight module, and to solve the problem of large thickness-color point fluctuation of the quantum dot light conversion film in production through the structural design of the quantum dot light conversion film.

[0004] According to a first aspect of the present disclosure, a quantum dot light conversion film is provided, comprising a base film, a first quantum dot film layer, a second quantum dot film layer and an encapsulation film layer which are sequentially arranged in contact; the base film comprises a barrier film layer and a PET film layer, and the barrier property of the base film is WVTR≤2g / m 2 ·day; the first quantum dot film layer includes the first quantum dots and the first resin, the second quantum dot film layer includes the second quantum dots and polyethylene terephthalate, the encapsulation film layer includes the second resin and inorganic oxide particles, the first quantum dots and the second quantum dots are selected from one or both of red quantum dots and green quantum dots; the mass fraction of the red quantum dots and the green quantum dots in the first quantum dot film layer is 0.01-1% in total.

[0005] Optionally, the refractive index of the first resin is lower than that of the PET film layer, the refractive index of the first resin is between 1.38 and 1.6, and the refractive index of the encapsulation film layer is higher than that of the first resin.

[0006] Optionally, the mass fraction of red quantum dots and green quantum dots in the second quantum dot film layer is 0.01-20%, preferably 0.1-10%. Preferably, the first quantum dot film layer and the second quantum dot film layer further comprise second diffusion particles.

[0007] Optionally, the thickness of the first quantum dot film layer is 1 to 100 μm, preferably 3 to 70 μm; the thickness of the second quantum dot film layer is 6 to 250 μm, preferably 12 to 125 μm.

[0008] Optionally, the base film has a thickness of 12 to 125 μm, and the packaging film layer has a thickness of 0.5 to 25 μm.

[0009] Optionally, the quantum dot light conversion film has a thickness of 37.5 to 75 μm.

[0010] Optionally, the second resin material includes one or more of acrylic resin, epoxy resin, and silicone resin, and the inorganic oxide particles are selected from one or more of zirconium oxide, titanium oxide, and silicon oxide.

[0011] Optionally, the fluorescence half-peak width of the first quantum dot film layer is less than or equal to 25 nm, and the external quantum efficiency is greater than or equal to 40%, and / or the fluorescence half-peak width of the second quantum dot film layer is greater than or equal to 25 nm, and the external quantum efficiency is less than 40%.

[0012] According to the second aspect of the present disclosure, a method for preparing the above-mentioned quantum dot light conversion film is provided, comprising melt co-extruding a composition containing the second quantum dots and particles of polyethylene terephthalate to obtain a single-layer or multi-layer second quantum dot film layer; preparing the base film and the glue containing the first quantum dots; using a coating device to coat the glue containing the first quantum dots between the base film and the second quantum dot film layer, and curing to obtain an intermediate, wherein the intermediate comprises a base film, the first quantum dot film layer and the second quantum dot film layer which are sequentially contacted; coating the glue containing the inorganic oxide particles on the second quantum dot film layer, and curing to obtain the encapsulation film layer, and finally obtaining the quantum dot light conversion film.

[0013] Optionally, the second quantum dot-containing composition includes red quantum dot masterbatch, green quantum dot masterbatch, diffusion masterbatch, stabilizer and antioxidant.

[0014] According to a third aspect of the present disclosure, a backlight module is provided, comprising any one of the above-mentioned quantum dot light conversion films.

[0015] By applying the above solution, the quantum dot content of the first quantum dot film layer can be reduced, the color point volatility of the layer can be reduced, and products with batch stability of color points can be produced more easily. BRIEF DESCRIPTION OF THE DRAWINGS

[0016] The drawings constituting part of the present application are used to provide a further understanding of the present disclosure. The exemplary embodiments of the present disclosure and their descriptions are used to explain the present disclosure and do not constitute an improper limitation on the present disclosure. In the drawings:

[0017] Figure 1 A structural schematic diagram of an embodiment of the present application is shown.

[0018] Figure 2 A flow chart of an embodiment of the present application is shown.

[0019] Figure 3 The aging performance diagrams of the examples and comparative examples of the present application are shown.

[0020] 1. Base film; 2. First quantum dot film layer; 3. Second quantum dot film layer; 4. Encapsulation film layer.

[0021] For ease of understanding, the position, size, range, etc. of each structure shown in the drawings and the like may not represent the actual position, size, range, etc. Therefore, the present disclosure is not limited to the position, size, range, etc. disclosed in the drawings and the like. DETAILED DESCRIPTION

[0022] It should be noted that the following detailed descriptions are illustrative and are intended to provide further explanation of the present application. Unless otherwise specified, all technical and scientific terms used herein have the same meanings as those commonly understood by those skilled in the art to which the present application belongs.

[0023] In addition, technologies, methods, and apparatus known to ordinary technicians in the relevant field may not be discussed in detail, but where appropriate, such technologies, methods, and apparatus should be considered part of the authorization specification.

[0024] In all examples shown and discussed herein, any specific values ​​should be interpreted as merely exemplary and not as limiting. Therefore, other examples of the exemplary embodiments may have different values.

[0025] The words "left", "right", "front", "back", "top", "bottom", "up", "down", "high", "low", etc., in the specification and claims, if present, are used for descriptive purposes and are not necessarily used to describe an unchanging relative position. It should be understood that the words so used are interchangeable under appropriate circumstances, so that the embodiments of the present disclosure described herein, for example, can operate in other orientations than those shown or otherwise described herein. For example, when the device in the drawings is turned over, features previously described as being "above" other features may now be described as being "below" the other features. The device may also be oriented in other ways (rotated 90 degrees or in other orientations), and the relative spatial relationships will be interpreted accordingly.

[0026] In the specification and claims, when an element is referred to as being "on", "attached", "connected", "coupled" or "coupled" to another element, the element may be directly on, directly attached, directly connected, directly coupled or directly coupled to another element, or one or more intermediate elements may be present. In contrast, when an element is referred to as being "directly" "on", "directly attached", "directly connected", "directly coupled" or "directly coupled" to another element, there will be no intermediate elements. In the specification and claims, a feature being arranged "adjacent" to another feature may refer to a feature having a portion that overlaps with an adjacent feature or a portion that is located above or below the adjacent feature.

[0027] As used herein, the word "exemplary" means "serving as an example, embodiment, or illustration" rather than as a "model" to be exactly copied. Any implementation described as exemplary herein is not necessarily to be construed as preferred or advantageous over other implementations. Furthermore, the present disclosure is not to be limited by any expressed or implied theory given in the technical field, background, summary, or detailed description.

[0028] As used herein, the term "substantially" is intended to include any minor variations due to design or manufacturing imperfections, device or component tolerances, environmental influences, and / or other factors. The term "substantially" also allows for deviations from a perfect or ideal condition due to parasitic effects, noise, and other practical considerations that may exist in actual implementations.

[0029] In addition, the terms "first", "second" and the like may also be used herein for reference purposes only, and thus are not intended to be limiting. For example, the terms "first", "second" and other such numerical terms referring to structures or elements do not imply a sequence or order unless the context clearly indicates otherwise.

[0030] It should also be understood that when the term “include / comprises” is used in this document, it indicates the presence of the specified features, integers, steps, operations, units and / or components, but does not exclude the presence or addition of one or more other features, integers, steps, operations, units and / or components and / or their combinations.

[0031] In this disclosure, the term "provide" is used in a broad sense to cover all ways of obtaining an object, and thus "providing an object" includes but is not limited to "purchasing", "preparing / manufacturing", "arranging / setting up", "installing / assembling", and / or "ordering" an object, etc.

[0032] As used herein, the term "and / or" includes any and all combinations of one or more of the associated listed items. The terms used herein are for the purpose of describing specific embodiments only and are not intended to limit the present disclosure. As used herein, the singular forms "a", "an", and "the" are also intended to include the plural forms, unless the context clearly indicates otherwise.

[0033] According to the first aspect of the present application, a quantum dot light conversion film is provided, comprising a base film, a first quantum dot film layer, a second quantum dot film layer and an encapsulation film layer which are sequentially arranged in contact; the base film comprises a barrier film layer and a PET film layer, and the barrier property of the base film is WVTR≤2g / m 2 .day; the first quantum dot film layer includes the first quantum dots and the first resin, the second quantum dot film layer includes the second quantum dots and polyethylene terephthalate, the encapsulation film layer includes the second resin and the inorganic oxide, the first quantum dots and the second quantum dots include one or two of red quantum dots and green quantum dots; the mass fraction of the red quantum dots and the green quantum dots in the first quantum dot film layer is 0.01-1%. WVTR refers to water vapor transmission rate (WaterVapor Transmission Rate).

[0034] The ratio of red and green quantum dots in the first quantum dot film layer and the second quantum dot film layer can be flexibly adjusted. Due to the presence of the second quantum dot film layer, the quantum dot content of the first quantum dot film layer can be reduced, the color point volatility can be reduced, and it is easier to produce products with color point batch stability. In addition, the inorganic oxide particles in the encapsulation film layer have the function of diffusing light, which can improve the luminescence uniformity of the quantum dot light conversion film.

[0035] In the base film, the barrier film layer is closer to the first quantum dot film layer than the PET film layer. In some embodiments, the barrier property of the base film is WVTR≤0.5g / m 2 day, preferably ≤0.08g / m 2 ·day, the higher the barrier property of the base film, the higher the cost, but the better the protection effect on quantum dots.

[0036] In some embodiments, the refractive index of the first resin is lower than that of the PET film layer, and the refractive index of the first resin is between 1.38-1.6, preferably 1.45-1.58, and the refractive index of the encapsulation film layer is higher than that of the first resin. In addition, the multi-layer compact structure design avoids total reflection inside the film layer, improves the light extraction rate, and improves the brightness of the quantum dot light conversion film during use.

[0037] In some embodiments, the barrier property of the encapsulation film layer is worse than that of the base film, and the cost of the encapsulation film layer is lower than that of the base film, thus reducing the cost of the overall quantum dot light conversion film.

[0038] In some embodiments, the quantum dot light conversion film has a hardness range of HB-3H.

[0039] In some embodiments, the first quantum dots and the second quantum dots each include two or more quantum dots with different peak emission wavelengths.

[0040] In some embodiments, the mass fraction of red quantum dots and green quantum dots in the second quantum dot film layer is 0.01-20%, preferably 0.1-10% or 0.1-1.5% or 0.1-1%. The comprehensive calculation is performed according to the color point requirements and the quantum dot mass fraction of the first quantum dot film layer.

[0041] In some embodiments, the first quantum dot film layer further includes first diffusion particles. The first diffusion particles are such as organic silicon particles or inorganic oxide particles. In some embodiments, the mass fraction of the organic silicon particles is 0.3-5%. In some embodiments, the inorganic oxide particles of the first diffusion particles are titanium oxide, zirconium oxide, silicon oxide, etc., and their D50 particle size is less than 1 μm, and the mass fraction is 0.1-2%.

[0042] In some embodiments, the second quantum dot film layer further comprises second diffusion particles, which are inorganic oxide particles, such as titanium oxide, zirconium oxide, silicon oxide, etc., and the mass fraction of the second diffusion particles is 0.5-5%. In some embodiments, the second quantum dot film layer further comprises an antioxidant, and the mass fraction is 0.1-5%.

[0043] In some embodiments, the particle size of the second diffusion particles D50 is 2-4 times the particle size of the first diffusion particles D50.

[0044] In some embodiments, the thickness of the first quantum dot film layer is 1 to 100 μm, preferably 3 to 70 μm; the thickness of the second quantum dot film layer is 6 to 250 μm, preferably 12 to 125 μm.

[0045] In some embodiments, the thickness of the first quantum dot film layer is 20-50 μm, and the thickness of the second quantum dot film layer is 23-75 μm.

[0046] In some embodiments, the base film has a thickness of 12 to 125 μm, and the encapsulation film layer has a thickness of 0.5 to 25 μm.

[0047] In some embodiments, the quantum dot light conversion film has a thickness of 19.5 to 500 μm or 37.5 to 345 μm or 37.5 to 220 μm or 37.5 to 150 μm or 37.5 to 100 μm.

[0048] In some embodiments, the thickness of the quantum dot light conversion film is 37.5-75 μm or the thickness of the quantum dot light conversion film is 37.5-70 μm, which is the thickness range of ultra-thin films.

[0049] In some embodiments, the second resin material includes one or more of acrylic resin, epoxy resin, and silicone resin, and the inorganic oxide particles are one or more of zirconium oxide, titanium oxide, silicon oxide, etc. The second resin is preferably a resin with low water and oxygen permeability. The refractive index of the inorganic oxide particles should be relatively high, so that the refractive index of the encapsulation film layer is higher than that of the first resin.

[0050] In some embodiments, the material of the first resin is selected from one or more of acrylic resin, epoxy resin, and silicone resin.

[0051] In some embodiments, the inorganic oxide particles account for 0.1-2% of the mass of the encapsulation film layer, so that the quantum dot light conversion film achieves a better light extraction rate.

[0052] In some embodiments, the particle size D50 of the inorganic oxide particles in the encapsulation film layer is less than 5 μm, preferably less than 0.5 μm.

[0053] In some embodiments, the fluorescence half-width (FWHM) of the first quantum dot film layer is less than or equal to 25nm, and the external quantum efficiency is greater than or equal to 40%. Preferably, the fluorescence half-width and quantum efficiency of the first quantum dot film layer are better than those of the second quantum dot film layer. Thus, the following preparation method can be more suitable.

[0054] In some embodiments, the fluorescence half-peak width of the second quantum dot film layer is greater than or equal to 25 nm, and the external quantum efficiency is less than 40%. According to the following method for preparing the second quantum dot film layer, the extrusion process reduces its luminescence performance.

[0055] The second aspect of the present application provides a method for preparing any of the above-mentioned quantum dot light conversion films, comprising melt co-extruding a composition containing second quantum dots and particles of polyethylene terephthalate to obtain a single-layer or multi-layer second quantum dot film layer; preparing a base film and a glue containing first quantum dots; using a coating device to coat the glue containing the first quantum dots between the base film and the second quantum dot film layer, and solidifying to obtain an intermediate, the intermediate comprising a base film, a first quantum dot film layer and a second quantum dot film layer arranged in contact with each other in sequence; coating the second quantum dot film layer with glue containing inorganic oxide particles, and solidifying to obtain an encapsulation film layer, and finally obtaining a quantum dot light conversion film.

[0056] The above preparation scheme reduces the difficulty of color point regulation. First, the second quantum dot film layer is used as a standard product. Only the color point of the first quantum dot film layer is adjusted (adjusting the corresponding glue formula) to adjust the color point of the final quantum dot light conversion film. Since the second quantum dot film layer already has some quantum dots, the quantum dot content in the first quantum dot film layer can be reduced, and the thickness-color point fluctuation when preparing this layer is greatly reduced. Due to the presence of the second quantum dot film layer, the thickness of the first quantum dot film layer can also be greatly reduced. Furthermore, since the melt extrusion method of the second quantum dot film layer can achieve ultra-thinness, the quantum dot light conversion film can achieve ultra-thinness. The above preparation method reduces the difficulty of producing ultra-thin films and quantum dot light conversion films with high color point accuracy.

[0057] The second quantum dot film layer is prepared by a single-layer or multi-layer extrusion process without changing the conventional PET double-drawing equipment and process, reducing the investment in equipment and process. The preparation cost of the second quantum dot film layer is low, and the thickness can be controlled within a thinner range, such as a minimum of 6 microns.

[0058] The preparation process of the intermediate can adopt a roll-to-roll production process to improve production efficiency. The specific process can refer to the existing technology.

[0059] If only the above-mentioned second quantum dot film layer method is used to prepare a quantum dot light conversion film, the following problems will be faced. 1. Waste caused by the color point control process. Different display device models require color point control of quantum dot light conversion films or color point monitoring during the production process. Due to the high speed of the double-pulling equipment (generally above 80m / min), the process of controlling and confirming the color point will cause a large waste of materials, thereby increasing costs; 2. Poor color rendering performance. In order to meet its high-temperature extrusion process, quantum dot materials undergo a lot of protective treatments, thus sacrificing more performance, such as relatively low quantum efficiency and generally wide half-peak width; 3. At the same time, since the second quantum dot film layer is a homogeneous structure, the optical path of the incident light is short after entering, resulting in less light absorption, and then less red and green light converted, making it difficult to achieve the color point of the high color gamut quantum dot solution required by display device customers. 4. Since PET is used as the film layer matrix, the hardness is not good. This solution can ensure that the hardness of the quantum dot light conversion film is suitable for the assembly of display equipment.

[0060] In some embodiments, the preparation of the second quantum dot film layer and the preparation of the glue containing the first quantum dots can be prepared simultaneously or sequentially, and the order can also be reversed.

[0061] In some embodiments, the composition containing the second quantum dot includes a red quantum dot masterbatch, a green quantum dot masterbatch, a stabilizer, a diffusion masterbatch and an antioxidant. Among them, the raw materials of various masterbatches include polymers, and the polymer can be polyethylene terephthalate. In some embodiments, the quantum dot masterbatch includes a mixture of quantum dot raw materials and polyethylene terephthalate, and its preparation can be granulated by melt co-extrusion of the raw materials. The aforementioned quantum dot raw materials can also be coated before use to improve the stability of the quantum dots. The preparation of the quantum dot masterbatch also includes the addition of antioxidants, stabilizers, etc. to reduce the damage of the quantum dots. In some embodiments, the composition containing the second quantum dot also includes second diffusion particles, and the second diffusion particles are inorganic oxide particles, such as titanium oxide, zirconium oxide, silicon oxide, etc., and the mass fraction of the second diffusion particles is 0.5-5%. In some embodiments, the mass fraction of the antioxidant in the composition containing the second quantum dot is 0.1-5%.

[0062] In some embodiments, the glue containing the first quantum dots includes quantum dots, a photoinitiator, and a polymer precursor of the first resin. In some embodiments, the glue containing the first quantum dots also includes first diffusion particles. The first diffusion particles are such as organosilicon particles or inorganic oxide particles. In some embodiments, the mass fraction of the organosilicon particles is 0.3-5%. In some embodiments, the inorganic oxide particles of the first diffusion particles are titanium oxide, zirconium oxide, silicon oxide, etc., and their D50 particle size is less than 1 μm, and the mass fraction is 0.1-2%.

[0063] In some embodiments, the glue containing the second inorganic oxide particles comprises inorganic oxide particles, a photoinitiator, and a polymer precursor of a second resin. The polymer precursor of the second resin may be the same as or different from the polymer precursor of the first resin.

[0064] In some embodiments, the melt temperature is 260-320°C.

[0065] In some embodiments, red quantum dot masterbatch, green quantum dot masterbatch and PET particles are prepared by double-wire co-extrusion.

[0066] In some embodiments, the quantum dot masterbatch contains materials for protecting the quantum dots at high temperatures, such as antioxidants and stabilizers.

[0067] In some embodiments, the curing method can be light curing or heat curing, mainly depending on the properties of the glue. The curing conditions in the above different steps can be the same or different.

[0068] In some embodiments, the total quantum dot requirement is calculated according to the final color point requirement, and the first quantum dot film layer and the second quantum dot film layer each account for a certain proportion. For example, the total content of red and green quantum dots in the first quantum dot film layer accounts for 0.1-50% or 0.1-40% or 0.1-30% of the total quantum dot requirement mass, which is more conducive to reducing thickness-color point volatility.

[0069] The third aspect of the present application provides a backlight module, which includes any of the above-mentioned quantum dot light conversion films. The above-mentioned backlight module can be used in display devices such as televisions, mobile phones, PADs, monitors, and notebook screens. The ultra-thin quantum dot light conversion film is particularly suitable for mobile phones.

[0070] Hereinafter, the embodiments are described in more detail with reference to specific examples. However, they are exemplary embodiments of the present disclosure, and the present disclosure is not limited thereto.

[0071] Example 1

[0072] 1. Preparation of the Second Quantum Dot Film Layer

[0073] 1. Preparation of quantum dot masterbatch

[0074] Red quantum dot masterbatch (2%): 200g red quantum dot powder (PL622nm peak wavelength, fluorescence half-peak width 24nm), 20g antioxidant 1010, and 9780g polyethylene terephthalate particles are mixed and stirred evenly, and prepared by twin-screw extrusion at 275°C, granulation, and drying.

[0075] Green quantum dot masterbatch (2%): 200g green quantum dot powder (PL532nm peak wavelength, fluorescence half-peak width 24nm), 20g antioxidant 1010, and 9780g polyethylene terephthalate are mixed and stirred evenly, and prepared by twin-screw extrusion at 275°C, granulation, and drying.

[0076] 2. Film preparation

[0077] 775g PET particles, 100g red quantum dot masterbatch, 100g green quantum dot masterbatch, 20g diffused particle titanium dioxide (D50 is 0.4μm), 5g antioxidant 1010 were prepared, and a single screw extruder with a screw diameter of 75 mm was used, and the screw speed was 30 rpm; the heating temperature was 275°C; after the co-extrusion die, the roll was pulled out and cooled to shape, and the mold was cut to obtain the second quantum dot film layer, wherein the second quantum dot film layer had a thickness of 50μm, the mass fraction of the red quantum dots in the film layer was 0.2%, and the mass fraction of the green quantum dots in the film layer was 0.2%. The QY of the second quantum dot film layer was 38%, and the FWHM was 25.5nm.

[0078] 2. Second quantum dot film layer, first quantum dot film layer, base film composite

[0079] 1. Preparation of glue containing the first quantum dots

[0080] Green and red CdSe-based quantum dots (the types of quantum dots are the same as those in quantum dot masterbatch) dissolved in toluene, 89g of matrix resin methacrylate resin, 1g of diffusion particles TiO2 (D50 is 0.5μm), 0.1g of photoinitiator 819 and 10g of diluent acetic acid are mixed, the mass fraction of green quantum dots in the glue is 0.15%, and the mass fraction of red quantum dots in the glue is 0.15%; after vacuum deoxygenation and nitrogen protection, after stirring at a speed of 50-300rpm for 1-3 hours, a glue containing the first quantum dots is obtained.

[0081] 2. Preparation of composite membrane

[0082] The glue containing the first quantum dots is coated with a PET base film with a barrier layer (base film thickness of 20 μm, WVTR = 0.8 g / m 2 ·day), and the second quantum dot film layer (50μm) are laminated together, and then exposed to 365nm UV light. At this time, the glue layer containing the first quantum dots is cured under UV light to form the first quantum dot film layer (20μm), forming a composite film with a total thickness of 90μm.

[0083] 3. Preparation of encapsulation film

[0084] 1. Preparation of inorganic oxide particle colloid

[0085] 88.8g of base resin methacrylic resin, 0.5g of diffusion particle TiO2 (D50 is 0.5μm), 0.5g of diffusion particle silica (D50 is 0.5μm), 0.2g of photoinitiator 819 and 10g of diluent acetic acid are mixed, the mass fraction of the diffusion particle TiO2 is 0.5%, and the mass fraction of the diffusion particle silica is 0.5%; after vacuum deoxygenation and nitrogen protection, stirring at a speed of 50-300rpm for 1-3 hours, an inorganic oxide particle glue solution is obtained;

[0086] 2. Coating and curing:

[0087] The inorganic oxide particle glue was coated on the composite film (film thickness 90 μm) prepared above by slit coating, and then irradiated with 390 nm UV light. At this time, the inorganic oxide particle glue was cured into an encapsulation film layer (10 μm) under UV light, forming a quantum dot light conversion film with a total thickness of 100 μm. The QY of the final quantum dot light conversion film was 42% and the FWHM was 25 nm.

[0088] Example 2

[0089] 1. Preparation of the Second Quantum Dot Film Layer

[0090] 1. Preparation of quantum dot masterbatch is the same as in Example 1

[0091] 2. Film preparation: 671g PET particles, 150g red quantum dot masterbatch, 150g green quantum dot masterbatch, 20g diffusion particle zirconium dioxide (D50 is 0.3μm), 10g antioxidant 626, using a single screw extruder with a screw diameter of 75mm and a screw speed of 27 rpm; heating temperature is 270℃; after co-extrusion die, rolling and pulling out to cool and shape, the second quantum dot film layer is obtained after the mold is cut, wherein the second quantum dot film layer has a thickness of 15μm, the mass fraction of red quantum dots in the film layer is 0.3%, and the mass fraction of green quantum dots in the film layer is 0.3%. The QY of the second quantum dot film layer is 38.5%, and the FWHM is 26nm.

[0092] 2. Second quantum dot film layer, first quantum dot film layer, base film composite

[0093] 1. Preparation of glue containing the first quantum dots

[0094] Green and red CdSe-based quantum dots (the same as those in Example 1) dissolved in toluene, 89 g of a matrix resin methacrylic resin, 1 g of a diffusion particle TiO2 (D50 is 0.3 μm), 0.1 g of a photoinitiator 819 and 10 g of a diluent acetic acid are mixed, the mass fraction of the green quantum dots in the glue is 0.2%, and the mass fraction of the red quantum dots in the glue is 0.2%; after vacuum deoxygenation and nitrogen protection, stirring at a speed of 50 to 300 rpm for 1 to 3 hours, a glue containing the first quantum dots is obtained.

[0095] 2. Preparation of composite membrane

[0096] The glue containing the first quantum dots was used to bond the PET base film with a barrier layer (base film thickness of 15 μm) to the second quantum dot film layer, and then irradiated with 365 nm UV light. At this time, the glue layer containing the first quantum dots was cured under UV light to form the first quantum dot film layer (10 μm), forming a composite film with a total thickness of 40 μm.

[0097] 3. Preparation of encapsulation film

[0098] 1. Preparation of inorganic oxide particle colloid

[0099] 78.8g of base resin methacrylic resin, 10g of butyl acrylate, 0.6g of diffusion particle zirconium dioxide (D50 is 0.3μm), 0.4g of diffusion particle silicon dioxide (D50 is 0.4μm), 0.2g of photoinitiator 819 and 10g of diluent acetic acid are mixed, the mass fraction of diffusion particle TiO2 is 0.6%, and the mass fraction of diffusion particle silicon dioxide is 0.4%; after vacuum deoxygenation and nitrogen protection, after stirring at a speed of 50-300rpm for 1-3 hours, an inorganic oxide particle colloid is obtained.

[0100] 2. Coating and curing:

[0101] The inorganic oxide particle glue was coated on the composite film (film thickness 40 μm) through a slit coating to form a layer of inorganic oxide particle glue, and then irradiated with 390 nm UV light. At this time, the inorganic oxide particle glue was cured into an encapsulation film layer (5 μm) under UV light, forming a quantum dot light conversion film with a total thickness of 45 μm. The QY of the final quantum dot light conversion film was 41% and the FWHM was 24 nm.

[0102] Example 3

[0103] 1. Preparation of the Second Quantum Dot Film Layer

[0104] 1. Preparation of quantum dot masterbatch is the same as in Example 1

[0105] 2. Film preparation

[0106] Prepare 560g PET particles, 200g red quantum dot masterbatch, 200g green quantum dot masterbatch, 20g diffused particle titanium dioxide (D50 is 0.5μm), 20g antioxidant 641, use a single screw extruder with a screw diameter of 75 mm, the screw speed is 35 rpm; the heating temperature is 280℃; after co-extrusion die, then rolling and pulling out cooling and shaping, the second quantum dot film layer is obtained after the mold is cut, wherein the second quantum dot film layer has a thickness of 60μm, the mass fraction of red quantum dots in the film layer is 0.4%, and the mass fraction of green quantum dots in the film layer is 0.4%. The QY of the second quantum dot film layer is 37.5%, and the FWHM is 26nm.

[0107] 2. Second quantum dot film layer, first quantum dot film layer, base film composite

[0108] 1. Preparation of glue containing the first quantum dots

[0109] Green and red CdSe-based quantum dots (the quantum dots are the same as those in Example 1) dissolved in toluene, 89g of matrix resin methacrylic resin, 1g of diffusion particles TiO2 (D50 is 0.5μm), 0.1g of photoinitiator 819 and 10g of diluent acetic acid are mixed, the mass fraction of green quantum dots in the glue is 0.3%, and the mass fraction of red quantum dots in the glue is 0.3%; after vacuum deoxygenation and nitrogen protection, stirring at a speed of 50-300rpm for 1-3 hours, a glue containing the first quantum dots is obtained.

[0110] 2. Preparation of composite membrane

[0111] The glue containing the first quantum dots was laminated to the PET base film with a barrier layer (base film thickness of 55 μm) and the second quantum dot film layer through slit coating, and then irradiated with 390 nm UV light. At this time, the glue layer containing the first quantum dots was cured under UV light to form the first quantum dot film layer (25 μm), forming a composite film with a total thickness of 140 μm.

[0112] 3. Preparation of encapsulation film

[0113] 1. Preparation of inorganic oxide particle colloid

[0114] 78.3g of base resin methacrylic resin, 10g of butyl acrylate, 1g of diffusion particle zirconium dioxide (D50 is 0.4μm), 0.5g of diffusion particle silicon dioxide (D50 is 0.4μm), 0.2g of photoinitiator 819 and 10g of diluent acetic acid are mixed, the mass fraction of diffusion particle TiO2 is 1%, and the mass fraction of diffusion particle silicon dioxide is 0.5%; after vacuum deoxygenation and nitrogen protection, stirring at a speed of 50-300rpm for 1-3 hours, an inorganic oxide particle glue solution is obtained;

[0115] 2. Coating and curing:

[0116] The inorganic oxide particle glue was applied to the composite film (film thickness 140 μm) by a doctor blade, and then irradiated with 390 nm UV light. At this time, the inorganic oxide particle glue was cured into an encapsulation film layer (10 μm) under UV light, forming a quantum dot light conversion film with a total thickness of 150 μm. The QY of the quantum dot light conversion film was 41.5% and the FWHM was 25 nm.

[0117] Example 4

[0118] 1. Preparation of the Second Quantum Dot Film Layer

[0119] 1. Preparation of quantum dot masterbatch is the same as in Example 1

[0120] 2. Film preparation: 560g PET particles, 300g red quantum dot masterbatch, 100g green quantum dot masterbatch, 20g diffused particle titanium dioxide (D50 is 0.2μm), 20g antioxidant 1024, using a single screw extruder with a screw diameter of 75mm and a screw speed of 35 rpm; heating temperature is 285℃; after co-extrusion die, rolling and pulling out to cool and shape, the second quantum dot film layer is obtained after the mold is cut, wherein the second quantum dot film layer has a thickness of 50μm, the mass fraction of red quantum dots in the film layer is 0.6%, and the mass fraction of green quantum dots in the film layer is 0.2%. The QY of the second quantum dot film layer is 38%, and the FWHM is 26nm.

[0121] 2. Second quantum dot film layer, first quantum dot film layer, base film composite

[0122] 1. Preparation of glue containing the first quantum dots

[0123] Green and red CdSe-based quantum dots (the quantum dots are the same as those in Example 1) dissolved in toluene, 89g of matrix resin methacrylic resin, 1g of diffusion particles TiO2 (D50 is 0.2μm), 0.1g of photoinitiator 819 and 10g of diluent acetic acid are mixed, the mass fraction of green quantum dots in the glue is 0.7%, and the mass fraction of red quantum dots in the glue is 0.3%; after vacuum deoxygenation and nitrogen protection, after stirring at a speed of 50-300rpm for 1-3 hours, a glue containing the first quantum dots is obtained.

[0124] 2. Preparation of composite membrane

[0125] The glue containing the first quantum dots was laminated with the PET base film with a barrier layer (base film thickness of 40 μm) and the second quantum dot film layer by comma coating, and then irradiated with 390 nm UV light. At this time, the glue layer containing the first quantum dots was cured into the first quantum dot film layer (40 μm) under UV light, forming a composite film with a total thickness of 130 μm.

[0126] 3. Preparation of encapsulation film

[0127] 1. Preparation of inorganic oxide particle colloid

[0128] 77.6g of base resin methacrylic resin, 10g of butyl acrylate, 1.5g of diffusion particle zirconium dioxide (D50 is 0.3μm), 0.7g of diffusion particle silicon dioxide (D50 is 0.4μm), 0.2g of photoinitiator 819 and 10g of diluent acetic acid are mixed, the mass fraction of the diffusion particle zirconium dioxide is 1.5%, and the mass fraction of the diffusion particle silicon dioxide is 0.7%; after vacuum deoxygenation and nitrogen protection, after stirring at a speed of 50-300rpm for 1-3 hours, an inorganic oxide particle colloid is obtained.

[0129] 2. Coating and curing:

[0130] The inorganic oxide particle glue was coated on the composite film (film thickness 130 μm) through a slit coating to form a layer of inorganic oxide particle glue, and then irradiated with 390 nm UV light. At this time, the inorganic oxide particle glue was cured into an encapsulation film layer (5 μm) under UV light, forming a quantum dot light conversion film with a total thickness of 135 μm. The QY of the quantum dot light conversion film was 42% and the FWHM was 25.5 nm.

[0131] Example 5

[0132] 1. Preparation of the Second Quantum Dot Film Layer

[0133] 1. The preparation of quantum dot masterbatch is the same as that in Example 1.

[0134] 2. Film preparation: 560g PET particles, 100g red quantum dot masterbatch, 300g green quantum dot masterbatch, 20g diffused particle titanium dioxide (D50 is 0.15μm), 20g antioxidant 1024, using a single screw extruder with a screw diameter of 75mm and a screw speed of 32 rpm; heating temperature is 290℃; after co-extrusion die, rolling and pulling out to cool and shape, the second quantum dot film layer is obtained after the mold is cut, wherein the second quantum dot film layer has a thickness of 50μm, the mass fraction of red quantum dots in the film layer is 0.2%, and the mass fraction of green quantum dots in the film layer is 0.6%. The QY of the second quantum dot film layer is 37%, and the FWHM is 25.5nm.

[0135] 2. Second quantum dot film layer, first quantum dot film layer, base film composite

[0136] 1. Preparation of glue containing the first quantum dots

[0137] Green and red CdSe-based quantum dots (the quantum dots are the same as those in Example 1) dissolved in toluene, 89g of matrix resin methacrylic resin, 1g of diffusion particles TiO2 (D50 is 0.15μm), 0.1g of photoinitiator 819 and 10g of diluent acetic acid are mixed, the mass fraction of green quantum dots in the glue is 0.3%, and the mass fraction of red quantum dots in the glue is 0.7%; after vacuum deoxygenation and nitrogen protection, after stirring at a speed of 50-300rpm for 1-3 hours, a glue containing the first quantum dots is obtained.

[0138] 2. Preparation of composite membrane

[0139] The glue containing the first quantum dots was laminated to the PET base film with a barrier layer (base film thickness of 40 μm) and the second quantum dot film layer through slit coating, and then irradiated with 390 nm UV light. At this time, the glue layer containing the first quantum dots was cured under UV light to form the first quantum dot film layer (40 μm), forming a composite film with a total thickness of 130 μm.

[0140] 3. Preparation of encapsulation film

[0141] 1. Preparation of inorganic oxide particle colloid

[0142] 77.6g of base resin methacrylic resin, 10g of butyl acrylate, 1.5g of diffusion particle zirconium dioxide (D50 is 0.3μm), 0.7g of diffusion particle silicon dioxide (D50 is 0.4μm), 0.2g of photoinitiator 819 and 10g of diluent acetic acid are mixed, the mass fraction of the diffusion particle zirconium dioxide is 1.5%, and the mass fraction of the diffusion particle silicon dioxide is 0.7%; after vacuum deoxygenation and nitrogen protection, after stirring at a speed of 50-300rpm for 1-3 hours, an inorganic oxide particle colloid is obtained.

[0143] 2. Coating and curing:

[0144] A layer of inorganic oxide particle glue was applied on the composite film (film thickness 130 μm) by slit coating, and then irradiated with 390 nm UV light. At this time, the inorganic oxide particle glue was cured into an encapsulation film layer (5 μm) under UV light, forming a quantum dot light conversion film with a total thickness of 135 μm. The QY of the quantum dot light conversion film was 42.5% and the FWHM was 24.5 nm.

[0145] Comparative Example 1

[0146] Preparation of quantum dot light conversion film by coating method

[0147] 1. Preparation of glue containing quantum dots:

[0148] Green and red CdSe-based quantum dots (the quantum dots are the same as those in Example 1) dissolved in toluene, 89 g of methacrylic resin, 1 g of diffused particles TiO2 (D50 is 0.5 μm), 0.1 g of photoinitiator 819 and 10 g of diluent acetic acid are mixed, wherein the mass fraction of green quantum dots in the glue is 0.22%, and the mass fraction of red quantum dots in the glue is 0.22%;

[0149] 2. Coating and curing

[0150] The glue containing quantum dots was bonded to two PET base films with barrier layers (same as in Example 1, single film thickness was 20 μm) by slit coating, and then irradiated with 390 nm UV light. At this time, the middle glue layer was cured into a quantum dot layer (thickness was 60 μm) under UV light, forming a quantum dot light conversion film with a total thickness of 100 μm. The QY of the quantum dot light conversion film was 36% and the FWHM was 26 nm.

[0151] Comparative Example 2

[0152] Preparation of Quantum Dot PET Film by Extrusion

[0153] 1. Preparation of quantum dot masterbatch is the same as in Example 1

[0154] 2. Film preparation: 775g PET particles, 100g red quantum dot masterbatch, 100g green quantum dot masterbatch, 20g diffused particle titanium dioxide (D50 is 0.4μm), 5g antioxidant 1010 were prepared, and a single screw extruder with a screw diameter of 75 mm was used, and the screw speed was 30 rpm; the heating temperature was 275°C; after the co-extrusion die, the roll was pulled out and cooled to shape, and the mold was cut to obtain a quantum dot PET film, wherein the quantum dot PET film thickness was 100μm, the mass fraction of red quantum dots in the film layer was 0.13%, and the mass fraction of green quantum dots in the film layer was 0.13%. The QY of the quantum dot PET film was 35%, and the FWHM was 26nm.

[0155] The red quantum dots, green quantum dots and base films used in the comparative examples and embodiments are the same. The results of the embodiments and comparative examples are shown in Table 1. |△Y|max or |△X|max represents the color point non-uniformity, which is tested before the film aging experiment begins. The color point uniformity, quantum efficiency and film hardness tests are all tested in accordance with national standards; the aging test conditions are: temperature 60°C, relative humidity 90%, and light power 20W / m 2 , brightness and color point change trends see Figure 3 ,, the brightness decrease and color point change trend of Example 1 are the slowest. As can be seen from the table below, the stability of Example 1 is higher than that of Comparative Example 1, and all aspects of performance are better. The color point uniformity of Comparative Example 2 is worse, and because the quantum dots are not well protected, the stability of the film is poor.

[0156] Table 1

[0157]

[0158]

[0159] The above description is only a preferred embodiment of the present disclosure and is not intended to limit the present disclosure. For those skilled in the art, the present disclosure may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present disclosure shall be included in the protection scope of the present disclosure.

Claims

1. A quantum dot light conversion film, It is characterized in that The invention comprises a base film, a first quantum dot film layer, a second quantum dot film layer and a packaging film layer which are arranged in contact with each other in sequence; the base film comprises a barrier film layer and a PET film layer, and the barrier property of the base film is WVTR≤2g / m 2 · day; the first quantum dot film layer includes first quantum dots and a first resin, the second quantum dot film layer includes second quantum dots and polyethylene terephthalate, the encapsulation film layer includes a second resin and inorganic oxide particles, the first quantum dots and the second quantum dots are selected from one or both of red quantum dots and green quantum dots; the mass fraction of the red quantum dots and the green quantum dots in the first quantum dot film layer is 0.01-1% in total.

2. The quantum dot light conversion film according to claim 1, It is characterized in that The refractive index of the first resin is lower than that of the PET film layer, the refractive index of the first resin is between 1.38 and 1.6, and the refractive index of the packaging film layer is higher than that of the first resin.

3. The quantum dot light conversion film according to claim 1, It is characterized in that The mass fraction of the red quantum dots and the green quantum dots in the second quantum dot film layer is 0.01-20% in total, preferably 0.1-10%; preferably, the first quantum dot film layer and the second quantum dot film layer further comprise second diffusion particles.

4. The quantum dot light conversion film according to claim 1, It is characterized in that The thickness of the first quantum dot film layer is 1 to 100 μm, preferably 3 to 70 μm; the thickness of the second quantum dot film layer is 6 to 250 μm, preferably 12 to 125 μm.

5. The quantum dot light conversion film according to claim 1, It is characterized in that The thickness of the base film is 12 to 125 μm, and the thickness of the encapsulation film layer is 0.5 to 25 μm; preferably, the thickness of the quantum dot light conversion film is 37.5 to 75 μm.

6. The quantum dot light conversion film according to claim 1, It is characterized in that The second resin material includes one or more of acrylic resin, epoxy resin, and silicone resin, and the inorganic oxide particles are selected from one or more of zirconium oxide, titanium oxide, and silicon oxide.

7. The quantum dot light conversion film according to claim 1, It is characterized in that The fluorescence half-peak width of the first quantum dot film layer is less than or equal to 25nm, and the external quantum efficiency is greater than or equal to 40%, and / or the fluorescence half-peak width of the second quantum dot film layer is greater than or equal to 25nm, and the external quantum efficiency is less than 40%.

8. A method for preparing the quantum dot light conversion film according to any one of claims 1 to 7, It is characterized in that The method comprises melt coextruding a composition containing the second quantum dots and particles of polyethylene terephthalate to obtain a single-layer or multi-layer second quantum dot film layer; preparing the base film and the glue containing the first quantum dots; using a coating device to coat the glue containing the first quantum dots between the base film and the second quantum dot film layer, and curing to obtain an intermediate, wherein the intermediate comprises the base film, the first quantum dot film layer and the second quantum dot film layer which are arranged in contact with each other in sequence; coating the glue containing the inorganic oxide particles on the second quantum dot film layer, and curing to obtain the encapsulation film layer, and finally obtaining the quantum dot light conversion film.

9. The method for preparing the quantum dot light conversion film according to claim 8, It is characterized in that The second quantum dot-containing composition comprises red quantum dot masterbatch, green quantum dot masterbatch, diffusion masterbatch, stabilizer and antioxidant.

10. A backlight module, It is characterized in that The invention comprises the quantum dot light conversion film as described in any one of claims 1 to 7.

Citation Information

Patent Citations

  • Quantum-dot film with low cadmium content and preparation method and application thereof

    CN108666404A

  • Quantum dot film, and preparation method and application thereof

    CN112596299A

  • Color conversion layer, manufacturing method thereof, and display panel

    US20200251675A1

  • Light conversion film comprising a quantum dot layer, backlight units for display devices including the light conversion film, and method of manufacturing a quantum dot dispersion

    US20210013382A1