Method for printing heterostructured materials by a combined slip surface,

The sliding surface is prepared on the polytetrafluoroethylene microporous filter membrane through combined sliding surface printing technology, and the thermoelectric materials are assembled using vacuum filtration technology, which solves the problems of complex assembly process and high cost of existing thermoelectric materials and achieves Efficient, low-cost production of heat sensing and collection devices, suitable for thermal sensors and thermoelectric generators.

CN118789956AActive Publication Date: 2024-10-18QILU UNIVERSITY OF TECHNOLOGY (SHANDONG ACADEMY OF SCIENCES)
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202410803293.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-20
Publication Date
2024-10-18
Estimated Expiration
2044-06-20

AI Technical Summary

Technical Problem

The assembly process of existing thermoelectric materials is complex and costly, making it difficult to achieve mass production, patterning and flexible applications.

Method used

A combined sliding surface printing method is used to prepare a sliding surface on the surface of a polytetrafluoroethylene microporous filter membrane through direct writing printing technology. Combined with vacuum filtration technology, the patterned assembly of two thermoelectric materials is achieved to form a heterogeneous structural material. .

Benefits of technology

It simplifies the assembly process of thermoelectric materials, reduces production costs, achieves uniform distribution and high uniformity of heterogeneous structural materials, improves the durability and sensitivity of heat sensing and collection devices, and is suitable for mass production of thermal sensors and thermoelectric generators. .

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118789956A_ABST
    Figure CN118789956A_ABST
Patent Text Reader

Abstract

The invention provides a method for printing a heterostructure material through a combined sliding surface, the heterostructure material and a heat sensing and collecting device, and relates to the field of heterostructure material preparation. Wherein the heterostructure material is prepared in a vacuum filtration mode through a method of combining a movable slippage surface and a fixed slippage surface, and the preparation method specifically comprises the following steps: S1, preparing polydimethylsiloxane prepolymer ink; s2, preparing a fixed sliding surface; s3, preparing a movable sliding surface; s4, carrying out controllable patterning assembly on the first thermoelectric material; and S5, carrying out controllable patterning assembly on the second thermoelectric material and forming a heterostructure material. According to the method for printing the heterostructure materials on the combined sliding surface, the two heterostructure materials are assembled in a vacuum suction filtration mode, the preparation process is simple and convenient, the production cost is low, and the requirement of large-scale batch production can be met.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of preparation of heterogeneous structural materials, and in particular to a method for printing heterogeneous structural materials through a combined sliding surface, heterogeneous structural materials and heat sensing and collecting devices. Background Art

[0002] The slip surface is a material surface with special functions, which has been widely used in anti-icing, anti-fouling, microfluid transport and other aspects. At present, the methods for preparing slip surfaces are limited to etching, surface grafting, etc., but they are usually costly, require complex operations, and process the entire surface, and cannot achieve patterned applications. The present invention uses polydimethylsiloxane (PDMS) as the ink for preparing the slip surface, and uses direct writing printing to prepare the slip surface on the surface of polytetrafluoroethylene microporous filter membrane (PTFE). By controlling the printing parameters, curing conditions, etc., the influence of the wetting ridge on the flexible surface is reduced, and a slip surface with good slip performance is prepared. And through strong acid corrosion and high temperature experiments, it is proved that the slip surface prepared by this method has the advantages of stability and reusability. The successful preparation of the direct writing printing slip surface provides a new low-cost and high-flexibility method for patterned slip surfaces, and provides a reliable reference for assembling patterned nanomaterials.

[0003] Thermoelectric generators can generate electricity under temperature gradients. This is a pollution-free method of generating electricity that can generate useful electricity from waste heat or solar radiation and has broad application prospects. Thermoelectric materials usually need to be mixed with polymers or organic compounds to obtain flexible and independent thermoelectric devices. Although some studies have promoted paper as a flexible substrate for electronic devices, assembly into thermoelectric devices requires assembly methods through cutting and pasting. Currently, widely used thermoelectric materials such as metal tellurium, metal tellurides and selenides are usually expensive. It is difficult to avoid material waste in the later cutting and connecting process. The preparation process is complicated, the cost is high, and it is difficult to achieve mass production. There is an urgent need to study new preparation processes. Summary of the invention

[0004] In view of the problems existing in the prior art, the present invention provides a method for printing heterogeneous structure materials through a combined sliding surface, wherein a movable sliding surface for direct writing printing is adhered to a fixed sliding surface for direct writing printing, and the position covered by the movable sliding surface is moved to realize the confined deposition of a heterogeneous structure of two different materials on a surface.

[0005] In a first aspect of the present invention, a method for printing a heterogeneous structure material by a combined sliding surface is provided, wherein the heterogeneous structure material is prepared by a vacuum filtration method by combining a movable sliding surface and a fixed sliding surface, and specifically comprises the following steps:

[0006] S1. Preparing polydimethylsiloxane prepolymer ink: weighing polydimethylsiloxane prepolymer and curing agent according to a set ratio, stirring at room temperature for 10-20 minutes, putting into a vacuum drying oven, and then preserving in vacuum for a set time to obtain polydimethylsiloxane prepolymer ink;

[0007] S2. Prepare a fixed sliding surface: Use 50-100W O 2 Plasma treatment is performed for 5-10 minutes, the treated polytetrafluoroethylene microporous filter membrane is fixed on a direct writing printing operation table as a printing substrate, the polydimethylsiloxane prepolymer ink is injected into an ink container, and printing is performed according to a preset printing step under a printing pressure of 0-50 psi, and the printed product is placed on a constant temperature heating table and heated until the polydimethylsiloxane prepolymer ink is solidified to obtain a fixed sliding surface;

[0008] S3, preparing a movable sliding surface: placing a polyester film and a trimethoxyfluorosilane liquid in a vacuum drying dish for pretreatment, printing on the pretreated polyester film plate and placing it on a heating table to heat until the polydimethylsiloxane prepolymer ink is solidified, and separating the movable sliding surface from the polyester film plate to obtain a movable sliding surface;

[0009] S4, controllable patterned assembly of the first thermoelectric material: according to the patterning requirements, the movable slip surface prepared in step S3 is attached to the fixed slip surface prepared in step S2 and fixed on the funnel, and after being fully wetted, the first dispersed solution is poured into the funnel for vacuum filtration to complete the controllable patterned assembly of the first thermoelectric material to obtain a combined slip surface with the first thermoelectric material;

[0010] S5. The second thermoelectric material is controllably patterned and assembled to form a heterostructure material: the movable sliding surface prepared in step S3 is moved to the area partially covered by the first thermoelectric material on the combined sliding surface with the first thermoelectric material prepared in step S4 and fixed on the funnel. After sufficient wetting, the second dispersed solution is poured into the funnel for vacuum filtration. The second thermoelectric material is controllably patterned and assembled to form a heterostructure material.

[0011] Preferably, the first setting ratio is a weight ratio and the ratio is 10:1, and the first setting time is 30±5min.

[0012] Preferably, in step S1, the polydimethylsiloxane prepolymer and the curing agent are mixed to undergo a cross-linking reaction, and the pressure of the vacuum drying oven is 0.5-1 MPa.

[0013] Preferably, in step S2, the pore size of the polytetrafluoroethylene microporous filter membrane is adjusted according to the size of the dispersed phase particles of the first dispersed solution and the second dispersed solution, the needle diameter used in the printing process is selected according to the resolution requirement of the printed pattern, and the funnel is a sand core funnel.

[0014] Preferably, in step S2, the heating temperature of the heating table is 85-90°C, the drying temperature of the drying oven is 85-90°C, and the drying time is 12-13h.

[0015] Preferably, in step S2, the size of the polyester film plate is 6×6 cm 2 The pretreatment is to evacuate the vacuum drying dish into a vacuum state and place it in a drying oven, heat it at 90±5°C for 10-12h, and place it in a container filled with ethanol for ultrasonic cleaning for 5-10min.

[0016] Preferably, the first dispersion solution and the second dispersion solution are matrix solutions of heterogeneous structural materials, and the first dispersion solution and the second dispersion solution are deionized water, ethanol or methane.

[0017] A second aspect of the present invention provides a heterostructure material, which is prepared by a combined sliding surface printing method for heterostructure materials.

[0018] The third aspect of the present invention provides a heat sensing and collecting device containing the heterogeneous structure material, wherein the heat sensing and collecting device contains the heterogeneous structure material, and the heat sensing and collecting device is a PN alternating thermoelectric generator and a thermal sensor.

[0019] Preferably, when preparing the heterostructure material, the PN alternating thermoelectric generator uses an N-type selenium-doped bismuth telluride dispersion solution as the first dispersion solution and a P-type antimony telluride dispersion solution as the second dispersion solution to prepare the PN alternating thermoelectric generator.

[0020] Compared with the prior art, the present invention has the following advantages:

[0021] 1. The present invention adopts a method for printing heterogeneous structural materials by combined sliding surface, and assembles two heterogeneous structural materials by vacuum filtration. The preparation process is simple, the production cost is low, and the requirements of large-scale batch production can be met.

[0022] 2. The present invention adopts a method for printing heterogeneous structural materials through a combined sliding surface. The movable sliding surface of direct writing printing cooperates with the fixed sliding surface to form a heterogeneous structure with two materials evenly distributed in a surface confinement, and the heterogeneous structural material prepared by this method has good uniformity.

[0023] 3. The heat sensing and collecting device prepared by the combined sliding surface printing heterogeneous structure material method of the present invention has excellent durability and stability. The resistance change of the heat sensing and collecting device after 6000 times of bending with a displacement of 15mm is less than 0.2.

[0024] 4. The heat sensing and collection device prepared by the combined sliding surface printing heterogeneous structure material method of the present invention has high sensitivity and a wide temperature response range, and can be used to prepare thermal sensors or thermoelectric generators. Through practical application tests, when the heat sensing and collection device responds to finger touch as a thermal sensor, the response time is 0.452s and the recovery time is 0.421s. The heat sensing and collection device can respond to human body temperature and hot water temperature, and has a wide temperature response range.

[0025] 5. The heat sensing and collecting device prepared by the combined sliding surface printing heterogeneous structure material method of the present invention is assembled into a thermoelectric generator, which can generate an open circuit voltage under the action of the temperature difference between the cold and hot ends. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 It is a schematic diagram of the overall process of the present invention;

[0027] Figure 2 It is a schematic diagram of a specific method flow of the present invention;

[0028] Figure 3 Schematic diagram of the thermoelectric mechanism of the PN heterostructure material of the present invention;

[0029] Figure 4 The present invention is a method for printing heterogeneous structure materials by combined sliding surface, and the printing needles with diameters of 100 μm, 150 μm and 300 μm are used to print, and the relationship between the crosslinking time of the polydimethylsiloxane prepolymer ink and the minimum printing pressure is shown;

[0030] Figure 5a-Figure 5b The infrared spectra of the polydimethylsiloxane prepolymer ink used in the method of printing heterogeneous structure materials through a combined sliding surface of the present invention at different curing times; wherein, Figure 5a This is the infrared spectrum at the beginning of curing. Figure 5b This is the infrared spectrum of curing for more than 10 minutes;

[0031] Figure 6a-6d The present invention is a method for printing heterogeneous structural materials through a combined sliding surface, wherein the sliding surface with different curing degrees and the morphology of deionized water at the moment of dripping are used; wherein, Figure 6a The morphology of deionized water droplets falling on the uncured sliding surface. Figure 6b The morphology of the slip surface dropped on 85℃ and cured for 1min. Figure 6c The morphology of the sliding surface cured at 85℃ for 2min. Figure 6d The morphology of the sliding surface of the drop cured at 85℃ for 10min

[0032] Figure 7a-7d The morphology diagram of the contact angle between the sliding surface with different curing degrees and the deionized water drop after a certain period of time; Figure 7a This is the morphology of the contact angle between the uncured sliding surface and deionized water droplets after a certain period of time. Figure 7b and Figure 7c They are the morphological diagrams of the contact angles of the sliding surface after curing for a certain time and the deionized water droplets after a certain time. Figure 7d The morphology diagram is the contact angle between the fully cured sliding surface and the deionized water drop after a certain period of time;

[0033] Figure 8a-8c The present invention is a scanning electron microscope image of a sliding surface and a sample during the application of the method for printing heterogeneous structure materials by combined sliding surface; wherein, Figure 8a It is a fixed sliding template; Figure 8b It is a P-type structural unit; Figure 8c It is a PN type structural unit; Figure 8d-8f Optical microscope morphology images of the interface between polydimethylsiloxane prepolymer ink and N-type unit and P-type unit respectively;

[0034] Figure 9a-9e The present invention is a scanning electron microscope image and an X-ray spectrum test image (EDS) of the N unit of the heat sensing and collecting device in the application of the method of printing heterogeneous structure materials by combined sliding surface, wherein: Figure 9a is the SEM image of N unit; Figure 9b is the element mapping diagram of Bi in N unit; Fig.9c Figure d is the element mapping diagram of Se in N unit; Figure e is the EDS spectrum of N unit;

[0035] Figure 10a-Figure 10d The present invention is a scanning electron microscope image and an X-ray spectrum test image (EDS) of the P unit of the heat sensing and collecting device in the application of the method for printing heterogeneous structure materials by combined sliding surface, wherein: Fig.10a is the SEM image of the P unit; Fig.10b is the element mapping diagram of Bi in P unit; Fig.10c Figure d is the EDS spectrum of the P unit;

[0036] Figure 11a-Figure 11d The invention is to test the bending performance of the heat sensing and collecting device in the application of the method of printing heterogeneous structure materials by combined sliding surface of the present invention;

[0037] Figure 12a-12d Thermoelectric performance test of heat sensing and collecting devices in the application of the method of printing heterogeneous structure materials by combined sliding surface of the present invention;

[0038] Figure 13a-13d It is a practical application test of the heat sensing and collecting device as a thermoelectric generator in the application of the method of printing heterogeneous structure materials by combined sliding surface of the present invention;

[0039] Fig.14 This is a practical application test of the heat sensing and collecting device as a thermal sensor in the application of the method of printing heterogeneous structure materials through combined sliding surface of the present invention. DETAILED DESCRIPTION

[0040] In order to fully describe the technical content, objectives and effects of the present invention, the following will be described in detail with reference to the accompanying drawings.

[0041] like Figure 1 and Figure 2 As shown, on the one hand, the present invention provides a method for printing a heterogeneous structure material by a combined sliding surface, wherein the heterogeneous structure material is prepared by a vacuum filtration method by combining a movable sliding surface and a fixed sliding surface, and specifically comprises the following steps:

[0042] S1. Prepare polydimethylsiloxane prepolymer ink: weigh polydimethylsiloxane prepolymer and curing agent according to the set ratio, stir at room temperature for 10-20 minutes, put into a vacuum drying oven, and then store in vacuum for a set time to obtain polydimethylsiloxane prepolymer ink. Among them, the first set ratio is a weight ratio and the ratio is 10:1, and the first set time is 30±5min. After the polydimethylsiloxane prepolymer and the curing agent are mixed, a cross-linking reaction occurs, and the pressure of the vacuum drying oven is 0.5~1Mpa.

[0043] S2. Prepare a fixed sliding surface: Use 50-100W O 2 After plasma treatment for 5-10 minutes, the treated polytetrafluoroethylene microporous filter membrane is fixed on a direct writing printing operation table as a printing substrate, polydimethylsiloxane prepolymer ink is injected into an ink container, and printing is performed according to a preset printing step at a printing pressure of 0-50 psi, and the printed product is placed on a constant temperature heating table and heated until the polydimethylsiloxane prepolymer ink is solidified to obtain a fixed sliding surface.

[0044] In a specific application embodiment, in step S2, the pore size of the polytetrafluoroethylene microporous filter membrane is adjusted according to the size of the dispersed phase particles of the first dispersed solution and the second dispersed solution, the needle diameter used in the printing process is selected according to the resolution requirement of the printed pattern, and the funnel is a sand core funnel.

[0045] In a specific application embodiment, in step S2, the heating temperature of the heating table is 85-90°C, the drying temperature of the drying oven is 85-90°C, and the drying time is 12-13h.

[0046] S3. Preparing a movable sliding surface: placing a polyester film and trimethoxyfluorosilane liquid in a vacuum drying dish for pretreatment, printing on the pretreated polyester film plate and placing it on a heating table to heat until the polydimethylsiloxane prepolymer ink is solidified, and separating the movable sliding surface from the polyester film plate to obtain a movable sliding surface.

[0047] In a specific application embodiment, in step S3, the size of the polyester film plate is 6×6 cm 2 The pretreatment is to evacuate the vacuum drying dish into a vacuum state and place it in a drying oven, heat it at 90±5℃ for 10-12h, and place it in a container filled with ethanol for ultrasonic cleaning for 5-10min.

[0048] S4. Controllable patterned assembly of the first thermoelectric material: according to the patterning requirements, the movable slip surface prepared in step S3 is bonded to the fixed slip surface prepared in step S2 and fixed on the funnel. After sufficient wetting, the first dispersed solution is poured into the funnel and vacuum filtered to complete the controllable patterned assembly of the first thermoelectric material to obtain a combined slip surface with the first thermoelectric material.

[0049] S5. The second thermoelectric material is controllably patterned and assembled to form a heterostructure material: the movable sliding surface prepared in step S3 is moved to the area partially covered by the first thermoelectric material on the combined sliding surface with the first thermoelectric material prepared in step S4 and fixed on the funnel. After sufficient wetting, the second dispersed solution is poured into the funnel for vacuum filtration. The second thermoelectric material is controllably patterned and assembled to form a heterostructure material.

[0050] In a specific application embodiment, the first dispersed solution and the second dispersed solution are matrix solutions of the heterogeneous structure material, and the first dispersed solution and the second dispersed solution are deionized water, ethanol or methane.

[0051] A second aspect of the present invention provides a heterostructure material, which is prepared by a combined sliding surface printing method for heterostructure materials.

[0052] The third aspect of the present invention provides a heat sensing and collecting device containing a heterogeneous structure material, the heat sensing and collecting device contains a heterogeneous structure material, and the heat sensing and collecting device is a PN alternating thermoelectric generator. When preparing the heterogeneous structure material, the PN alternating thermoelectric generator uses a dispersion solution of N-type selenium-doped bismuth telluride as a first dispersion solution and a P-type antimony telluride dispersion solution as a second dispersion solution to prepare the PN alternating thermoelectric generator. Figure 3 A schematic diagram of the thermoelectric mechanism of the PN heterostructure material of the present invention is shown.

[0053] The method and application of printing heterogeneous structure materials by combined sliding surface of the present invention are further described below in conjunction with the embodiments:

[0054] Example 1: Printability test of polydimethylsiloxane prepolymer ink.

[0055] The polydimethylsiloxane prepolymer and the curing agent were mixed in a mass ratio of 10:1, stirred for 20 minutes at room temperature, and then placed in a vacuum drying oven, and stored in a vacuum at a pressure of 1.0 MPa for 0.5 hours to eliminate bubbles, thereby obtaining a polydimethylsiloxane prepolymer ink.

[0056] A 0.22 μm pore size polytetrafluoroethylene microporous filter was used with 100 W of O 2 Plasma treatment for 5 minutes to improve its wettability, and then fixed it on the direct writing printing operation table, PDMS was cross-linked at room temperature for 1h, 2h, 3h, 4h, 5h, and 6h, and then injected into the ink container, using 100μm, 150μm, and 300μm diameter printing needles, and printing was performed according to the set printing program at the minimum printing pressure. After the printing process, a constant temperature heating table was used to heat at 85℃ for 15 minutes to gradually solidify the PDMS and obtain a slip surface.

[0057] Example 2: The polydimethylsiloxane prepolymer and the curing agent were mixed in a mass ratio of 10:1, stirred for 20 minutes at room temperature, and then placed in a vacuum drying oven, and stored in a vacuum oven at a pressure of 1.0 MPa for 0.5 hours to eliminate bubbles, thereby obtaining a polydimethylsiloxane prepolymer ink.

[0058] The 0.22 μm pore size polytetrafluoroethylene microporous membrane was used with 100 W O 2Plasma treatment was performed for 5 min to improve its wettability, and it was fixed on the direct writing printing operation table. The PDMS was cross-linked at room temperature for 1 h, 2 h, 3 h, 4 h, 5 h, and 6 h, respectively, and then injected into the ink container. Printing was performed using 100 μm, 150 μm, and 300 μm diameter printing needles at the minimum printing pressure according to the set printing program. After the printing process was completed, a constant temperature heating table was used to heat at 85 ° C for 15 min to gradually solidify the PDMS and obtain a slip surface. The PET plate was cut into 6×6 cm 2 Size, place in a container filled with ethanol and ultrasonically clean for 5 minutes. Add 20μL of trimethoxy (1H, 1H, 2H, 2H-heptadecafluorodecyl) silane dropwise in a vacuum drying dish, and place the cleaned PET in a vacuum drying dish, evacuate the device and heat it in a drying oven at 90°C for 12 hours. Prepare polydimethylsiloxane prepolymer ink according to a weight ratio of 10:1, take out the treated PET, and print a patterned slip surface on its surface using direct writing printing as a removable mask. Place the prepared slip surface on a heating table and heat it at 85°C for 15 minutes to completely cure it. Separate the slip surface from the PET plate and fit it to the fixed slip surface according to the patterning requirements.

[0059] Weigh 100 mg of N-type bismuth telluride (Bi 2 Te 3 ) and 10 mg sodium carboxymethyl cellulose (CMC-Na), disperse the weighed mixture in 30 mL deionized water, and place it on a magnetic stirrer and stir it at a speed of 400 rpm for 40 minutes to obtain a mixed solution. The mixed solution is ultrasonically dispersed for 60 minutes using 100% power to fully disperse the solution to obtain an N-type bismuth telluride dispersion solution. Weigh 100 mg P-type antimony telluride (Sb 2 Te 3 ) and 10 mg sodium carboxymethyl cellulose, and the same method was used to prepare P-type antimony telluride (Sb 2 Te 3 ) dispersion solution.

[0060] The assembled slip surface is placed on the sand core funnel, and the air tightness of the device is tested with deionized water. The printed patterned slip surface is fixed on the sand core funnel, fully wetted, and the treated N-type dispersion solution is poured into the solution bottle for vacuum-assisted filtration assembly to obtain a slip surface with N-type thermoelectric material, and placed on a heating table at 70°C for 1h. Move the movable slip surface to cover the assembled N-type thermoelectric material part, and use the same method to assemble the P-type dispersion solution in the blank area. After drying, an integrated PN alternating thermoelectric generator is obtained.

[0061] According to the test steps of Example 1, the present invention uses printing needles with diameters of 100 μm, 150 μm and 300 μm to print, and tests the relationship between the crosslinking time of the polydimethylsiloxane prepolymer ink and the minimum printing pressure. The qualitative relationship between the curing degree, curing time and contact state of the sliding surface of Example 1 is tested; Example 2 is an application of the method of printing electrical heterostructure materials through a combined sliding surface of the present invention in a thermoelectric device. Scanning electron microscope characterization, optical microscope characterization, energy dispersive X-ray spectroscopy test, temperature difference power generation test, bending resistance test and heat perception and collection test are performed on Example 2. The specific conclusions are as follows:

[0062] Figure 4 The relationship between the crosslinking time and the minimum printing force of the polydimethylsiloxane prepolymer ink prepared in Example 1 is shown in the figure, wherein the horizontal axis is the crosslinking time and the vertical axis is the printing force. The components of the polydimethylsiloxane prepolymer and the curing agent are siloxane polymer and alkaline catalyst, respectively. After being fully mixed, the catalyst reacts with the silicon-hydrogen bonds in the prepolymer to promote crosslinking between siloxane chains, thereby forming a fixed network structure. As time goes by, the crosslinking degree of the ink gradually increases, so the printing parameters change continuously during the printing process. Figure 4 As shown, the printing pressure required for printing needles of different sizes at room temperature (~25°C) varies with the crosslinking time. When using a 100μm printing needle, the minimum printing pressure is between 13.5 and 55.5psi; when using a 150μm printing needle, the minimum printing pressure is between 6.0 and 29.5psi; when using a 300μm printing needle, the minimum printing pressure is between 0 and 6.4psi. At room temperature, polydimethylsiloxane prepolymer ink can maintain printability for a long period of time, and has good compatibility with the direct writing printing method. In addition, the dispensing system used in this embodiment can output a printing pressure between 0 and 99psi, and the minimum unit of printing pressure adjustment in the range of 0 to 16.9psi is 0.01psi. After it is greater than 16.9psi, the minimum unit of printing pressure adjustment is 0.5psi. Therefore, the control of polydimethylsiloxane prepolymer ink at a printing pressure lower than 16.9psi is more accurate.

[0063] Figure 5a-Figure 5b : is the infrared spectrum of the polydimethylsiloxane prepolymer ink prepared in Example 1 at different curing times, wherein the abscissa is the wavelength and the ordinate is the transmittance. Figure 5a As shown, the infrared spectrum of the PDMS layer is characterized by methyl groups, showing a -1 Asymmetric stretch at 2900cm -1 Symmetrical stretching vibration at 1266 cm -1 The sharper strong band belongs to Si-CH 3Symmetrical CH deformation vibration of the group (umbrella mode). 1423cm -1 and 1443cm -1 There are two deformation bands of CH at 1043cm -1 and 1112cm -1 The asymmetric stretching vibration of Si-O-Si appears at 790 cm -1 The band at is attributed to Si-C in Si-CH 3 In addition, due to the special ink properties of PDMS, slow crosslinking occurs at room temperature and the crosslinking speed is accelerated under heating conditions. The crosslinking reaction involves the connection between two H2C=CH- end groups and Si-H in the curing agent, so it appears at 2157cm -1 The strength of the Si-H groups at the PDMS can quantitatively reflect the degree of PDMS cross-linking. Figure 5b As shown in Figure 2, with the increase of curing time, the intensity of Si-H groups increases, indicating that more molecules participate in the cross-linking reaction, resulting in more polymer chains covalently bonded to other curing agents. When the curing time of the sliding surface is 10 min or more, the Si-H peak intensity does not change significantly, so the surface cured at 85 ° C for 10 min is defined as a fully cured surface.

[0064] Figure 6a-6d The morphology of deionized water dropped on surfaces with different curing degrees is recorded by a contact angle meter at the moment of dropping on the sliding surface. Figure 6a The morphology of deionized water droplets falling on the uncured sliding surface. Figure 6b The morphology of the slip surface dropped on 85℃ and cured for 1min. Figure 6c The morphology of the sliding surface cured at 85℃ for 2min. Figure 6d The morphology of the drop on the slip surface cured at 85℃ for 10min is shown in Figure 2. Figure 6a As shown in the figure, the contact angle of a water drop dropped on the uncured surface is small, and there are obvious wetting ridges at the front and rear contact lines. This is because the PDMS is in a liquid state under uncured conditions and is very easy to deform. A vertical component of surface tension is generated at the three-phase contact line between the droplet and the surface. The PDMS layer in this state cannot balance this vertical component without deformation, so a wetting ridge is generated at the contact line. The larger wetting ridges around the droplet will cause the liquid PDMS sliding layer to be exhausted, resulting in a decrease in liquid repellency. In addition, in this state, the droplet movement is in a sticky state, and the solute is not easy to leave the sliding part, resulting in more solutes being fixed in the sliding part during the vacuum filtration assembly process, resulting in poor patterning effect. Figure 6b-6dAs shown, with the increase of solidification time, the contact angle between the droplet and the sliding surface increases, and the wetting ridges before and after the droplet decrease and gradually disappear, indicating that during the solidification process, the interaction force between the liquid and the solid surface gradually decreases. When vacuum filtration assembly is performed on the fully solidified sliding surface, the solute will not be fixed after contacting the sliding surface, but tends to move and finally deposit on the blank part to form a patterned deposition. Figure 7a-7d This is a morphology diagram of deionized water drops falling on surfaces with different degrees of solidification after a certain period of time, and the morphology of the water droplets on the surface is recorded every ten minutes. Figure 7a As shown in Figure 2, the droplet has a more serious wetting ridge phenomenon on the uncured sliding surface, and it increases with the increase of residence time, indicating that the longer the residence time in this state, the more serious the damage to the liquid PDMS layer. Figure 7b-7d As shown in the figure, with the increase of curing degree, the wetting ridge gradually decreases and finally disappears. This phenomenon is similar to the verification results of the experiment in the previous section. Therefore, the fully cured sliding surface, that is, the sliding surface heated at 85℃ for 10min or more, will have a longer service life and is more suitable as a patterning template.

[0065] Figure 8a-8f The scanning electron microscope images of the sliding surface and the sample in Example 2 and the optical microscope morphology of the interface between the polydimethylsiloxane prepolymer ink and the N-type unit and the P-type unit are shown in Figure 2. In order to analyze the patterning effect of the movable sliding surface in detail, the sliding surface after direct writing printing is cured to obtain the following Figure 8a The fixed sliding surface shown; after the movable sliding surface is removed, the Figure 8b and Figure 8c The P-type structural unit and the PN-type structural unit shown in FIG. Figure 8e As shown in the figure, a clear boundary line is observed under a microscope between the printed part with polydimethylsiloxane prepolymer ink and the unprinted blank part, and the blank part on the right has certain pores, which can quickly filter the solution in the dispersed solution under the action of vacuum-assisted filtration, while the polydimethylsiloxane prepolymer ink is clearly observed on the left part to penetrate into the micropores of the filter membrane, with good barrier and slip properties. Figure 8e As shown, the P-type unit boundary is clear and there is no Sb in the PDMS part. 2 Te 3 Residue; After the second filtration, the following Figure 8f The N-type unit shown is at the junction with PDMS. The boundary of the N-type unit is clear, and there is no Sb in the PDMS part. 2 Te 3 and Bi 2 Te 3Therefore, the fixed sliding surface of direct writing printing forms an effective pattern in cooperation with the movable sliding surface, and has stability and can be used for multiple vacuum-assisted filtration.

[0066] 9-10 are energy dispersive X-ray spectra (EDS) of the N unit and P unit of the sample in Example 2, wherein the abscissa is the X-ray energy and the ordinate is the energy. Figures 9a-9d is the surface morphology in the N unit area and the element mapping results of Bi, Te and Se atoms, such as Fig.9e The EDS spectrum shows that the atomic composition of the N-type unit is: Bi atomic content is 54.76%, Te atomic content is 40.92%, and doped Se atomic content is 4.32%. Through EDS analysis, it can be determined that the material of the N-type unit is Se-doped Bi. 2 Te 3 Material. Figure 10a-10c The surface morphology and element mapping results of Sb and Te atoms in this area. Fig.10d This is the EDS spectrum of the P-type unit. The atomic content ratio in the illustration shows that the Sb atomic content is 39.22% and the Te atomic content is 60.78%. Through EDS testing, it can be determined that the material of the P-type unit is pure Sb 2 Te 3 Materials, heat sensing and collection devices are heterogeneous structures.

[0067] Figure 11a-Figure 11d To test the bending performance of heat sensing and collection devices, such as Fig.11a As shown, the deposited Sb 2 Te 3 and Bi 2 Te 3 The material does not warp or break under large bending conditions and has high flexibility. However, in order for thermoelectric devices to utilize this property for a long time, sustainable performance must be demonstrated through multiple cycle simulations. Fig.11b and Fig.11c As shown, the two ends of the thermoelectric device are fixed on the reciprocating motor and the displacement is set to 15 mm. Fig.11c The bending state of the device is simulated through continuous bending and recovery process to simulate the use of flexible devices. Fig.11d As shown in Figure 2, the resistance change of the thermoelectric device increases slowly with the increase of the number of bends. The bending resistance change within 6000 bends is less than 0.2, indicating that the Sb deposited on the surface during the bending process 2 Te 3 and Bi 2 Te 3 The material is in a stable state on the substrate without serious fracture, and the device exhibits good electrical stability and durability.

[0068] Figure 12a-12d To test the thermoelectric performance of heat sensing and collection devices, due to the different properties of P-type semiconductors and N-type semiconductors, when a temperature difference occurs at both ends of a PN structure unit, the holes in the P-type semiconductor move from the hot end to the cold end, showing a thermoelectric potential from the high temperature end to the low temperature end; while the free electrons in the N-type semiconductor move from the hot end to the cold end, showing a thermoelectric potential from the low temperature end to the high temperature end. By using Fig.12a The experimental device shown in the figure tests the power generation performance of a thermoelectric generator containing a PN structural unit. One end of the thermoelectric device is heated by the metal material in the red box and used as the hot end. The position in the blue box is suspended, and a layer of insulation material is pasted between the glass sheet and the device as the cold end. Figure 12b The side view of the experimental device is shown in Figure 2. The prepared PN alternating generator senses the temperature difference between the two ends under the action of the Seebeck effect and converts heat into electrical energy. First, the thermoelectric device containing a pair of PN structures was tested. The results are shown in Figure 2. Fig.12c As shown in the figure, an open circuit voltage of 0.2mV is generated at a temperature difference of 5K. The open circuit voltage is linearly related to the temperature difference at both ends. When the temperature difference increases to 65K, a voltage of 1.97mV is generated. The open circuit voltages generated by the three pairs of PN structures as the temperature difference changes are shown in the figure. Fig.12d As shown, an open circuit voltage of 0.9 mV is generated at a temperature difference of 5 K, and a maximum voltage of 6 mV is generated when the temperature difference is increased to 65 K. Although more PN structures mean that more PN contact points are required, there is no phenomenon of reduced thermoelectric performance. This is because the thermoelectric materials assembled by vacuum filtration are evenly distributed on the substrate, and the open circuit voltage generated is comparable to the output of flexible devices reported in previous literature. The PN alternating units are connected by patterning and vacuum-assisted filtration, so no additional cutting and assembly are required, which has special advantages in the size design and easy manufacturing of the overall device.

[0069] Figure 13a-13d The heat sensing and collecting devices prepared in Example 2 were used as practical application tests of thermoelectric generators. Three pairs of heat sensing and collecting devices were packaged to form a thermoelectric generator assembly. The packaged thermoelectric generator was attached to the arm. Fig.13a and Fig.13b As shown in the figure, a stable voltage of 0.9mV is generated after contact with the arm; Fig.13c and Fig.13d The thermoelectric generator that had been treated in the same way was placed above a beaker filled with 100°C hot water. After sensing the heat source, the generator generated an open-circuit voltage of 38.1mV. The experiment showed that the open-circuit voltage has a wide temperature detection range and has application potential as a heat source detection. It is expected to be used in self-powered environmental monitoring to avoid natural disasters such as fire.

[0070] Fig.14 The heat sensing and collecting device prepared in Example 2 is used as a practical application test of a heat sensor. Fig.14 Part a shows the voltage response of the heat sensing and collection device under the touch of a finger. The frequency of finger contact and removal is controlled to be 1 second each time. The test results show that the open circuit voltage increases and decreases sharply with the touch of a finger, indicating that the device is very sensitive to changes in external temperature. Fig.14 Part b in the middle is an amplified display of the voltage change results within 15-20s, where the illustration is a schematic diagram of the operation of touching and removing the device. When the finger is fully pressed on one side of the device to heat it, the open circuit voltage of the paper reaches about 0.5mV. The response time refers to the time from the beginning of the finger touching to the maximum open circuit voltage, which is about 0.452s; the recovery time refers to the time from the finger leaving the device to the open circuit voltage returning to zero, which is about 0.421s. The maximum voltage of each cycle is inconsistent. This is because the temperature change caused by each finger touch is slightly different. The heat sensing and collection device as a paper-based thermal sensor can realize self-powered control of wearable electronic devices.

[0071] The embodiments described above are only descriptions of the preferred implementation modes of the present invention, and are not intended to limit the scope of the present invention. Without departing from the design spirit of the present invention, various modifications and improvements made to the technical solutions of the present invention by ordinary technicians in this field should all fall within the protection scope determined by the claims of the present invention.

Claims

1. A method for printing heterogeneous structure materials by combined sliding surface, characterized in that: The heterogeneous structure material is prepared by a vacuum filtration method by combining a movable sliding surface and a fixed sliding surface, which specifically includes the following steps: S1. Preparing polydimethylsiloxane prepolymer ink: weighing polydimethylsiloxane prepolymer and curing agent according to a set ratio, stirring at room temperature for 10-20 minutes, putting into a vacuum drying oven, and then preserving in vacuum for a set time to obtain polydimethylsiloxane prepolymer ink; S2. Preparing a fixed slip surface: treating a polytetrafluoroethylene microporous filter membrane with 50-100W O2 plasma for 5-10 minutes, fixing the treated polytetrafluoroethylene microporous filter membrane on a direct writing printing operation table as a printing substrate, injecting the polydimethylsiloxane prepolymer ink into an ink container, printing according to a preset printing step at a printing pressure of 0-50psi, placing the printed product on a constant temperature heating table and heating it until the polydimethylsiloxane prepolymer ink is solidified, thereby obtaining a fixed slip surface; S3, preparing a movable sliding surface: placing a polyester film and a trimethoxyfluorosilane liquid in a vacuum drying dish for pretreatment, printing on the pretreated polyester film plate and placing it on a heating table to heat until the polydimethylsiloxane prepolymer ink is solidified, and separating the movable sliding surface from the polyester film plate to obtain a movable sliding surface; S4, controllable patterned assembly of the first thermoelectric material: according to the patterning requirements, the movable slip surface prepared in step S3 is attached to the fixed slip surface prepared in step S2 and fixed on the funnel, and after being fully wetted, the first dispersed solution is poured into the funnel for vacuum filtration to complete the controllable patterned assembly of the first thermoelectric material to obtain a combined slip surface with the first thermoelectric material; S5. Controllable patterned assembly of the second thermoelectric material to form a heterostructure material: the movable sliding surface prepared in step S3 is moved to the area partially covered by the first thermoelectric material on the combined sliding surface with the first thermoelectric material prepared in step S4 and fixed on the funnel. After sufficient wetting, the second dispersed solution is poured into the funnel for vacuum filtration to complete the controllable patterned assembly of the second thermoelectric material and form a heterostructure material.

2. The method for printing heterogeneous structure materials by combined sliding surface according to claim 1, characterized in that: The setting ratio is a weight ratio and the ratio is 10:1, and the setting time is 30±5min.

3. The method for printing heterogeneous structure materials by combined sliding surface according to claim 1, characterized in that: In step S1, the polydimethylsiloxane prepolymer and the curing agent are mixed to undergo a cross-linking reaction, and the pressure of the vacuum drying oven is 0.5-1 MPa.

4. The method for printing heterogeneous structure materials by combined sliding surface according to claim 1, characterized in that: In step S2, the pore size of the polytetrafluoroethylene microporous filter membrane is adjusted according to the size of the dispersed phase particles of the first dispersed solution and the second dispersed solution, the needle diameter used in the printing process is selected according to the resolution requirement of the printed pattern, and the funnel is a sand core funnel.

5. The method for printing heterogeneous structure materials by combined sliding surface according to claim 1, characterized in that: In step S2, the heating temperature of the heating table is 85-90°C, the drying temperature of the drying oven is 85-90°C, and the drying time is 12-13h.

6. The method for printing heterogeneous structure materials by combined sliding surface according to claim 1, characterized in that: In step S2, the size of the polyester film plate is 6×6 cm 2 The pretreatment is to evacuate the vacuum drying dish into a vacuum state and place it in a drying oven, heat it at 90±5°C for 10-12h, and place it in a container filled with ethanol for ultrasonic cleaning for 5-10min.

7. The method for printing heterogeneous structure materials by combined sliding surface according to claim 1, characterized in that: The first dispersion solution and the second dispersion solution are matrix solutions of heterogeneous structural materials, and the first dispersion solution and the second dispersion solution are deionized water, ethanol or methane.

8. A heterostructure material, characterized in that: The heterostructure material is prepared by the method for printing heterostructure materials by combined sliding surface as described in claim 1.

9. A heat sensing and collecting device comprising the heterogeneous structure material according to claim 8, characterized in that: The heat sensing and collecting device comprises the heterogeneous structure material, and the heat sensing and collecting device is a PN alternating thermoelectric generator.

10. The heat sensing and collecting device according to claim 9, characterized in that: The PN alternating thermoelectric generator uses N-type selenium-doped bismuth telluride dispersion solution as the first dispersion solution and P-type antimony telluride dispersion solution as the second dispersion solution when preparing the heterostructure material to prepare the PN alternating thermoelectric generator.

Citation Information

Patent Citations

  • Method of transferring a membrane image to an article in a membrane image transfer printing process

    CN1938159A

  • Inkjet printing on polycarbonate substrates

    EP3663095A1