Method for large-scale preparation of sulfide electrolyte for solid-state battery and all-solid-state lithium battery
Through the process of low-speed mixing, high-speed shearing and high-temperature calcination in a low dew point environment, the problems of complex sulfide electrolyte preparation process and unstable performance are solved, and efficient and stable sulfide electrolyte production is achieved, which is suitable for large-scale applications.
Patent Information
- Application Number
- CN202411287760.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-14
- Publication Date
- 2024-10-18
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The existing sulfide electrolyte preparation process is complex and has unstable performance. It needs to be carried out in a glove box environment, and solvent intervention leads to high energy consumption and low production efficiency, making it difficult to achieve large-scale mass production.
Using low-speed mixing, high-speed shearing and high-temperature calcination in a low dew point environment, combined with molding and crushing processes, the preparation of sulfide-silvergermanium ore-type sulfide electrolytes is achieved, avoiding solvent intervention and simplifying equipment requirements and production processes.
It realizes the continuous production of high-performance sulfide electrolytes, reduces environmental and equipment requirements, improves production efficiency, shortens time, has high ionic conductivity and stable particle size distribution, and is suitable for large-scale production.
Smart Images

Figure CN118791019A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of solid-state power batteries, and specifically relates to a method for large-scale preparation of sulfide electrolytes for solid-state batteries and an all-solid-state lithium battery. Background Art
[0002] Lithium-ion batteries have the characteristics of high energy density, long life, and low cost, and are widely used in the field of energy storage. At present, lithium-ion batteries mainly use electrolytes. Since this type of electrolyte is in liquid form, organic solvents are often used. Under certain conditions, it is easy to leak and cause fires, posing serious safety hazards. Based on the dual considerations of safety and energy density, the industry continues to make efforts to develop solid electrolytes as the next generation of lithium-ion batteries. Compared with liquid batteries, solid-state batteries will not leak electrolytes under the action of external forces to cause safety problems due to the solid electrolyte. At the same time, the structural simplification brought about by it further improves the energy density of solid-state batteries. The strong mechanical properties of solid-state electrolytes can also prevent the piercing of lithium dendrites.
[0003] Solid electrolytes mainly include oxide electrolytes, sulfide electrolytes, halide electrolytes and polymer electrolytes. Among them, sulfide electrolytes, due to the particularity of their crystal structure, are conducive to the diffusion and transmission of lithium ions, so they have higher ionic conductivity, and even under certain conditions, their ionic conductivity exceeds that of liquid electrolytes. Among sulfide electrolytes, argyrodite-type solid electrolytes not only have simple preparation processes and high ionic conductivity, but also have good electrochemical stability, good compatibility with lithium metal, and low cost. They are the most widely studied of sulfide solid electrolytes.
[0004] The current sulfide electrolyte preparation process is immature, complex, and unstable in performance. The entire process needs to be carried out in a glove box environment. At the same time, the mixing and refinement processes require long-term processing under solvent intervention conditions, resulting in many limiting factors in energy consumption, production efficiency, equipment requirements, etc., making it difficult to achieve mass production levels. The present invention optimizes the pain points in the production process of sulfide electrolytes for solid-state batteries, which can help the large-scale application of all-solid-state batteries. Summary of the invention
[0005] In view of the above problems, on the one hand, the present invention provides a method for large-scale preparation of sulfide electrolyte for solid-state batteries, which solves the technical problems in the existing production process of sulfide electrolyte for solid-state batteries and can realize large-scale mass production of sulfide electrolyte for solid-state batteries. On the other hand, the present invention proposes an all-solid-state lithium battery containing the sulfide electrolyte.
[0006] In order to achieve the above object, the technical solution adopted by the present invention is: The present invention provides a method for large-scale preparation of a sulfide electrolyte for solid-state batteries, wherein the sulfide electrolyte is an argyrodite-type sulfide electrolyte having a chemical composition of Li 6-x PS 5-x X 1+x-y Y y , wherein X, Y are selected from one or more of the halogen elements F, Cl, Br, I; the value range of x is 0 to 0.8; the value range of y is 0 to 0.7; the value range of x+y is 0 to 0.8; The method comprises the following steps: S1: In a low dew point environment, the Li source, S source, P source, X source and Y source are mixed at a low speed to obtain a primary powder; S2: In a low dew point environment, the primary powder is subjected to high-speed shearing for refinement to obtain secondary powder; S3: Under a low dew point environment, the secondary powder is molded into blocks to obtain a precursor material; S4: calcining the precursor material at high temperature in an inert gas environment, and crushing the product in a low dew point environment after the calcination is completed, so as to obtain the sulfide electrolyte.
[0007] Furthermore, the Li source is selected from any one or more of Li2S, Li2S2, LiCl, LiBr and LiI; the S source is selected from any one or more of P2S5, P4S9, Li2S and Li2S2; the P source is selected from any one or more of P2S5, P4S9, Li2S and Li2S2. 10 and P4S9; the X source and the Y source are selected from any one or more of LiF, LiCl, LiBr and LiI.
[0008] Furthermore, the low dew point environment has a dew point of -40°C to -80°C and a temperature of 0°C to 40°C.
[0009] Furthermore, the equipment used for low-speed mixing is selected from one or more of a high-speed mixer, a powder mill, a sand mill, and a ball mill; the rotation speed of the low-speed mixing process is 200 to 2000 rpm; the low-speed mixing time is 30 to 600 s; and the primary powder satisfies a particle size of 50 to 200 meshes.
[0010] Furthermore, the equipment used for high-speed shearing is selected from one or more of a high-speed mixer, a powder mill, a sand mill, and a ball mill; the rotation speed of the high-speed shearing process is 1000 to 10000 rpm; the high-speed shearing time is 30 to 600 s; and the secondary powder satisfies a particle size of 150 to 1000 mesh.
[0011] Furthermore, the equipment used in the molding process includes one or more of an automatic tablet press, an automatic molding machine, an automatic tablet forming machine, and a fully automatic desktop tablet press; the molding pressure is 1 to 20t, and the molding size is Φ10 to Φ300mm.
[0012] Furthermore, the inert gas environment includes one or more of an argon atmosphere, a nitrogen atmosphere, and a helium atmosphere; the precursor calcination temperature is 400 to 600° C., and the holding time is 2 to 20 hours.
[0013] Furthermore, the equipment used for crushing the calcined sample includes one or more of a high-speed powder grinder, a fine crusher, a powder crusher, and a powder wall breaker; and the crushing time is 10 to 300 seconds.
[0014] The present invention also provides an all-solid-state lithium battery, comprising a sulfide electrolyte prepared by the preparation method as described above.
[0015] Compared with the prior art, the technical solution of the present invention has the following beneficial effects: (1) The process of preparing primary powder by low-speed mixing, preparing secondary powder by high-speed shearing, and crushing the sample after calcination can be carried out in a low dew point environment. Due to the innovative production process and process design of the present invention, the product performance is consistent with that of the product produced in a traditional glove box environment, which greatly reduces the requirements for environment and equipment, and can be directly produced using the existing liquid battery production line; (2) After the raw materials are mixed at a low speed, due to electrostatic adsorption, the raw materials attract and cover each other, and the primary powder particle size is relatively large at this time; after high-speed shearing, the raw materials are refined to obtain secondary powders with smaller particle size and uniform mixing. At this time, calcination ensures a large contact area between different raw materials, allowing for full solid-phase reaction, and ultimately obtaining a sulfide electrolyte with high crystallinity, single crystal phase, and high ionic conductivity; (3) The secondary powder is continuously tableted with low pressure, and the final product performance is consistent with that of manual tableting with high pressure, but the efficiency is significantly improved. The present invention realizes the cycle process of rapid and continuous filling, molding, demolding, and refilling of secondary powder, ensuring the continuous production of sulfide electrolyte.
[0016] (4) In the process of preparing sulfide solid electrolytes in the prior art, the entire process needs to be carried out in a glove box environment. At the same time, the mixing and refinement processes require long-term processing under solvent intervention conditions, resulting in many limiting factors in energy consumption, production efficiency, equipment requirements, etc. In the process of preparing sulfide electrolytes in this application, solvent-free production is achieved, that is, the entire production process is free of solvents, which greatly shortens the production time, reduces equipment requirements, and significantly reduces energy consumption. At the same time, continuous operation can be achieved. The prepared sulfide electrolyte powder has a consistent particle size distribution and stable ionic conductivity, which can realize large-scale production of sulfide electrolytes for solid-state batteries.
[0017] In summary, the method for large-scale preparation of sulfide electrolytes for solid-state batteries provided by the present invention can be prepared in large quantities and also has high and stable ionic conductivity, and has broad application prospects. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] Figure 1 This is the particle size distribution diagram of Example 1.
[0019] Figure 2 Schematic diagram of the sulfide electrolyte test model.
[0020] Figure 3 This is the AC impedance curve (Nyquist curve) of Example 1.
[0021] Figure 4 This is the AC impedance curve (Nyquist curve) of Example 2.
[0022] Figure 5 This is the AC impedance curve (Nyquist curve) of Example 3.
[0023] Figure 6 This is the AC impedance curve (Nyquist curve) of Comparative Example 1.
[0024] Figure 7 1 is an equivalent circuit diagram of the impedance fitting process of Examples 1-3 and Comparative Example 1. DETAILED DESCRIPTION
[0025] To make the purpose, technical solution and advantages of the present invention clearer, the technical solution of the present invention will be described in detail below. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments. Based on the embodiments of the present invention, all other implementation methods obtained by ordinary technicians in this field without creative work belong to the scope of protection of the present invention.
[0026] It should be noted that the ionic conductivity test of the sulfide solid electrolyte is carried out by assembling Figure 2Specifically, a certain mass of sulfide electrolyte powder is placed in a test mold with ion-blocking electrodes on both sides, pressurized to 390MPa, and the sulfide electrolyte is tested for AC impedance at a polarization voltage of 50mV. The test range is 1MHz-1Hz, and the AC impedance spectrum of the test is obtained by Figure 7 The equivalent circuit is fitted, R2 is the AC impedance of the sulfide electrolyte under the current conditions. The electrolyte powder is taken out to test the thickness h and the cross-sectional area A, and the ionic conductivity of the sulfide electrolyte is calculated by the formula σ=h / (R2×A).
[0027] Preferably, the solid-state battery uses a sulfide electrolyte with a D 50 0.01-10μm.
[0028] Preferably, the solid-state battery uses a sulfide electrolyte with a D 50 0.3-2μm.
[0029] In the present invention, D 50 It refers to the particle size corresponding to when the cumulative particle size volume distribution number of the sulfide electrolyte measured by a laser particle size analyzer reaches 50%, that is, particles with a particle size smaller than (or larger than) this particle size account for 50%.
[0030] The present invention will be described in detail below by way of examples. In the following examples, unless otherwise specified, the instruments, reagents, materials, etc. involved are conventional instruments, reagents, materials, etc., which can be obtained through regular commercial channels.
[0031] Example 1
[0032] According to the chemical formula Li 5.5 PS 4.5 Cl 1.5(x=0.5, y=0) Weigh Li2S, LiCl, and P2S5 in a high-speed mixer with a filling rate of 50%. The high-speed mixer is mixed at a low speed of 500rpm for 300s to obtain a primary powder. Replace the knife group of the high-speed mixer, increase the speed to 8000rpm, and high-speed shear refinement for 600s to obtain a secondary powder. The secondary powder is sieved to ensure that the particle size (mesh number) is greater than 200 mesh. The secondary powder is transferred to an automatic tablet press for tableting. The tablet specifications are Φ20mm, 15mm thick, and the tableting pressure is set to 6t. All the above steps need to be carried out in an environment with a dew point below -60℃. The precursor material obtained by tableting is placed in a box furnace for high-temperature calcination. The calcination temperature is 500℃, the insulation time is 10h, and the heating rate is 10℃ / min. The entire calcination process needs to be carried out in an argon environment (water <0.01ppm, oxygen <0.01ppm). After calcination, the sample was transferred to a low dew point environment (dew point below -60°C) for crushing. The speed of the powder crusher was set to 10,000 rpm and the crushing time was 300 s.
[0033] The product was tested using a solid electrolyte powder ion conductivity test mold at 25°C and 400MPa. The impedance spectrum is shown in Figure 3 As shown, the equivalent circuit of the data fitting is Figure 7 As shown, the ionic conductivity of the final product is 10.3 mS / cm.
[0034] Example 2
[0035] According to the chemical formula Li6PS5Cl (x=0, y=0), Li2S, LiCl, and P2S5 were weighed in a high-speed mixer with a filling rate of 50%. The high-speed mixer was mixed at a low speed of 500rpm for 300s to obtain a primary powder. The knife group of the high-speed mixer was replaced, the speed was increased to 8000rpm, and high-speed shearing and refining was performed for 600s to obtain a secondary powder. The secondary powder was sieved to ensure that the particle size (mesh number) was greater than 200 mesh. The secondary powder was transferred to an automatic tablet press for tableting. The tablet specifications were Φ20mm, 15mm thick, and the tableting pressure was set to 6t. All the above steps need to be carried out in an environment with a dew point below -60℃. The precursor material obtained by tableting was placed in a box furnace for high-temperature calcination. The calcination temperature was 510, the holding time was 10h, and the heating rate was 10℃ / min. The entire calcination process needs to be carried out in an argon environment (water <0.01ppm, oxygen <0.01ppm). After calcination, the sample was transferred to a low dew point environment (dew point below -60°C) for crushing. The speed of the powder crusher was set to 10,000 rpm and the crushing time was 300 s.
[0036] The product was tested using a solid electrolyte powder ion conductivity test mold at 25°C and 400MPa. The impedance spectrum is shown in Figure 4 As shown, the equivalent circuit of the data fitting is Figure 7 As shown, the ionic conductivity of the final product is 6.8 mS / cm.
[0037] Example 3
[0038] According to the chemical formula Li 5.3 PS 4.3 ClBr 0.7 (x=0.5, y=0.7) Weigh Li2S, LiCl, LiBr, and P2S5 in a high-speed mixer with a filling rate of 50%. The high-speed mixer is mixed at a low speed of 500rpm for 300s to obtain a primary powder. Replace the knife group of the high-speed mixer, increase the speed to 8000rpm, and high-speed shear refinement for 600s to obtain a secondary powder. The secondary powder is sieved to ensure that the particle size (mesh number) is greater than 200 mesh. The secondary powder is transferred to an automatic tablet press for tableting. The tableting specifications are Φ20mm, 15mm thick, and the tableting pressure is set to 6t. All the above steps need to be carried out in an environment with a dew point below -60℃. The precursor material obtained by tableting is placed in a box furnace for high-temperature calcination. The calcination temperature is 480℃, the insulation time is 15h, and the heating rate is 10℃ / min. The entire calcination process needs to be carried out in an argon environment (water <0.01ppm, oxygen <0.01ppm). After calcination, the sample was transferred to a low dew point environment (dew point below -60°C) for crushing. The speed of the powder crusher was set to 10,000 rpm and the crushing time was 300 s. The product was tested using a solid electrolyte powder ion conductivity test mold. The test conditions were 25°C and 400 MPa. The impedance spectrum was as follows: Figure 5 As shown, the equivalent circuit of the data fitting is Figure 7 As shown, the ionic conductivity of the final product is 16.6 mS / cm.
[0039] Comparative Example 1 According to the chemical formula Li 5.5 PS 4.5 Cl 1.5(x=0.5, y=0) Weigh Li2S, LiCl, P2S5 in a ball mill, add 2mm, 3mm, 5mm ball milling beads in a mass ratio of raw material: ball milling beads = 1:3, and add n-heptane in a mass ratio of raw material: n-heptane = 1:1. Ball milling at 500rpm for 24h, the product is dried at 90℃ for 12h, and a powder tablet press is used for tableting. The tablet specifications are Φ30mm, 10mm thick, and the tableting pressure is set to 6t. All the above steps need to be carried out in a glove box environment (water <0.01ppm, oxygen <0.01ppm). The precursor material obtained by tableting is placed in a tube furnace for high-temperature calcination. The calcination temperature is 500℃, the insulation time is 10h, and the heating rate is 5℃ / min. The entire calcination process needs to be carried out in an argon environment (water <0.01ppm, oxygen <0.01ppm). After calcination, the sample was transferred to a glove box and crushed using a powder grinder for 300 seconds.
[0040] The product was tested using a solid electrolyte powder ion conductivity test mold at 25°C and 400MPa. The impedance spectrum is shown in Figure 6 As shown, the equivalent circuit of the data fitting is Figure 7 As shown, the ionic conductivity of the final product is 9.3 mS / cm.
[0041] Table 1 below shows comparative data of preparation time, ionic conductivity, and particle size distribution of Examples 1-3 and Comparative Example 1.
[0042]
[0043] from Figures 1 to 4 It can be seen from the data in Table 1 that the new process is used to prepare the sulfide electrolyte in the embodiment. Compared with Comparative Example 1, due to the use of the low-speed mixing + high-speed shearing process, the preparation time is significantly shortened, and the total mass of a single preparation is greatly increased. In addition, the ionic conductivity of the product is close to the laboratory process represented by Comparative Example 1, and the particle size distribution of the product is narrow and the particle size is close.
[0044] The above is only a specific embodiment of the present invention, but the protection scope of the present invention is not limited thereto. Any person skilled in the art can easily think of changes or substitutions within the technical scope disclosed by the present invention, which should be included in the protection scope of the present invention. Therefore, the protection scope of the present invention should be based on the protection scope of the claims.
Claims
1. A method for large-scale preparation of sulfide electrolytes for solid-state batteries, characterized in that: The sulfide electrolyte is an argyrodite-type sulfide electrolyte, and its chemical composition is Li 6-x PS 5-x X 1+x-y Y y , wherein X, Y are selected from one or more of the halogen elements F, Cl, Br, I, At; the value range of x is 0 to 0.8; the value range of y is 0 to 0.7; the value range of x+y is 0 to 0.8; The method comprises the following steps: S1: In a low dew point environment, the Li source, S source, P source, X source and Y source are mixed at a low speed to obtain a primary powder; S2: In a low dew point environment, the primary powder is subjected to high-speed shearing for refinement to obtain secondary powder; S3: Under a low dew point environment, the secondary powder is molded into blocks to obtain a precursor material; S4: In an inert gas environment, the precursor material is calcined at a high temperature, and crushed after calcination to obtain the sulfide electrolyte.
2. The method for large-scale preparation of sulfide electrolyte for solid-state batteries according to claim 1, characterized in that: The Li source is selected from any one or more of Li2S, Li2S2, LiCl, LiBr and LiI; the S source is selected from any one or more of P2S5, P4S9, Li2S and Li2S2; the P source is selected from any one or more of P2S5, P4S9, Li2S and Li2S2; 10 and P4S9; the X source and the Y source are selected from any one or more of LiCl, LiBr and LiI.
3. The method for large-scale preparation of sulfide electrolyte for solid-state batteries according to claim 1, characterized in that: The low dew point environment has a dew point of -40°C to -80°C and a temperature of 0°C to 40°C.
4. The method for large-scale preparation of sulfide electrolyte for solid-state batteries according to claim 1, characterized in that: The equipment used for low-speed mixing is selected from one or more of a high-speed mixer, a powder mill, a sand mill, and a ball mill; the rotation speed of the low-speed mixing process is 200 to 2000 rpm; the low-speed mixing time is 30 to 600 s; and the primary powder satisfies a particle size of 50 to 200 meshes.
5. The method for large-scale preparation of sulfide electrolyte for solid-state batteries according to claim 1, characterized in that: The equipment used for high-speed shearing is selected from one or more of a high-speed mixer, a powder mill, a sand mill, and a ball mill; the rotation speed of the high-speed shearing process is 1000 to 10000 rpm; the high-speed shearing time is 30 to 600 s; and the secondary powder satisfies a particle size of 150 to 1000 meshes.
6. The method for large-scale preparation of sulfide electrolyte for solid-state batteries according to claim 1, characterized in that: The equipment used in the molding block process includes one or more of an automatic tablet press, an automatic molding machine, an automatic tablet forming machine, and a fully automatic desktop tablet press; the molding block pressure is 1 to 20t, and the molding size is Φ10 to Φ300mm.
7. The method for large-scale preparation of sulfide electrolyte for solid-state batteries according to claim 1, characterized in that: The inert gas environment includes one or more of an argon atmosphere, a nitrogen atmosphere, and a helium atmosphere; the precursor calcination temperature is 400 to 600° C., and the insulation time is 2 to 20 hours.
8. The method for large-scale preparation of sulfide electrolyte for solid-state batteries according to claim 1, characterized in that: The equipment used for crushing the calcined samples includes one or more of a high-speed powder grinder, a fine crusher, a powder crusher, and a powder wall breaker; the crushing time is 10 to 300 seconds.
9. An all-solid-state lithium battery, characterized in that: A sulfide electrolyte prepared by the method for large-scale preparation of sulfide electrolyte for solid-state batteries according to any one of claims 1 to 8.
Citation Information
Patent Citations
Sulfide solid electrolyte and preparation method and application thereof
CN112421102A
Batch production method of sulfide solid electrolyte
CN112599848A
Preparation method of argyrodite phase sulfide solid electrolyte
CN118598165A
KR20240079294A
Cited By
Method for large-scale rapid preparation of sulfide all-solid-state electrolyte
CN121317821A