A Ni-MOFs-based O3-type sodium ion battery positive electrode material and its preparation method and application
Through the preparation of the positive electrode material of Ni-MOFs-based O3 sodium ion battery, Ni-MOFs is used to change the local chemical environment of the material, and the problems of complex phase transformation and air reactivity of O3 NaNi0.5Mn0.5O2 during charging and discharge process are solved. , achieving high performance and stability improvement.
Patent Information
- Application Number
- CN202411273987.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-12
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2044-09-12
AI Technical Summary
The O3 type NaNi0.5Mn0.5O2 sodium ion battery positive electrode material has complex phase transition, slow sodium ion kinetics, and performance losses caused by reactive Na in the air during charging and discharging.
Ni-MOFs (nickel-based metal organic frame) is used as the precursor, manganese and sodium sources are added, and the positive electrode material of Ni-MOFs-based O3 type sodium ion battery is synthesized by high-temperature solid phase method to increase the sodium source to compensate for the losses caused by high-temperature calcination. , change the local chemical environment of the material and increase the Na layer spacing.
The electrochemical performance of the positive electrode material of sodium ion battery is significantly improved, the reversible capacity at 0.1C and the capacity retention rate of 100 cycles is improved, the air stability of the material is enhanced, and the excellent electrochemical performance and high discharge specific capacity are shown.
Smart Images

Figure CN118791056B_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of chemical power sources, and in particular relates to a Ni-MOFs-based O3 type sodium ion battery positive electrode material and a preparation method and application thereof. Background Art
[0002] Sodium-ion batteries (SIBs) are more promising than lithium-ion batteries (LIBs) for large-scale energy storage due to their low cost and safety. Sodium is the next element after lithium in the periodic table due to its abundant content. In terms of safety, sodium-ion batteries have a more stable chemical property. In addition, sodium-ion batteries have a higher internal resistance than lithium-ion batteries, which results in no immediate accumulation of heat in the case of insufficient power. Layered oxide materials, polyanionic compounds, and Prussian blue compounds have been widely used to prepare SIBs positive electrodes. In particular, layered oxides have attracted attention due to their high specific capacity, simple synthesis method, and low price. In addition, the transition metal layer in the layered oxide of SIBs has more electrochemically active elements (such as nickel, iron, and manganese) than LIBs.
[0003] After layered lithium-containing oxides were used as cathodes for commercial lithium-ion batteries, sodium-ion layered oxide materials (transition layer TMO2, TM = Mn, Fe, Co, Ni, etc.) have been widely used as the main materials for SIBs cathodes. They are divided into different phase structures according to the position of sodium atoms (P represents prismatic sites, O represents octahedral sites) and the construction order of oxygen atoms. The Na phase is determined according to the sodium content and the characteristics of the transition metal. x TMO2 is divided into P2, O3 and dual-phase coexistence structure.
[0004] O3-phase layered oxides are considered to be the most promising cathode materials due to their excellent early coulombic efficiency and specific capacity. Specifically, NaNi 0.5 Mn 0.5 O2 is a typical cobalt-free layered oxide with high theoretical specific capacity (240 mAh × g-1) and large packing density. However, there are still some disadvantages: O3-type NaNi 0.5 Mn 0.5 O2 undergoes a more complex phase transition during charge and discharge, which is different from Na + The charge is related to the vacancy. The slower sodium ion kinetics of O3-type materials is due to the smaller spacing between the sodium layers. In addition, O3-type NaNi 0.5 Mn 0.5 The surface of the O2 material generates reactive Na in the presence of air, followed by structural deformation and oxidation of transition metal ions in the body, and the separated Na +Rapid reaction with H2O / CO2 in the surrounding air forms NaOH or Na2CO3 on the surface of the active material, resulting in battery performance loss. Therefore, finding a solution strategy to address the above unfavorable factors is crucial to the preparation of a high-performance sodium-ion battery. Summary of the invention
[0005] In order to solve the above technical problems, the present invention proposes a Ni-MOFs-based O3 type sodium ion battery positive electrode material and a preparation method and application thereof.
[0006] To achieve the above object, the present invention provides a method for preparing a Ni-MOFs-based O3 type sodium ion battery positive electrode material, using Ni-MOFs (nickel-based metal organic framework) as a precursor, adding a manganese source and a sodium source, and synthesizing the Ni-MOFs-based O3 type sodium ion battery positive electrode material (O3 type NaNi 0.5 Mn 0.5 O2).
[0007] Furthermore, a method for preparing a Ni-MOFs-based O3 type sodium ion battery positive electrode material comprises the following steps:
[0008] By NaNi 0.5 Mn 0.5 Ni-MOFs, a manganese source and a sodium source are weighed in an O2 stoichiometric ratio, mixed and ground, and the sodium source is added again. The resulting mixture is calcined and then cooled to room temperature to obtain the Ni-MOFs-based O3 type sodium ion battery positive electrode material.
[0009] Furthermore, in a method for preparing a Ni-MOFs-based O3-type sodium ion battery positive electrode material, the Ni-MOFs preparation method comprises the following steps:
[0010] 2 mmol of Ni(NO3)2 and 2 mmol of terephthalic acid were dissolved in 24 mL of DMF (N,N-dimethylformamide) solution, and the solution was continuously stirred until all solid particles were dissolved. The solution was then poured into a high-temperature reactor and reacted at 120°C for 12 hours. The solution was taken out of the reactor and centrifuged with ethanol for 3 to 4 times. The solid in the centrifuge tube was dried at 80°C for 6 hours to obtain the Ni-MOFs.
[0011] Furthermore, in a method for preparing a Ni-MOFs-based O3-type sodium-ion battery positive electrode material, the amount of sodium source added again is 5% of the mass of the sodium source added for the first time, and the purpose of adding the sodium source again is to compensate for the loss of sodium source caused by high-temperature calcination.
[0012] Furthermore, in a method for preparing a Ni-MOFs-based O3 type sodium ion battery positive electrode material, the calcination time is 24 hours, the temperature is 900°C, and the heating rate is 5°C / min.
[0013] Furthermore, in a method for preparing a Ni-MOFs-based O3 type sodium ion battery positive electrode material, the manganese source is manganese dioxide, and the sodium source is sodium carbonate.
[0014] The present invention also provides a Ni-MOFs-based O3 type sodium ion battery positive electrode material, which is prepared according to the preparation method and has a molecular formula of NaNi 0.5 Mn 0.5 O2.
[0015] The present invention also provides the use of the Ni-MOFs-based O3 type sodium ion battery positive electrode material in the preparation of a sodium ion battery.
[0016] Compared with the prior art, the present invention has the following advantages and technical effects:
[0017] The Ni-MOFs-based O3 type sodium ion battery positive electrode material proposed in the present invention utilizes Ni-MOFs to replace the commercially available nickel source (nickel hydroxide). The local chemical environment of the sodium ion battery positive electrode material is significantly changed by Ni-MOFs. The high porosity and large specific surface area of Ni-MOFs increase the Na interlayer spacing, which is beneficial to the improvement of the surface diffusion coefficient of sodium ions. As a result, the prepared Ni-MOFs-based O3 type sodium ion battery positive electrode material exhibits excellent electrochemical performance in a wide potential range of 2.0-4.0V, and the reversible capacity at 0.1C is 124mAh×g -1 The capacity retention rate after 100 cycles is 66.75%, and the capacity at 2C is 99.24 mAh×g -1 It has a high discharge specific capacity and greatly improves the air stability of the material. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] The drawings constituting a part of the present application are used to provide a further understanding of the present application. The illustrative embodiments and descriptions of the present application are used to explain the present application and do not constitute an improper limitation on the present application. In the drawings:
[0019] Figure 1 XRD patterns of M-NNMO prepared in Example 1 and NNMO prepared in Comparative Example 1 (a), schematic structure of M-NNMO prepared in Example 1 (b), and detailed XRD patterns of M-NNMO (c) and NNMO (d);
[0020] Figure 2SEM images of Ni-MOFs (a), M-NNMO (b) prepared in Example 1 and NNMO (c) prepared in Comparative Example 1, and EDS image of M-NNMO (d);
[0021] Figure 3 Specific surface area and pore size distribution diagram of NNMO (a) prepared in Comparative Example 1 and M-NNMO (b) prepared in Example 1;
[0022] Figure 4 a is the full spectrum of M-NNMO, b is the high-resolution XPS spectrum of Mn 2p, c is the high-resolution XPS spectrum of Ni 2p, d is the full spectrum after the reaction of M-NNMO and NNMO, e is the XPS spectrum of the reacted Mn 2p after the cycle, and f is the XPS spectrum of the reacted Ni 2p;
[0023] Figure 5 The charge and discharge curves of NNMO (a) and M-NNMO (b) at different cycle numbers, the performance comparison of M-NNMO and NNMO at different rate performances (c), and the long cycle performance test results of M-NNMO and NNMO materials at 0.1C (d) and 2C (e);
[0024] Figure 6 CV curves of NNMO (a) and M-NNMO (b) at a scan rate of 0.1 mV / s, Nyquist plots, and equivalent circuits of NNMO and M-NNMO (c);
[0025] Figure 7 XRD patterns of NNMO (a) and M-NNMO (b) after air aging test, first cycle charge and discharge curves of aged NNMO and M-NNMO (c), and cycle stability curves of NNMO and M-NNMO at 0.1C and 2.0V-4.0V (d). DETAILED DESCRIPTION
[0026] Various exemplary embodiments of the present invention will now be described in detail. This detailed description should not be considered as limiting the present invention, but should be understood as a more detailed description of certain aspects, features, and embodiments of the present invention.
[0027] It should be understood that the terms described in the present invention are only for describing special embodiments and are not intended to limit the present invention. In addition, for the numerical range in the present invention, it should be understood that each intermediate value between the upper and lower limits of the scope is also specifically disclosed. Each smaller range between the intermediate value in any stated value or stated range and any other stated value or intermediate value in the described range is also included in the present invention. The upper and lower limits of these smaller ranges can be independently included or excluded in the scope.
[0028] Unless otherwise indicated, all technical and scientific terms used herein have the same meanings as those generally understood by those skilled in the art. Although the present invention describes only preferred methods and materials, any methods and materials similar or equivalent to those described herein may also be used in the implementation or testing of the present invention. All documents mentioned in this specification are incorporated by reference to disclose and describe the methods and / or materials associated with the documents. In the event of a conflict with any incorporated document, the content of this specification shall prevail.
[0029] It will be apparent to those skilled in the art that various modifications and variations may be made to the specific embodiments of the present invention description without departing from the scope or spirit of the present invention. Other embodiments derived from the present invention description will be apparent to those skilled in the art. The present invention description and examples are exemplary only.
[0030] The words “include,” “including,” “have,” “contain,” etc. used in this document are open-ended terms, meaning including but not limited to.
[0031] The embodiment of the present invention provides a method for preparing a Ni-MOFs-based O3 type sodium ion battery positive electrode material, using Ni-MOFs (nickel-based metal organic framework) as a precursor, adding a manganese source and a sodium source, and synthesizing the Ni-MOFs-based O3 type sodium ion battery positive electrode material (O3 type NaNi 0.5 Mn 0.5 O2), more specifically, includes the following steps:
[0032] By NaNi 0.5 Mn 0.5 Ni-MOFs, a manganese source and a sodium source are weighed in an O2 stoichiometric ratio, mixed and ground, and the sodium source is added again. The resulting mixture is calcined and then cooled to room temperature to obtain the Ni-MOFs-based O3 type sodium ion battery positive electrode material.
[0033] In a preferred embodiment of the present invention, the method for preparing Ni-MOFs comprises the following steps:
[0034] 2 mmol of Ni(NO3)2 and 2 mmol of terephthalic acid were dissolved in 24 mL of DMF (N,N-dimethylformamide) solution, and the solution was continuously stirred until all solid particles were dissolved. The solution was then poured into a high-temperature reactor and reacted at 120°C for 12 hours. The solution was taken out of the reactor and centrifuged with ethanol for 3 to 4 times. The solid in the centrifuge tube was dried at 80°C for 6 hours to obtain the Ni-MOFs.
[0035] During the preparation of Ni-MOFs, all the nickel elements in the raw materials enter the metal skeleton and are almost completely converted in the high-temperature reactor. The chemical bonds of Ni(NO3)2×6H2O are all broken. Due to the strength of the ionic bond, the Ni atoms combine with terephthalic acid, and there is almost no loss.
[0036] In a preferred embodiment of the present invention, the amount of the sodium source added again is 5% of the mass of the sodium source added for the first time.
[0037] In a preferred embodiment of the present invention, the calcination time is 24 hours, the temperature is 900° C., and the heating rate is 5° C. / min.
[0038] In a preferred embodiment of the present invention, the manganese source is manganese dioxide, and the sodium source is sodium carbonate.
[0039] The present invention also provides a Ni-MOFs-based O3 type sodium ion battery positive electrode material, which is prepared according to the preparation method and has a molecular formula of NaNi 0.5 Mn 0.5 O2.
[0040] The raw materials used in the embodiments of the present invention are all commercially available, wherein sodium carbonate (sodium source) (Na2CO3, AR, 99.8%) and manganese dioxide (manganese source) (MnO2, AR, 99.0%) were purchased from Shanghai Yiang Chemical Technology Co., Ltd., nickel hydroxide (Ni(OH)2) was purchased from Shanghai McLean Biochemical Technology Co., Ltd., and nickel nitrate hexahydrate (Ni(NO3)2×6H2O) was purchased from Shanghai Tatian Technology Co., Ltd.
[0041] The technical solution of the present invention is further illustrated by the following embodiments.
[0042] Example 1
[0043] 2 mmol of Ni(NO3)2×6H2O and 2 mmol of terephthalic acid were dissolved in 24 mL of DMF (N,N-dimethylformamide) solution, and the solution was continuously stirred until all solid particles were dissolved. The solution was then poured into a high-temperature reactor and reacted at 120°C for 12 hours. The solution was taken out of the reactor and centrifuged with ethanol for 3 to 4 times. The solid in the centrifuge tube was dried at 80°C for 6 hours to obtain Ni-MOFs.
[0044] By NaNi 0.5 Mn 0.5The Ni-MOFs, manganese source (manganese dioxide) and sodium source (sodium carbonate) prepared above were weighed in an O2 stoichiometric ratio, mixed and ground, and then an excess of 5wt% sodium source (sodium carbonate) was added again. The resulting mixture was heated to 900°C at a heating rate of 5°C / min and calcined for 24h, and then naturally cooled to room temperature to obtain a Ni-MOFs-based O3-type sodium ion battery positive electrode material (O3-type NaNi 0.5 Mn 0.5 O2, denoted as M-NNMO).
[0045] Comparative Example 1
[0046] The same as Example 1, the only difference is that the stoichiometric ratio of Ni-MOFs is replaced by Ni(OH)2, and the obtained sodium ion battery positive electrode material is recorded as NNMO.
[0047] Performance Testing
[0048] 1. Characterization of Materials
[0049] The crystal structure of M-NNMO prepared in Example 1 and NNMO prepared in Comparative Example 1 was tested by XRD-600X-ray diffractometer. The target material is a copper target material, and the diffraction wavelength λ=0.15406nm. The experimental results of the physical structure information of the material were analyzed using Jade software and Rietveld refinement software to determine parameters such as crystal surface indicators and crystal surface spacing. The manufacturer of the scanning electron microscope used is Japan Advanced Technology Co., Ltd., model JSM-7610FPLUS. The model used in the fully automatic surface porosity analyzer is MikeASAP2020, and the adsorbed gas is high-purity nitrogen. The high magnification is: 100-1000K; the voltage is 15KV, and the element distribution of the material is measured using an EDS spectrometer. The X-ray photoelectron spectrum of the elements in the material was tested using a Hermo Scientific K-Alpha X-ray photoelectron spectrometer.
[0050] The XRD patterns of M-NNMO prepared in Example 1 and NNMO prepared in Comparative Example 1 are shown in Figure 1 a in the figure, and the detailed XRD patterns are shown in Figure 1 As shown in Figures c and d, the XRD patterns of M-NNMO at scanning angles of 16.7° and 42° have strong diffraction peaks, indicating that the (003) and (104) crystal planes of O3-NaNi 0.5 Mn 0.5 O2 (JCPDS card number 54-0887), has a high degree of crystallinity.
[0051] The structure of M-NNMO prepared in Example 1 is shown in FIG. Figure 1As shown in middle b, it can be seen that the lattice oxygen in the O3 phase is arranged in the form of face-centered cubic dense stacking, in which transition metal ions (Mn, Ni) and sodium ions occupy octahedral sites alternately in layers and use common edges to connect the sodium ions in the octahedral coordination centers.
[0052] The lattice parameters of the M-NNMO prepared in Example 1 and the NNMO prepared in Comparative Example 1 are shown in Table 1.
[0053] Table 1 Lattice parameters of M-NNMO and NNMO
[0054]
[0055] As can be seen from Table 1, all characteristic diffraction peaks can be regarded as rhombic lattices with space group R3m. However, Ni-MOFs significantly changed the local chemical environment of the M-NNMO cathode material. The battery parameters in the M-NNMO cathode material were a=b=2.946 (Å), the transition metal layer was reduced, and c=16.125 (Å), indicating that the Na interlayer spacing increased, which was beneficial to Na + diffusion, indicating that M-NNMO has a potential good multiplication performance. 0.5 Mn 0.5 Calculation of the O2 model structure showed that the Rwp of M-NNMO and NNMO increased by 7.90% and 7.21%, respectively, and the crystal structure of M-NNMO did not change significantly compared with that of NNMO, indicating the successful synthesis of M-NNMO.
[0056] The scanning electron microscope (SEM) images of Ni-MOFs, M-NNMO prepared in Example 1 and NNMO prepared in Comparative Example 1 are shown in FIG. Figure 2 a, b, c in Figure 2, EDS images of M-NNMO are shown in Figure 2 In d. By Figure 2 As can be seen in a, the Ni-MOFs precursor is composed of irregular circular flakes, and the nearby particles are impurities that have not yet been converted into Ni-MOFs. Figure 2 The SEM image in b shows that NNMO has an irregular block shape with a particle size of about 4 μm. Figure 2 As can be seen from the figure c, M-NNMO has a clear layered structure at around 1 μm, and its particle size is also significantly smaller than that of NNMO. Figure 2 As shown in (d), the energy dispersive spectroscopy (EDS) elemental map shows that the sodium, nickel, manganese and oxygen elements are almost uniformly distributed throughout the particle.
[0057] The Brunauer-Emmett-Teller (BET) method and the Barrett-Joiner-Halenda (BJH) model were used to characterize the NNMO ( Figure 3 a) and M-NNMO prepared in Example 1 ( Figure 3 b) The specific surface area and pore size distribution of the two materials (inset) were characterized. As shown in the figure, it can be clearly seen that the adsorption-desorption isotherm belongs to the H3 hysteresis loop, which further confirms that the material is layered in structure, which is consistent with the SEM image. The specific surface area of M-NNMO is 9.6009 m 2 ×g -1 , much larger than NNMO's 1.4072 m 2 ×g -1 , which can be attributed to the addition of Ni-MOFs.
[0058] The pore size distributions (PSDs) of NNMO and M-NNMO materials were calculated using the BJH model, which are mainly concentrated in the range of 1-50 nm. Both are between micropores and mesopores. The specific values of the BET specific surface areas of NNMO and M-NNMO materials are shown in Table 2.
[0059] Table 2 BET specific surface areas of NNMO and M-NNMO
[0060]
[0061] The oxidation states of the transition metals in M-NNMO were determined using X-ray photoelectron spectroscopy (XPS). Figure 4 , Figure 4 a is the full spectrum of M-NNMO, b is the high-resolution XPS spectrum of Mn 2p, c is the high-resolution XPS spectrum of Ni 2p, d is the full spectrum after the reaction of M-NNMO and NNMO, e is the XPS spectrum of Mn 2p after the reaction cycle, and f is the XPS spectrum of Ni 2p after the reaction.
[0062] The sample binding energy (BE) was calibrated to 284.85 eV using the C1s line, Figure 4 In b, Mn2p 3 / 2 The peak is located at about 642.8eV, Mn2p 1 / 2 The peak is located at about 654.4 eV, and the peaks with binding energies of 642.58 eV and 654.4 eV are Mn 4+ The characteristic peaks of Mn in M-NNMO indicate that Mn 4+ Have the upper hand. Figure 4 Figure c shows the Ni 2p XPS spectrum, which contains Ni P at around 855 eV. 3 / 2The Ni 2p spectrum has a NiP peak at 855eV. 3 / 2 peaks, and a Ni 2p satellite peak at 862.0eV and 880eV, indicating that Ni 2+ The existence of Ni in NiO 2+ The peaks are close, and M-NNMO is mainly composed of covalent Ni-O bonds, which is conducive to narrowing the transition metal layer and widening the Na layer spacing. In order to further study the changes in the oxidation state of the transition metal after the material reaction, the material was tested by XPS (df) after 5 charge and discharge cycles at 2-4V. The results showed that the intensity of the peaks in the full spectrum decreased significantly, indicating that a series of changes in the surface concentration of the elements occurred. After the M-NNMO material reacted, the binding energy of Mn2p3 / 2 moved to a higher energy value (643.5eV), and the binding energy of Ni2p3 / 2 was located at 856.5eV, indicating that both manganese and nickel participated in the redox reaction and contributed to the capacity. The peaks of other valence states did not appear. In contrast, the Mn 2p of NNMO showed peaks at 640.9 / 652.2eV and 643.7 / 654.7eV, representing Mn 3+ and Mn 4+ The presence of a small amount of Mn 2+ It also appears at 641.5eV and 653eV, which is based on the appearance of the MnO satellite peak at 647eV. 3+ The Jahn-Teller effect affects the reversible phase transition of the material and reduces the cycling stability of NNMO. 3 / 2 The binding energies of 2+ 、Ni 3+ 、Ni 4+ and the characteristic peak of NiO is 859.8eV. 2+ The decrease in the percentage leads to a decrease in covalent Ni-O bonds, which is not conducive to the expansion of the spacing between the Na layer and the transition metal layer.
[0063] 2. Electrochemical performance test
[0064] 80wt% of N-methyl-2-pyrrolidone (NMP) solvent, 10wt% of SuperP carbon (conductive carbon black) and 10wt% of polyvinylidene fluoride (PVDF) binder were mixed according to mass percentage to form a uniform slurry. After the resulting mixture was coated on aluminum foil, it was vacuum dried at 80°C for 12h. The button-type (CR2025) battery was assembled in an argon-filled glove box with a metal sodium disk as the negative electrode, the electrolyte was a 1.0M NaClO4 solution dissolved in a mixed solvent of propylene carbonate (PC) / ethylene carbonate (EC), and the separator was glass fiber (GF / D). The CT4008W system was used to test the performance of the battery at various current intensities (0.1C-5C, 1C=240mA×g -1 ) and room temperature. The constant current charge / discharge cycles were run in the voltage interval of 2.0–4.0 V. Cyclic voltammetry (CV) and electrochemical impedance spectroscopy (EIS) measurements were performed using an electrochemical workstation (CHI660E).
[0065] At 0.1C (24 mA × g -1 The charge and discharge curves of M-NNMO and NNMO were tested at a current density of 2.5 %. Figure 5 From a and b in Figure 1, it can be clearly seen that the specific capacity of the M-NNMO material to the electrode is as high as 124 mA×g in the first cycle. -1 , while the specific capacity of NNMO electrode material is only 95 mA×g -1 From the charge and discharge curves of different turns, it can be seen that the specific capacities of M-NNMO and NNMO electrodes are different. The charge and discharge efficiency of M-NMMO electrode is higher than that of NNMO electrode material. After 50 cycles of charge and discharge, the specific capacity of M-NNMO electrode material is still 106 mA×g -1 , compared with NNMO electrode materials, M-NMMO always maintains excellent reversibility.
[0066] Comparison of M-NNMO and NNMO performance at different rates is shown in Figure 5 In c, Figure 5 As can be seen from the figure, the M-NNMO electrode material is significantly improved over the NNMO electrode material at 0.1C, 0.2C, 0.5C, 1C, 2C, and 5C magnifications. The high porosity and large specific surface area of Ni-MOFs lead to an increase in the Na interlayer spacing, which is beneficial to the improvement of the surface diffusion coefficient of sodium ions, which is consistent with the above XRD Rietveld refinement results.
[0067] The long cycle performance test results of M-NNMO and NNMO materials at 0.1C and 2C are shown in Figure 5The long cycle performance results of NNMO and M-NMMO at 0.1C for 100 cycles show that the capacity retention rate of M-NNMO is 66.75%, while that of NNMO is only 58.34%. The coulombic efficiency of the two materials is close to 100%. The multiplicity of electrode materials is an important way to test electrode materials. The performance of the materials was tested for 100 cycles at 2C. The initial discharge specific capacities of M-NNMO and NNMO decreased significantly by 99.24 mAh×g -1 and 80.34 mAh×g -1 The capacity retention of M-NNMO is 66.11% and that of NNMO is 58.75%, which can be attributed to the porous surface of M-NNMO, which facilitates the electrolyte-electrode interaction.
[0068] CV curves of NNMO (a) and M-NNMO (b) at a scan rate of 0.1 mV / s in the voltage range of 2-4 V, Nyquist plots, and equivalent circuits of NNMO and M-NNMO (c) are shown in Figure 6 , it can be seen that during the three-turn cycle, four current pulse peaks were found at 2.479V, 3.181V, 3.439V and 3.562V in the cathode scan, but during repeated cycles, the NNMO electrode had almost no overlap, indicating that there are limitations in the reversible extraction / insertion process of sodium ions in ordinary NNMO materials, which is not as good as M-NNMO synthesized by Ni-MOFs. In the figure, the M-NNMO positive electrode material has four pairs of more symmetrical redox peaks at 2.783 / 2.538 V, 3.25 / 3.176 V, 3.518 / 3.455 V, and 3.682 / 3.556 V, respectively, which accurately correspond to the four voltage platforms in the charge / discharge curve. At the same time, the M-NNMO positive electrode material exhibits larger positive and negative electrode peak currents, which means that the material has better energy storage performance. The advantages of this material mainly come from the O3-type NaNi synthesized by Ni-MOFs. 0.5 Mn 0.5 O2 has a larger specific surface area, providing more electroactive sites.
[0069] Depend on Figure 6As can be seen in Figure c, the charge transfer resistance (Rct) at the electrode / electrolyte interface of the sample collected at a current density of 0.1C after 3 cycles is represented by the partial peaks in the high-frequency region and the slope in the low-frequency region of its EIS spectrum, as well as the Wahlberg impedance (Zw) associated with the electrolyte ion dispersion. Generally, a smaller peak indicates a lower Rct, and a larger vertical slope of the line means a shorter ion diffusion path, and the specific values are shown in Table 3. It can be clearly seen that M-NNMO has a smaller internal resistance and a good electrode that can make contact with the electrolyte. This phenomenon indicates that Ni-MOFs promote charge transfer within the material, which is attributed to the larger Na interlayer spacing of M-NNMO, which reduces the Na diffusion process. + Resistance process. The NNMO and M-NNMO materials have similar slopes, but M-NNMO exhibits a more vertical slope, indicating that the M-NNMO material has a relatively shorter ion diffusion process during the redox reaction.
[0070] Table 3 Nyquist plot fitting results of NNMO and M-NNMO
[0071]
[0072] The two materials were exposed to air for 7 days for air aging test, and the aged NNMO ( Figure 7 a) and M-NNMO ( Figure 7 From the structure of (b), it is clear that in addition to the appearance of NiO impurities, the NNMO material also undergoes a phase transition from P3 to O'3 due to the alkaline reaction of Na and the insertion of water molecules. In contrast, the M-NNMO material introduced by Ni-MOFs did not undergo obvious structural changes. The electrochemical performance was further tested, and the first discharge capacity of the aged NNMO (i.e., NNMO in air) was 85 mAh×g -1 The discharge capacity of aged M-NNMO (i.e., M-NNMO in air) is still better than that of NNMO, reaching up to 112 mAh×g -1 ( Figure 7 c). The capacity retention of the aged NNMO material is much lower than that of the aged M-NNMO material, which are 42.5% and 62% respectively in the 100-cycle performance. Figure 7 These results further indicate that Ni-MOFs reduce the Na interlayer spacing of transition metals and improve the O3-type NaNi 0.5 Mn 0.5 The stability of O2 in air.
[0073] In summary, it can be seen that the present invention changes the O3 type NaNi by replacing the common nickel source with a Ni-based metal organic framework material. 0.5Mn 0.5 The local chemical environment of O2 enhances the electrochemical performance of the material. More specifically, at 0.1C, the O3-type NaNi 0.5 Mn 0.5 The O2 capacity retention of the half-cell is improved from 58.34% to 66.75% over 100 cycles, which is mainly due to the enhanced stability of the transition metal layer, Mn 3+ The reduction of Na inhibits the Jahn-Teller phenomenon. At a test current density of 5C, the capacity of M-NNMO is increased by 87.5% compared with NNMO. Therefore, when exposed to air for a long time, M-NNMO material is more stable than NNMO. This is due to the increase in the Na layer gap and the Na + The diffusion rate is faster. The present invention proposes a method of constructing an O3-type NaNi with excellent performance by using Ni-MOFs. 0.5 Mn 0.5 Effective strategies for O2 electrode materials will help accelerate the creation of long-life SIBs for large-scale energy storage.
[0074] The above are only preferred specific implementations of the present application, but the protection scope of the present application is not limited thereto. Any changes or substitutions that can be easily thought of by a person skilled in the art within the technical scope disclosed in the present application should be included in the protection scope of the present application. Therefore, the protection scope of the present application should be based on the protection scope of the claims.
Claims
1. A method for preparing a Ni-MOFs-based O3 type sodium ion battery positive electrode material, characterized in that: Using Ni-MOFs as a precursor, adding a manganese source and a sodium source, and synthesizing the Ni-MOFs-based O3 type sodium ion battery positive electrode material by a high temperature solid phase method; The molecular formula of the Ni-MOFs-based O3-type sodium ion battery positive electrode material is NaNi 0.5 Mn 0.5 O2; The manganese source is manganese dioxide, and the sodium source is sodium carbonate; The temperature of the high-temperature solid phase method is 900° C., the calcination time is 24 h, and the heating rate is 5° C. / min.
2. The method for preparing the Ni-MOFs-based O3 type sodium ion battery positive electrode material according to claim 1, characterized in that: The following steps are involved: By NaNi 0.5 Mn 0.5 Ni-MOFs, a manganese source and a sodium source are weighed in an O2 stoichiometric ratio, mixed and ground, and the sodium source is added again. The resulting mixture is calcined and then cooled to room temperature to obtain the Ni-MOFs-based O3 type sodium ion battery positive electrode material.
3. The method for preparing the Ni-MOFs-based O3 type sodium ion battery positive electrode material according to claim 2, characterized in that: The amount of sodium source added again is 5% of the mass of the sodium source added for the first time.
4. A Ni-MOFs-based O3 type sodium ion battery positive electrode material, characterized in that: Prepared according to the preparation method according to any one of claims 1 to 3, the molecular formula is NaNi 0.5 Mn 0.5 O2.
5. Use of the Ni-MOFs-based O3 type sodium ion battery positive electrode material as claimed in claim 4 in the preparation of sodium ion batteries.
Citation Information
Cited By
Preparation method of low-cost high-performance sodium-ion battery cell
CN120674610A