Ceramic-based neutron absorbing material, preparation method thereof and reactor control rod

Ceramic-based neutron absorbing materials are prepared through high-energy ball milling and discharge plasma sintering methods, which solves the problems of insufficient thermal conductivity and heat resistance of traditional materials and achieves efficient neutron absorption and long-term stable operation of ceramic-based materials in nuclear reactors.

CN118791306APending Publication Date: 2024-10-18CHINA NUCLEAR POWER TECH RES INST CO LTD +2
View PDF 11 Cites 0 Cited by

Patent Information

Application Number
CN202410925318.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-11
Publication Date
2024-10-18

AI Technical Summary

Technical Problem

Traditional neutron absorbing materials have poor thermal conductivity and heat resistance, making it difficult to meet the stable operation requirements of nuclear reactor control rods.

Method used

After high-energy ball milling of ceramic substrates, ytterbium oxide and holmium oxide, ceramic-based neutron absorbing materials are prepared through discharge plasma sintering to control the density and neutron absorption properties of the materials and improve thermal conductivity and heat resistance.

Benefits of technology

The thermal conductivity and heat resistance of ceramic-based neutron absorbing materials are significantly improved, allowing them to withstand thermal shock in pressurized water reactors, operate stably for a long time, and extend service life.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118791306A_ABST
    Figure CN118791306A_ABST
Patent Text Reader

Abstract

The invention provides a preparation method of a ceramic-based neutron absorbing material, which comprises the following steps: mixing a ceramic base material, ytterbium oxide and holmium oxide, and carrying out high-energy ball milling treatment to form mixed powder, in the mixed powder, the mass fraction of the ceramic base material is 30-70 parts, the mass fraction of the ytterbium oxide is 10-30 parts, and the mass fraction of the holmium oxide is 10-30 parts; the mass part of the holmium oxide is less than 40 parts; and sintering the mixed powder by adopting a spark plasma sintering method.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of nuclear reactors, and in particular to a ceramic-based neutron absorbing material, a preparation method thereof and a reactor control rod. Background Art

[0002] Nuclear energy is an important choice for energy sustainability. In nuclear power equipment, control rod assemblies play a role in regulating nuclear reactions and play an important role in the safe operation of nuclear power plants. Both black control rod assemblies and gray control rod assemblies are usually used to control the nuclear reaction process. Among them, black control rod assemblies usually use strong neutron absorbing materials, such as Ag-In-Cd alloy and B4C. Gray control rod assemblies usually use weak neutron absorbing materials, such as molybdenum-based dysprosium oxide materials and stainless steel.

[0003] In a reactor where control rods participate in normal operation control, part of the control rod assembly needs to be inserted into the reactor all the time, and the insertion depth of the control rods is mechanically adjusted to achieve precise control of the nuclear reaction. In order to ensure the stable operation of the control rod assembly, it is usually hoped that the reactivity curve of the neutron absorbing material in it with the change of burnup is as stable as possible, while having good physical properties. However, the thermal conductivity and heat resistance of traditional neutron absorbing materials are poor, which is difficult to meet actual needs. Summary of the invention

[0004] Based on this, in order to solve the problems in the above background, it is necessary to provide a method for preparing a ceramic-based neutron absorbing material that can significantly improve thermal conductivity and heat resistance.

[0005] According to some embodiments of the present disclosure, a method for preparing a ceramic-based neutron absorbing material is provided, which comprises the following steps:

[0006] A ceramic substrate, ytterbium oxide and holmium oxide are mixed and subjected to high-energy ball milling to form a mixed powder, in which the mass fraction of the ceramic substrate is 30 to 70 parts, the mass fraction of ytterbium oxide is 10 to 30 parts, and the mass fraction of holmium oxide is less than 40 parts; and the mixed powder is sintered by spark plasma sintering.

[0007] In some embodiments of the present disclosure, in the mixed powder, the mass proportion of ytterbium oxide is 10% to 25%.

[0008] In some embodiments of the present disclosure, in the mixed powder, the mass proportion of holmium oxide is 5% to 40%.

[0009] In some embodiments of the present disclosure, in the mixed powder, the mass proportion of the ceramic substrate is 30% to 80%.

[0010] In some embodiments of the present disclosure, the ceramic substrate includes aluminum nitride.

[0011] In some embodiments of the present disclosure, the step of sintering the mixed powder includes a heating process and a heat preservation process;

[0012] During the heating process, the heating rate is controlled to be 50℃ / min~150℃ / min, and an axial pressure of 3MPa~7MPa is applied when the temperature is raised to 400℃~600℃, and an axial pressure of 8MPa~12MPa is applied when the temperature is raised to 800℃~1200℃; at the same time, during the insulation process, the sintering temperature is controlled to be 1500℃~1800℃, the sintering time is controlled to be 5min~20min, and the applied pressure is controlled to be 10MPa~50MPa.

[0013] In some embodiments of the present disclosure, in the step of performing high-energy ball milling, wet grinding media is added to the ball mill, and the mass ratio of the solid component to the wet grinding media is 1:(1-5);

[0014] In the step of high-energy ball milling, the grinding ball is made of zirconium oxide, and the ball-to-material ratio is (5-15):1;

[0015] In the step of high-energy ball milling, the total ball milling time is 10 h to 20 h, and the ball milling speed is 200 rpm to 600 rpm.

[0016] In some embodiments of the present disclosure, after the high-energy ball milling treatment and before the sintering treatment, a step of screening to obtain the mixed powder with a mesh size of 200-500 mesh is also included.

[0017] Furthermore, the present disclosure also provides a ceramic-based neutron absorption material, which is prepared by the method for preparing the ceramic-based neutron absorption material as described in any of the above embodiments.

[0018] Furthermore, the present disclosure also provides a reactor control rod, which includes the ceramic-based neutron absorbing material as described in any of the above embodiments.

[0019] In the preparation method of the ceramic-based neutron absorber of the embodiment of the present disclosure, the ceramic substrate, ytterbium oxide and holmium oxide are subjected to high-energy ball milling to obtain a mixed powder, and then the mixed powder is sintered by spark plasma sintering. Among them, by using raw materials of specific components and combining high-energy ball milling and spark plasma sintering for sintering, the excessive growth of the grain size of the material can be effectively controlled, so that the holmium oxide and ytterbium oxide materials are evenly dispersed in the ceramic substrate, and the density thereof is improved, so that it has good neutron absorption performance in a wide energy range, and has good service life performance, which can be applied to multiple types of nuclear reactor designs. After experimental verification, the ceramic-based neutron absorber prepared by the preparation method has good thermal conductivity and low linear expansion coefficient, can withstand thermal shock in a pressurized water reactor, and can operate stably for a long time under radiation conditions. This is conducive to improving the thermal stability and high cycle service life of the neutron absorber.

[0020] The above description is only an overview of the technical solution of the present invention. In order to more clearly understand the technical means of the present invention and implement it according to the contents of the specification, the following is a detailed description of the preferred embodiments of the present invention in conjunction with the accompanying drawings. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1 This is a picture of the neutron absorption material sample prepared in Example 6;

[0022] Figure 2 This is a scanning electron microscope image of the neutron absorption material prepared in Example 6. DETAILED DESCRIPTION

[0023] To facilitate understanding of the present invention, a more comprehensive description of the present invention is provided below. The preferred embodiments of the present invention are given herein. However, the present invention can be implemented in many different forms and is not limited to the embodiments described herein. On the contrary, the purpose of providing these embodiments is to make the content of the present invention more thorough and comprehensive.

[0024] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art to which this document pertains. The terms used herein in the specification of this document are only for describing specific embodiments and are not intended to limit this document.

[0025] It should be understood that when an element or layer is referred to as being "on, "adjacent to, "connected to, or "coupled to" another element or layer, it may be directly on, adjacent to, connected to, or coupled to the other element or layer, or there may be intervening elements or layers. In contrast, when an element is referred to as being "directly on, "directly adjacent to, "directly connected to, or "directly coupled to" another element or layer, there may be no intervening elements or layers. It should be understood that although the terms first, second, third, etc. may be used to describe various elements, components, regions, layers, and / or portions, these elements, components, regions, layers, and / or portions should not be limited by these terms. These terms are merely used to distinguish one element, component, region, layer, or portion from another element, component, region, layer, or portion.

[0026] Spatially relative terms such as "under," "beneath," "below," "under," "above," "above," and the like may be used herein for ease of description to describe the relationship of one element or feature to other elements or features. It should be understood that the spatially relative terms are intended to also include different orientations of the device in use and operation. For example, if the device in the accompanying drawings is flipped, then the elements or features described as "under other elements" or "under" or "under" will be oriented as "over" the other elements or features. Thus, the exemplary terms "under" and "under" may include both upper and lower orientations. The device may be otherwise oriented (e.g., rotated 90 degrees or other orientations) and the spatial descriptors used may be interpreted accordingly.

[0027] The purpose of the terms used herein is only to describe specific embodiments and is not intended to be a limitation of the present disclosure. When used herein, the singular forms "a", "an" and "the" are also intended to include plural forms, unless the context clearly indicates otherwise. It should also be understood that the terms "consisting of" and / or "comprising", when used in this specification, determine the presence of features, integers, steps, operations, elements and / or parts, but do not exclude the presence or addition of one or more other features, integers, steps, operations, elements, parts and / or groups. When used herein, the term "and / or" includes any and all combinations of the relevant listed items.

[0028] The present invention provides a method for preparing a ceramic-based neutron absorbing material. The method for preparing a ceramic-based neutron absorbing material comprises steps S1 and S2, which are specifically as follows.

[0029] Step S1, mixing a ceramic substrate, ytterbium oxide and holmium oxide and subjecting them to high-energy ball milling to form a mixed powder.

[0030] In this embodiment, in the mixed powder, the mass fraction of the ceramic substrate is 30 to 70 parts, the mass fraction of ytterbium oxide is 10 to 30 parts, and the mass fraction of holmium oxide is less than 40 parts. Controlling the masses of the ceramic substrate, ytterbium oxide and holmium oxide within the above mass fraction range is conducive to avoiding excessive growth of the ceramic substrate, ytterbium oxide and holmium oxide grains, and ensuring that the neutron absorption material has good neutron absorption performance and high density.

[0031] Among them, the role of high-energy ball milling treatment is to make the ceramic substrate, ytterbium oxide and holmium oxide fully mixed under the collision of the grinding balls, so that the surface of each material is deformed and broken, and then ytterbium oxide and holmium oxide form a composite oxide phase and are more evenly distributed in the ceramic substrate.

[0032] In some examples of this embodiment, in the mixed powder, the mass proportion of ytterbium oxide is 10% to 25%. For example, the mass proportion of ytterbium oxide can be 10%, 12%, 15%, 18%, 20%, 22%, 25%, or the mass proportion of ytterbium oxide can also be in the range between any two of the above mass proportions. Among them, ytterbium oxide has good neutron absorption ability and plays a very significant role in controlling the nuclear reaction process. When the mass proportion of ytterbium oxide is low, its neutron absorption ability is difficult to be fully exerted.

[0033] In some examples of this embodiment, in the mixed powder, the mass proportion of holmium oxide is 5% to 40%. For example, the mass proportion of holmium oxide can be 5%, 8%, 10%, 12%, 15%, 18%, 20%, 22%, 25%, 28%, 30%, 35%, 40%, or the mass proportion of holmium oxide can also be within the range between any two of the above mass proportions. The combination of holmium oxide and ytterbium oxide can make the reactivity of the material more stable with the change of burnup.

[0034] In some examples of this embodiment, the ceramic substrate may include aluminum nitride. Aluminum nitride has a low thermal expansion coefficient, good thermal conductivity, and good corrosion resistance. Selecting aluminum nitride as the matrix of the neutron absorber material can greatly improve the out-of-pile performance and service life of its components.

[0035] In some examples of this embodiment, the ceramic substrate may be selected from aluminum nitride particles. Further, the D50 particle size of the aluminum nitride particles may be 500 nm to 10 μm.

[0036] In some examples of this embodiment, the mass proportion of aluminum nitride in the ceramic-based neutron absorber can be more than 30%. Further, the mass proportion of aluminum nitride in the ceramic-based neutron absorber can be 30% to 80%. For example, the mass proportion of aluminum nitride in the ceramic-based neutron absorber can be 30%, 35%, 40%, 45%, 50%, 55%, 60%, 65%, 70%, 75%, 80%, or the mass proportion of aluminum nitride in the ceramic-based neutron absorber can also be in the range between any two of the above mass proportions. Among them, if the mass proportion of aluminum nitride is below 30%, it is difficult to fully exert its matrix function, which will cause the thermal conductivity of the neutron absorber to be too low and the linear expansion coefficient to be too high.

[0037] In some examples of this embodiment, the step of mixing the ceramic substrate, ytterbium oxide, and holmium oxide further includes adding a sintering aid, and the sintering aid may include one or more of yttrium oxide and calcium oxide.

[0038] In some examples of this embodiment, the high-energy ball milling treatment is wet milling. It can be understood that wet milling refers to adding wet milling media to the ball mill during the high-energy ball milling treatment. In this embodiment, the wet milling method can further improve the dispersion degree of the mixed powder.

[0039] In some examples of this embodiment, in the step of high-energy ball milling, the mass ratio of the solid component to the wet grinding medium can be controlled to be 1: (1~5). Wherein, the solid component refers to the raw materials including ceramic substrate, ytterbium oxide and holmium oxide. Further, the mass ratio of the solid component to the wet grinding medium can be controlled to be 1:1, 1:2, 1:3, 1:4, 1:5, or the mass ratio of the solid component to the wet grinding medium can be controlled to be within the range between any two of the above mass ratios. If the amount of wet grinding medium is too low, the viscosity of the mixed slurry may be higher, resulting in poor dispersion of the mixed powder. If the amount of wet grinding medium is too high, the effects of cold pressing and cold welding of ball milling are less significant.

[0040] In some examples of this embodiment, the wet grinding medium can be selected from an organic solvent, such as anhydrous ethanol.

[0041] In some examples of this embodiment, in the step of high-energy ball milling, the ball-to-material ratio can be controlled to be (5~15):1, wherein the ball-to-material ratio refers to the mass ratio of the grinding balls to the material being ball milled. Further, the ball-to-material ratio can be controlled to be 5:1, 6:1, 7:1, 8:1, 9:1, 10:1, 11:1, 12:1, 13:1, 14:1, 15:1, or the ball-to-material ratio can be controlled to be in the range between any two of the above mass ratios. Under this ball-to-material ratio condition, the raw materials are strongly impacted, ground and stirred by the high-speed rotation or vibration of the grinding balls, so that the raw material particles are crushed and recombined. Finally, the powder that has been ball-milled, refined, solid-solutionized, amorphous and nano-crystallized has an extremely high surface energy, which helps to improve the activation degree of the mixed powder and improve the sintering reaction efficiency.

[0042] In some examples of this embodiment, in the step of performing high-energy ball milling, the material of the milling balls used may be zirconium oxide.

[0043] In some examples of this embodiment, there may be multiple types of grinding balls, and the diameters of the multiple grinding balls are different. Further, in this embodiment, the multiple grinding balls may include a first grinding ball with a diameter of 5 mm, a second grinding ball with a diameter of 10 mm, and a third grinding ball with a diameter of 15 mm, and the number ratio of the first grinding ball, the second grinding ball, and the third grinding ball may be (40-80): (5-40): (0-10).

[0044] In some examples of this embodiment, in the step of high-energy ball milling, the ball milling speed can be controlled to be 200 rpm to 600 rpm. For example, the ball milling speed can be controlled to be 200 rpm, 250 rpm, 300 rpm, 350 rpm, 400 rpm, 450 rpm, 500 rpm, 550 rpm, 600 rpm, or the ball milling speed can be controlled to be in the range between any two of the above speeds.

[0045] In some examples of this embodiment, in the step of high-energy ball milling, the high-energy ball milling time can be controlled to be 10 hours to 20 hours. Further, the ball milling time can be controlled to be 10 hours, 11 hours, 12 hours, 13 hours, 14 hours, 15 hours, 16 hours, 17 hours, 18 hours, 19 hours, 20 hours, or the ball milling time can be controlled to be within the range between any two of the above times.

[0046] In some examples of this embodiment, after the high-energy ball milling process is completed, the wet milling medium can be removed to obtain a mixed powder. Further, the wet milling medium can be removed by vacuum drying.

[0047] In some examples of this embodiment, after the ball milling process and before the sintering process, a step of screening to obtain a mixed powder with a mesh size of 200-500 mesh is also included.

[0048] Step S2, sintering the mixed powder in a vacuum environment by using a spark plasma sintering method.

[0049] In this embodiment, the purpose of the sintering treatment is to further crystallize the mixed powder formed after ball milling, thereby further improving the out-of-pile performance of the prepared ceramic-based neutron absorber.

[0050] In this embodiment, in the step of sintering the mixed powder, the spark plasma sintering method is used to perform the sintering treatment in a vacuum environment. Among them, the spark plasma sintering method (Spark Plasma Sintering, referred to as SPS) is a process for sintering by plasma generated by pulse current. In traditional technology, radiation heating is usually used for sintering. Compared with the radiation heating method, by sintering the mixed powder including the ceramic substrate, ytterbium oxide and holmium oxide by first high-energy ball milling and then plasma sintering, the formed ceramic-based neutron absorption material can have good thermal conductivity and low linear expansion coefficient, can withstand thermal shock in a pressurized water reactor, can operate stably for a long time under radiation conditions, which is beneficial to improve the thermal stability and high cycle service life of the neutron absorption material.

[0051] In addition, compared with the traditional heating and sintering method, the plasma sintering method used in this embodiment can significantly reduce the sintering time while obtaining a denser ceramic-based neutron absorber, which can greatly improve the preparation efficiency of the ceramic-based neutron absorber and is conducive to large-scale industrial production.

[0052] In some examples of this embodiment, in the step of sintering the mixed powder, the sintering temperature can be controlled to be 1500° C. to 1800° C. For example, the sintering temperature can be controlled to be 1500° C., 1550° C., 1600° C., 1650° C., 1700° C., 1750° C., 1800° C., or the sintering temperature can be controlled to be within a range between any two of the above temperatures.

[0053] In some examples of this embodiment, in the step of sintering the mixed powder, the sintering time can be controlled to be 5min~20min. For example, the sintering time can be controlled to be 5min, 6min, 7min, 8min, 9min, 10min, 12min, 14min, 15min, 18min, 20min, or the sintering time can be controlled to be in the range between any two of the above sintering times. When the sintering time is less than 5min, the densification degree of the sintered body is low, and there are many defects inside the sintered body, such as pores, segregation, etc., which ultimately affect the out-of-pile performance of the neutron absorber. When the sintering time is higher than 20min, it is easy to cause coarse grains in the sintered body, which seriously affects the mechanical properties of the sintered body.

[0054] In some examples of this embodiment, in the step of sintering the mixed powder, the applied pressure can be controlled to be 10MPa to 50MPa. For example, the applied pressure can be controlled to be 10MPa, 15MPa, 20MPa, 25MPa, 30MPa, 35MPa, 40MPa, 45MPa, 50MPa, or the applied pressure can be controlled to be within the range between any two of the above pressures.

[0055] In some examples of this embodiment, the step of sintering the mixed powder can be performed in a vacuum environment. Further, in the step of sintering, the gas pressure of the sintering environment can be controlled to be lower than 10 -3 Pa.

[0056] In some examples of this embodiment, before the mixed powder is sintered, a step of heating the mixed powder may be included. In the step of heating the mixed powder, the heating rate may be controlled to be 50°C / min to 150°C / min. For example, the heating rate may be controlled to be 50°C / min, 60°C / min, 80°C / min, 100°C / min, 120°C / min, 140°C / min, 150°C / min, or the heating rate may be controlled to be within a range between any two of the above heating rates.

[0057] In some examples of this embodiment, in the step of heating the mixed powder, the pressure on the mixed powder can be gradually increased as the temperature increases, thereby improving the density of the prepared ceramic-based neutron absorber. For example, an axial pressure of 3MPa to 7MPa is applied when the temperature is raised to 500°C to 700°C, and an axial pressure of 8MPa to 12MPa is applied when the temperature is raised to 800°C to 1200°C.

[0058] In this embodiment, a pressure of 5 MPa may be applied when the temperature rises to 600°C, and a pressure of 10 MPa may be applied when the temperature rises to 1000°C.

[0059] It can be understood that the ceramic-based neutron absorption material of the present invention can be prepared through steps S1 to S2.

[0060] In the preparation method of the ceramic-based neutron absorber of the embodiment of the present disclosure, the ceramic substrate, ytterbium oxide and holmium oxide are subjected to high-energy ball milling to obtain a mixed powder, and then the mixed powder is sintered by spark plasma sintering. Among them, by using raw materials of specific components and combining high-energy ball milling and spark plasma sintering for sintering, the excessive growth of the grain size of the material can be effectively controlled, so that the holmium oxide and ytterbium oxide materials are evenly dispersed in the ceramic substrate, and the density thereof is improved, so that it has good neutron absorption performance in a wide energy range, can absorb neutrons of different energies, and can be applied to multiple types of nuclear reactor designs. After experimental verification, the ceramic-based neutron absorber prepared by the preparation method has good thermal conductivity and heat resistance, can withstand thermal shock in a pressurized water reactor, can operate stably for a long time under radiation conditions, and is conducive to improving the thermal stability and high cycle service life of the neutron absorber.

[0061] Furthermore, the present invention also provides a reactor control rod, which includes the ceramic-based neutron absorbing material of the above embodiment. It can be understood that in step S1 to step S2, the mixed powder can be filled into a mold and then sintered, and by controlling the shape of the mold, the sintered neutron absorbing material can be used as a reactor control rod.

[0062] In some examples of this embodiment, the reactor control rod can be used in a nuclear reactor, which can be a pressurized water reactor.

[0063] In order to facilitate the description of the ceramic-based neutron absorbing material and its preparation method of the present invention, the present invention also provides the following more specific embodiments and corresponding comparative examples. Through the following embodiments and comparative examples, the advantages of the ceramic-based neutron absorbing material of the present invention will also be more obvious.

[0064] Example 1

[0065] By mass fraction, 65 parts of aluminum nitride, 25 parts of ytterbium oxide, 5 parts of holmium oxide, 2.5 parts of yttrium oxide and 2.5 parts of calcium oxide were mixed evenly and added to an agate ball mill, using zirconium oxide grinding balls with a ball-to-material ratio of 10:1, and then anhydrous ethanol was added to the ball mill as a wet grinding medium, with a mass ratio of solid components to wet grinding medium of 1:2. The ball milling time was set to 15 hours, the ball milling speed was set to 400 rpm, and ball milling was performed to form a slurry.

[0066] The slurry was placed in a vacuum drying oven at 70°C for drying to obtain a mixed powder, and the mixed powder was sieved with a 300-mesh sieve for 5 minutes to 30 minutes to screen the mixed powder.

[0067] The screened mixed powder is filled into a graphite mold, compacted and vacuumed until the pressure is less than 10 -3 Pa. Spark plasma sintering was used for sintering, wherein the heating rate was set at 100°C / min, an axial pressure of 5 MPa was applied when heated to 500°C, an axial pressure of 10 MPa was applied when heated to 1000°C, and an axial pressure of 20 MPa was applied when heated to 1600°C. After keeping the temperature for 10 min, the pressure was released and the sample was cooled to room temperature.

[0068] Example 2

[0069] By mass fraction, 65 parts of aluminum nitride, 25 parts of ytterbium oxide, 5 parts of holmium oxide, 2.5 parts of yttrium oxide and 2.5 parts of calcium oxide were mixed evenly and added to an agate ball mill, using zirconium oxide grinding balls with a ball-to-material ratio of 3:1, and then anhydrous ethanol was added to the ball mill as a wet grinding medium, with a mass ratio of solid components to wet grinding medium of 1:2. The ball milling time was set to 15 hours, the ball milling speed was set to 400 rpm, and ball milling was performed to form a slurry.

[0070] The slurry was placed in a vacuum drying oven at 70°C for drying to obtain a mixed powder, and the mixed powder was sieved with a 300-mesh sieve for 5 minutes to 30 minutes to screen the mixed powder.

[0071] The screened mixed powder is filled into a graphite mold, compacted and vacuumed until the pressure is less than 10 -3 Pa. Spark plasma sintering was used for sintering, wherein the heating rate was set at 100°C / min, an axial pressure of 5 MPa was applied when heated to 500°C, an axial pressure of 10 MPa was applied when heated to 1000°C, and an axial pressure of 20 MPa was applied when heated to 1600°C. After keeping the temperature for 10 min, the pressure was released and the sample was cooled to room temperature.

[0072] Example 3

[0073] By mass fraction, 65 parts of aluminum nitride, 25 parts of ytterbium oxide, 5 parts of holmium oxide, 2.5 parts of yttrium oxide and 2.5 parts of calcium oxide were mixed evenly and added to an agate ball mill, using zirconium oxide grinding balls with a ball-to-material ratio of 10:1, and then anhydrous ethanol was added to the ball mill as a wet grinding medium, with a mass ratio of solid components to wet grinding medium of 1:2. The ball milling time was set to 15 hours, the ball milling speed was set to 400 rpm, and ball milling was performed to form a slurry.

[0074] The slurry was placed in a vacuum drying oven at 70°C for drying to obtain a mixed powder, and the mixed powder was sieved with a 300-mesh sieve for 5 minutes to 30 minutes to screen the mixed powder.

[0075] The screened mixed powder is filled into a graphite mold, compacted and vacuumed until the pressure is less than 10 -3 Pa. Spark plasma sintering was used for sintering, wherein the heating rate was set at 100°C / min, an axial pressure of 5 MPa was applied when heated to 500°C, an axial pressure of 10 MPa was applied when heated to 1000°C, and an axial pressure of 20 MPa was applied when heated to 1600°C. After keeping the temperature for 3 minutes, the pressure was released and the sample was cooled to room temperature.

[0076] Example 4

[0077] By mass fraction, 65 parts of aluminum nitride, 30 parts of ytterbium oxide, 5 parts of holmium oxide, 2.5 parts of yttrium oxide and 2.5 parts of calcium oxide were mixed evenly and added to an agate ball mill, using zirconium oxide grinding balls with a ball-to-material ratio of 10:1, and then anhydrous ethanol was added to the ball mill as a wet grinding medium, with a mass ratio of solid components to wet grinding medium of 1:2. The ball milling time was set to 15 hours, the ball milling speed was set to 400 rpm, and ball milling was performed to form a slurry.

[0078] The slurry was placed in a vacuum drying oven at 70°C for drying to obtain a mixed powder, and the mixed powder was sieved with a 300-mesh sieve for 5 minutes to 30 minutes to screen the mixed powder.

[0079] The screened mixed powder is filled into a graphite mold, compacted and vacuumed until the pressure is less than 10 -3 Pa. Spark plasma sintering was used for sintering, wherein the heating rate was set at 100°C / min, an axial pressure of 5 MPa was applied when heated to 500°C, an axial pressure of 10 MPa was applied when heated to 1000°C, and an axial pressure of 20 MPa was applied when heated to 1600°C. After keeping the temperature for 10 min, the pressure was released and the sample was cooled to room temperature.

[0080] Example 5

[0081] By mass fraction, 65 parts of aluminum nitride, 25 parts of ytterbium oxide, 2 parts of holmium oxide, 2.5 parts of yttrium oxide and 2.5 parts of calcium oxide were mixed evenly and added to an agate ball mill, using zirconium oxide grinding balls with a ball-to-material ratio of 10:1, and then anhydrous ethanol was added to the ball mill as a wet grinding medium, with a mass ratio of solid components to wet grinding medium of 1:2. The ball milling time was set to 15 hours, the ball milling speed was set to 400 rpm, and ball milling was performed to form a slurry.

[0082] The slurry was placed in a vacuum drying oven at 70°C for drying to obtain a mixed powder, and the mixed powder was sieved with a 300-mesh sieve for 5 minutes to 30 minutes to screen the mixed powder.

[0083] The screened mixed powder is filled into a graphite mold, compacted and vacuumed until the pressure is less than 10-3 Pa. Spark plasma sintering was used for sintering, wherein the heating rate was set at 100°C / min, an axial pressure of 5 MPa was applied when heated to 500°C, an axial pressure of 10 MPa was applied when heated to 1000°C, and an axial pressure of 20 MPa was applied when heated to 1600°C. After keeping the temperature for 10 min, the pressure was released and the sample was cooled to room temperature.

[0084] Example 6

[0085] According to the mass fraction, 65 parts of aluminum nitride, 25 parts of ytterbium oxide, and 5 parts of holmium oxide were mixed evenly and added to an agate ball mill, and zirconium oxide grinding balls were used, with a ball-to-material ratio of 10:1. Anhydrous ethanol was then added to the ball mill as a wet grinding medium, and the mass ratio of the solid component to the wet grinding medium was 1:2. The ball milling time was set to 15 hours, the ball milling speed was set to 400 rpm, and ball milling was performed to form a slurry.

[0086] The slurry was placed in a vacuum drying oven at 70°C for drying to obtain a mixed powder, and the mixed powder was sieved with a 300-mesh sieve for 5 minutes to 30 minutes to screen the mixed powder.

[0087] The screened mixed powder is filled into a graphite mold, compacted and vacuumed until the pressure is less than 10 -3 Pa. Spark plasma sintering was used for sintering, wherein the heating rate was set at 100°C / min, an axial pressure of 5 MPa was applied when heated to 500°C, an axial pressure of 10 MPa was applied when heated to 1000°C, and an axial pressure of 20 MPa was applied when heated to 1600°C. After keeping the temperature for 10 min, the pressure was released and the sample was cooled to room temperature.

[0088] Comparative Example 1

[0089] According to the mass fraction, 25 parts of aluminum nitride, 25 parts of ytterbium oxide, 5 parts of holmium oxide, 2.5 parts of yttrium oxide and 2.5 parts of calcium oxide were mixed evenly and added to an agate ball mill, and zirconium oxide grinding balls were used, with a ball-to-material ratio of 10:1. Anhydrous ethanol was added to the ball mill as a wet grinding medium, and the mass ratio of the solid component to the wet grinding medium was 1:2. The ball milling time was set to 15h, the ball milling speed was set to 400rpm, and ball milling was performed to form a slurry.

[0090] The slurry was placed in a vacuum drying oven at 70°C for drying to obtain a mixed powder, and the mixed powder was sieved with a 300-mesh sieve for 5 minutes to 30 minutes to screen the mixed powder.

[0091] The screened mixed powder is filled into a graphite mold, compacted and vacuumed until the pressure is less than 10 -3Pa. Spark plasma sintering was used for sintering, wherein the heating rate was set at 100°C / min, an axial pressure of 5 MPa was applied when heated to 500°C, an axial pressure of 10 MPa was applied when heated to 1000°C, and an axial pressure of 20 MPa was applied when heated to 1600°C. After keeping the temperature for 10 min, the pressure was released and the sample was cooled to room temperature.

[0092] Comparative Example 2

[0093] By mass fraction, 65 parts of aluminum nitride, 35 parts of ytterbium oxide, 5 parts of holmium oxide, 2.5 parts of yttrium oxide and 2.5 parts of calcium oxide were mixed evenly and added to an agate ball mill, using zirconium oxide grinding balls with a ball-to-material ratio of 10:1, and then anhydrous ethanol was added to the ball mill as a wet grinding medium, with a mass ratio of solid components to wet grinding medium of 1:2. The ball milling time was set to 15 hours, the ball milling speed was set to 400 rpm, and ball milling was performed to form a slurry.

[0094] The slurry was placed in a vacuum drying oven at 70°C for drying to obtain a mixed powder, and the mixed powder was sieved with a 300-mesh sieve for 5 minutes to 30 minutes to screen the mixed powder.

[0095] The screened mixed powder is filled into a graphite mold, compacted and vacuumed until the pressure is less than 10 -3 Pa. Spark plasma sintering was used for sintering, wherein the heating rate was set at 100°C / min, an axial pressure of 5 MPa was applied when heated to 500°C, an axial pressure of 10 MPa was applied when heated to 1000°C, and an axial pressure of 20 MPa was applied when heated to 1600°C. After keeping the temperature for 10 min, the pressure was released and the sample was cooled to room temperature.

[0096] Comparative Example 3

[0097] By mass fraction, 65 parts of aluminum nitride, 25 parts of ytterbium oxide, 50 parts of holmium oxide, 2.5 parts of yttrium oxide and 2.5 parts of calcium oxide were mixed evenly and added to an agate ball mill, using zirconium oxide grinding balls with a ball-to-material ratio of 10:1, and then anhydrous ethanol was added to the ball mill as a wet grinding medium, with a mass ratio of solid components to wet grinding medium of 1:2. The ball milling time was set to 15 hours, the ball milling speed was set to 400 rpm, and ball milling was performed to form a slurry.

[0098] The slurry was placed in a vacuum drying oven at 70°C for drying to obtain a mixed powder, and the mixed powder was sieved with a 300-mesh sieve for 5 minutes to 30 minutes to screen the mixed powder.

[0099] The screened mixed powder is filled into a graphite mold, compacted and vacuumed until the pressure is less than 10 -3Pa. Spark plasma sintering was used for sintering, wherein the heating rate was set at 100°C / min, an axial pressure of 5 MPa was applied when heated to 500°C, an axial pressure of 10 MPa was applied when heated to 1000°C, and an axial pressure of 20 MPa was applied when heated to 1600°C. After keeping the temperature for 10 min, the pressure was released and the sample was cooled to room temperature.

[0100] Experiment 1: Samples of neutron absorbing materials prepared in Example 6 can be found in Figure 1 The morphology of the neutron absorbing material after sintering in Example 1 was observed using a scanning electron microscope. The results are shown in Figure 2 .

[0101] Test 2: The room temperature thermal conductivity and linear expansion coefficient of the above embodiments and comparative examples were tested, and the results are shown in Table 1. The higher the thermal conductivity and the lower the linear expansion coefficient, the longer the service life of the material.

[0102] Table 1

[0103]

[0104] Reference Figure 1 As shown, in the ceramic-based neutron absorption material of Example 1, the aluminum nitride material exists in the form of a particle phase, ytterbium oxide and holmium oxide are composited to form a whole and are uniformly dispersed in the aluminum nitride particle phase. The structure in which the composite oxide phase is uniformly dispersed in the aluminum nitride particle phase helps to make the neutron absorption material as a whole have a higher thermal conductivity and a lower linear expansion coefficient.

[0105] As shown in Table 1, the ceramic-based neutron absorption material of Example 1 uses 30-70 parts of ceramic substrate, 10-30 parts of ytterbium oxide and less than 40 parts of holmium oxide as raw materials. The thermal conductivity of the sintered material reaches 60 W / (m*K) and the linear expansion coefficient (CTE) reaches 6×10 -6 / ℃. Compared with Example 1, the amount of aluminum nitride in Comparative Example 1 is lower and less than 30 parts, and its thermal conductivity is only 35W / (m*K), which is significantly lower than that of Example 1, and its linear expansion coefficient is 8.5×10 -6 / ℃, which is significantly higher than Example 1, and accordingly, the service life of Example 1 will also be relatively low. The amount of ytterbium oxide in Example 2 is relatively high and higher than 30 parts, its thermal conductivity is lower than Example 1, and its linear expansion coefficient is higher than Example 1, indicating that when the amount of ytterbium oxide is relatively high, it will have a negative impact on the service life of the neutron absorber. The amount of holmium oxide in Example 3 is relatively high and higher than 40 parts, its thermal conductivity is higher than Example 1, and its linear expansion coefficient is lower than Example 1, indicating that when the amount of holmium oxide is relatively high, it will have a negative impact on the service life of the neutron absorber.

[0106] In addition, compared with Example 1, Example 2 has a lower ball material ratio and a relatively poor high-energy ball milling effect, so Example 2 has a lower thermal conductivity and a higher linear expansion coefficient. The sintering time of Example 3 is relatively short, at which time the ceramic substrate, ytterbium oxide and holmium oxide have not been fully sintered, and accordingly the performance of the sintered material is also significantly poor.

[0107] Please note that the above embodiments are for illustrative purposes only and are not meant to be limiting of this document.

[0108] It should be understood that, unless otherwise specified herein, there is no strict order restriction for the execution of the steps, and the steps may be executed in other orders. Moreover, at least a portion of the steps in the preparation process may include multiple sub-steps or multiple stages, and these sub-steps or stages are not necessarily executed at the same time, but may be executed at different times, and the execution order of these sub-steps or stages is not necessarily sequential, but may be executed in turn or alternately with other steps or at least a portion of the sub-steps or stages of other steps.

[0109] The various embodiments in this specification are described in a progressive manner, and each embodiment focuses on the differences from other embodiments. The same or similar parts between the various embodiments can be referenced to each other.

[0110] The technical features of the above embodiments may be combined arbitrarily. To make the description concise, not all possible combinations of the technical features in the above embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

Claims

1. A method for preparing a ceramic-based neutron absorbing material, It is characterized in that The steps include: A ceramic substrate, ytterbium oxide and holmium oxide are mixed and subjected to high-energy ball milling to form a mixed powder, wherein the ceramic substrate has a mass fraction of 30 to 70 parts, the ytterbium oxide has a mass fraction of 10 to 30 parts, and the holmium oxide has a mass fraction of less than 40 parts; and, The mixed powder is sintered by spark plasma sintering.

2. The method for preparing the ceramic-based neutron absorbing material according to claim 1, It is characterized in that In the mixed powder, the mass proportion of ytterbium oxide is 10% to 25%.

3. The method for preparing the ceramic-based neutron absorbing material according to claim 1, It is characterized in that In the mixed powder, the mass proportion of holmium oxide is 5% to 40%.

4. The method for preparing a ceramic-based neutron absorbing material according to claim 1, It is characterized in that In the mixed powder, the mass proportion of the ceramic substrate is 30% to 80%.

5. The method for preparing the ceramic-based neutron absorbing material according to any one of claims 1 to 4, It is characterized in that The ceramic substrate includes aluminum nitride.

6. The method for preparing the ceramic-based neutron absorbing material according to any one of claims 1 to 4, It is characterized in that The step of sintering the mixed powder includes a heating process and a heat preservation process; During the heating process, the heating rate is controlled to be 50℃ / min~150℃ / min, and an axial pressure of 3MPa~7MPa is applied when the temperature is raised to 400℃~600℃, and an axial pressure of 8MPa~12MPa is applied when the temperature is raised to 800℃~1200℃; at the same time, during the insulation process, the sintering temperature is controlled to be 1500℃~1800℃, the sintering time is controlled to be 5min~20min, and the applied pressure is controlled to be 10MPa~50MPa.

7. The method for preparing the ceramic-based neutron absorbing material according to any one of claims 1 to 4, It is characterized in that In the step of high-energy ball milling, wet grinding media is added to the ball mill, and the mass ratio of solid components to wet grinding media is 1: (1-5); In the step of high-energy ball milling, the grinding ball is made of zirconium oxide, and the ball-to-material ratio is (5-15):1; In the step of high-energy ball milling, the total ball milling time is 10 h to 20 h, and the ball milling speed is 200 rpm to 600 rpm.

8. The method for preparing the ceramic-based neutron absorbing material according to any one of claims 1 to 4, It is characterized in that After the high-energy ball milling treatment and before the sintering treatment, the method further includes a step of screening to obtain the mixed powder with a mesh size of 200 to 500 meshes.

9. A ceramic-based neutron absorbing material, It is characterized in that The neutron absorbing material is prepared by the method for preparing the ceramic-based neutron absorbing material according to any one of claims 1 to 8.

10. A reactor control rod, It is characterized in that Comprising the ceramic-based neutron absorbing material as claimed in claim 9.

Citation Information

Patent Citations

  • Preparation method of aluminum nitride ceramic LED lamp thermal-conducting material

    CN102875156A

  • Rare earth doped tungstic acid-based high-entropy ceramic and preparation method thereof

    CN114075074A

  • Chlorapatite ceramic as well as preparation method and application thereof

    CN114075076A

  • Neutron absorbing material, application thereof and control rod for nuclear reactor core

    CN117756527A

  • Preparation method of xenotime structure high-entropy phosphate ceramic powder

    CN118206378A